Method for producing high purity manganese and high purity manganese

The method addresses the insufficient reduction of oxygen and boron in high-purity manganese production by forming an oxide film and capturing boron impurities, resulting in high-purity manganese that prevents semiconductor device deterioration.

JP7594808B2Active Publication Date: 2024-12-05ASAHI METAL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023094708
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-08
Publication Date
2024-12-05
Estimated Expiration
2039-12-04

AI Technical Summary

Technical Problem

Existing methods for producing high-purity manganese fail to sufficiently reduce both oxygen and boron concentrations, which can lead to deterioration of semiconductor device characteristics.

Method used

A method involving heat treatment of raw manganese in a controlled oxygen partial pressure and temperature range to form an oxide film, followed by vaporization and cooling to capture boron impurities, combined with electrolytic treatment and sublimation or evaporation to further reduce impurities.

Benefits of technology

The method achieves high-purity manganese with oxygen and boron concentrations of 3 ppm or less, effectively suppressing semiconductor device deterioration by reducing impurity effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594808000003
    Figure 0007594808000003
  • Figure 0007594808000004
    Figure 0007594808000004
  • Figure 0007594808000001
    Figure 0007594808000001
Patent Text Reader

Abstract

To provide a method for producing high purity manganese capable of sufficiently reducing an oxygen concentration and a boron concentration.SOLUTION: There is provided a method for producing high purity manganese which comprises: a step of preparing raw material manganese; a step of oxidizing the surface of the raw material manganese by performing heat treatment in which the raw material manganese is maintained at a temperature range of 40°C or higher and 200°C or lower for 1 hour or more and 48 hours or less in the atmosphere adjusted so that the partial pressure of oxygen is 1.5×104 Pa or more and 8×104 Pa or less; and a step of heating the raw material manganese of which surface is oxidized to generate manganese vapor, followed by cooling the manganese vapor to obtain high purity manganese.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing high purity manganese (Mn) and high purity manganese. do. [Background technology]

[0002] Manganese is sometimes added to copper (Cu), which is the wiring material for semiconductor devices. By adding manganese, copper can be diffused into silicon (Si), a semiconductor material. When high purity manganese is used as the manganese, There are two methods for producing high purity manganese: electrolytic treatment and the use of raw manganese. A method of distilling or sublimating benzene has been proposed (for example, Patent Documents 1 to 4). In Patent Document 2, a method of performing electrolysis and a method of sublimation are combined. A method has been proposed to obtain high-purity manganese with a reduced oxygen (O) concentration by combining . [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-152528 [Patent Document 2] JP 2002-285373 A [Patent Document 3] International Publication No. 2013 / 105291 [Patent Document 4] International Publication No. 2015 / 060018 Summary of the Invention [Problem to be solved by the invention]

[0004] In the above high purity manganese, it is possible to reduce not only the oxygen concentration but also the boron (B) concentration. Therefore, it is necessary to sufficiently reduce the oxygen concentration and boron concentration. One of the objectives of the present invention is to provide a method for producing high purity manganese and high purity manganese that can do. [Means for solving the problem]

[0005] The method for producing high purity manganese according to the present disclosure includes the steps of preparing raw manganese and reacting with oxygen. The partial pressure is 1.5×10 4 Pa or more 8×10 4 In an atmosphere adjusted to a pressure of less than 1 Pa The raw manganese is kept at a temperature range of 40°C to 200°C for 1 hour to 48 hours. The surface of the raw manganese is oxidized by carrying out a heat treatment. The manganese vapor is generated by heating the manganese raw material, and then cooled. and a step of converting the resulting manganese to high purity manganese.

[0006] The high purity manganese according to the present disclosure has an oxygen content of 3 mass ppm or less and a boron content of 0.01% or less. The content is 3 ppm by mass or less. Effect of the Invention

[0007] According to the present disclosure, high purity manganese having sufficiently reduced oxygen and boron concentrations is provided. The high purity manganese disclosed herein can prevent the formation of semiconductors due to oxygen and boron. This makes it possible to suppress deterioration of the characteristics of the device. [Brief description of the drawings]

[0008] [Figure 1] 1 is a flowchart showing an example of a method for producing high purity manganese in the first embodiment. [Diagram 2] 11 is a flowchart showing an example of a method for producing high purity manganese in the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. The method for producing high purity manganese according to the present disclosure includes the following steps: The process of preparing raw manganese and oxygen partial pressure is 1.5×10 4 Pa or more 8×10 4 Pa In an atmosphere adjusted to the temperature below 40℃, the raw manganese is heated to 40℃ or higher and 200℃ or lower. By carrying out heat treatment in a temperature range of 1 hour to 48 hours, A step of oxidizing the surface of the raw manganese and heating the surface-oxidized manganese raw material to produce manganese and cooling the manganese vapor to obtain high purity manganese.

[0010] In the method for producing high purity manganese disclosed herein, the partial pressure of oxygen is 1.5×10 4 More than Pa 8×10 4 In an atmosphere adjusted to a pressure of 0.01 Pa or less, the manganese raw material is heated to 40°C or higher. The heat treatment is carried out by holding the material at a temperature of 200°C or less for 1 hour or more and 48 hours or less. By carrying out such a heat treatment, the surface of the raw manganese is oxidized and a manganese oxide film is formed. In order to generate manganese vapor without forming an oxide film on manganese, the raw manganese is When manganese is heated, some of the boron contained as an impurity in the raw manganese is converted into In contrast, the surface of the raw manganese is oxidized by the above heat treatment and mixed into the manganese vapor. By forming the film, the boron in the raw manganese is captured by the oxide film. This reduces the amount of boron mixed into the manganese vapor. Thus, it is possible to obtain high-purity manganese with a sufficiently reduced boron concentration. According to the disclosed method for producing high purity manganese, the oxygen concentration and boron concentration are sufficiently reduced. Therefore, high purity manganese can be obtained.

[0011] In the above-mentioned method for producing high purity manganese, the oxygen concentration in the raw manganese is 570 mass %. By using such a manganese raw material, the oxygen concentration is sufficiently low. This makes it easy to obtain high purity manganese with reduced solubility.

[0012] In the method for producing high purity manganese, the step of preparing raw manganese includes the steps of: A raw material containing at least one of manganese chloride and manganese dioxide is dissolved in hydrochloric acid. The manganese chloride aqueous solution is then contacted with a chelating resin. and purifying the aqueous manganese chloride solution by contacting the aqueous manganese chloride solution with water. The electrolytic process is carried out to electrolytically deposit manganese using the above as an electrolyte, and the raw manganese is obtained by electrowinning. The electrowinning manganese obtained by carrying out the electrolytic treatment may include a step of obtaining manganese. Manganese is suitable as the raw manganese.

[0013] In the above-mentioned method for producing high purity manganese, in the step of obtaining high purity manganese, Manganese vapor is generated by heating manganese to sublimate it, and then the manganese vapor is cooled to High purity manganese may be obtained by sublimating raw manganese as described above. By generating gun steam, the oxygen and boron concentrations in high purity manganese can be further increased. It can be further reduced.

[0014] In the process for producing high purity manganese, the raw manganese The manganese vapor is then cooled and heated to a high temperature. As described above, manganese can be obtained by evaporating raw manganese. By generating manganese vapor, high purity manganese can be obtained at a lower cost.

[0015] In the high purity manganese disclosed herein, the oxygen content is 3 ppm by mass or less, and boron The oxygen and boron content is 3 ppm by mass or less. This makes it possible to suppress the deterioration of semiconductor device characteristics caused by oxygen and boron. can.

[0016] [Details of the embodiment of the present disclosure] Next, embodiments of the high purity manganese and the method for producing high purity manganese according to the present disclosure will be described. The following description will be given with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals. Reference numbers are given to the respective parts and their descriptions will not be repeated.

[0017] (Embodiment 1) First, the high purity manganese according to one embodiment of the present application will be described. In high purity manganese, the oxygen content is 3 mass ppm or less and the boron content is By setting the oxygen and boron contents in the above ranges, In this way, it is possible to suppress the deterioration of the characteristics of semiconductor devices caused by oxygen and boron. For example, when the high purity manganese disclosed in the present disclosure is used for wiring materials, the oxygen content is sufficiently reduced. Therefore, it is possible to suppress the decrease in the conductivity of the copper wiring. When the high purity manganese disclosed in the present disclosure is used as a sputtering target material, the oxygen content Since the amount of particles is sufficiently reduced, the generation of particles can be reduced and the reliability of the device can be improved. According to the studies by the present inventors, the high purity manganese dioxide of the present disclosure can suppress the decrease in reliability. In the case of silicon, the boron concentration is sufficiently reduced, so that it can be used for, for example, the active layer of a semiconductor device. This reduces the diffusion of boron and suppresses the deterioration of the life span of semiconductor devices. The oxygen content of the high purity manganese is preferably 1 mass ppm or less. The content of oxygen is preferably 2 mass ppm or less. It can be measured by the Instrumental Gas Analysis method. More specifically, it can be measured by infrared absorption method. For example, GDMS (Glow Discharge Mass Spectrometer) It can be measured by glow discharge mass spectrometry.

[0018] Next, a procedure for producing high purity manganese according to the present embodiment will be described with reference to FIG. In the method for producing high purity manganese in the first embodiment, first, raw manganese is In the present embodiment, a preparation step (S10) is carried out. The purity of the raw manganese in this embodiment is, for example, 99.9 mass % (3N In this disclosure, purity is the mass of the entire sample measured by the GDMS method. The ratio of the total mass of the metal impurities in the sample to the total mass of the sample (mass In this embodiment, the oxygen concentration of the raw manganese is 570 mass ppm or less. The oxygen concentration of the raw manganese is preferably 535 mass ppm or less, more preferably or 500 ppm by mass or less.

[0019] Next, referring to FIG. 1, in step (S20), a step of oxidizing the surface of raw manganese is performed. More specifically, the partial pressure of oxygen is 1.5×10 4 Pa or more 8×10 4 Pa In an atmosphere adjusted to the temperature below 40℃, the raw manganese is heated to 40℃ or higher and 200℃ or lower. The first heat treatment is carried out by holding the material in the temperature range for 1 hour or more and 48 hours or less. Before this, the raw manganese is washed with acid such as nitric acid to remove any foreign matter adhering to its surface. By carrying out the first heat treatment, the surface of the raw manganese is oxidized, and the manganese An oxide film of silicon is formed.

[0020] The partial pressure of oxygen in the first heat treatment in step (S20) is 1.5 × 10 4 If less than Pa In this case, the surface of the raw manganese is not sufficiently oxidized, and it is difficult to form a sufficient manganese oxide film. The partial pressure of oxygen in the first heat treatment is 8×10 4 If the temperature exceeds 1 Pa, manganese is Excessive oxidation may affect subsequent purification processes. The partial pressure of oxygen in the first heat treatment is 1.5×10 4 Pa or more 8×10 4 Pa or less The partial pressure of oxygen is preferably 2×10 4 Pa or more 6×10 4 Pa or less When the treatment temperature in the first heat treatment is less than 40° C., the surface of the raw manganese In the first heat treatment, the manganese oxide film is not sufficiently formed. If the treatment temperature is higher than 200°C, manganese is excessively oxidized, resulting in This may affect the subsequent refining process. Therefore, the treatment temperature in the first heat treatment is The treatment temperature is preferably 40° C. or higher and 200° C. or lower. The treatment temperature is more preferably 50° C. or higher. The treatment time in the first heat treatment is set to 150° C. or less from the viewpoint of forming a sufficient oxide film. The treatment time is preferably from 1 hour to 48 hours. The treatment time is more preferably from 3 hours to 3 hours. Less than 6 hours.

[0021] Next, referring to FIG. 1, a step (S30) of obtaining high purity manganese is carried out. More specifically, manganese vapor is produced by heating the raw manganese with an oxidized surface. After the manganese vapor is generated, high purity manganese is obtained by cooling the manganese vapor. In the process of obtaining high-purity manganese, the raw manganese is heated to sublimate it. After manganese vapor is generated, the vapor is cooled to obtain high-purity manganese (hereinafter referred to as "manganese vapor"). The purification equipment used in the sublimation method is a crucible in which the raw manganese is placed. a heating section for heating the raw manganese; and a cooling section for cooling the manganese vapor. Equipped with.

[0022] An example of the sublimation method according to the present embodiment will be specifically described. First, The manganese raw material is placed in a crucible in a refining device. The inside of the crucible is evacuated to remove the manganese from the crucible. The inside of the crucible is evacuated and the manganese raw material is heated to 500℃. Preheating may be performed by heating the material to about 1000° C. and maintaining the temperature for about 1 hour. By applying this treatment, it is possible to reduce the volatile impurities contained in the raw manganese. While maintaining a vacuum inside the vessel, the raw manganese is heated to a temperature range of 1000°C to 1200°C. The sublimation process is carried out by holding the temperature at 40°C for 20 to 50 hours. The gaseous vapor is cooled in the cooling section of the purification plant and condensed into a solid, high-purity If the sublimation temperature is less than 1000°C, the manganese obtained is The rate of evolution will be slow, and it may take a long time to obtain high-purity manganese. If the temperature exceeds 1200℃, the raw manganese may partially melt depending on the loading conditions of the raw materials. The liquid manganese produced by melting in this way may enter the refining equipment. Adherence to the walls can damage the inner walls of the refinery and result in the sublimation of the resulting impurities. This may result in contamination of the high purity manganese. The temperature is preferably 1000° C. or higher and 1200° C. or lower. The vacancy is 10 -5 The pressure is preferably from 1 Pa to 1 Pa. Until the mass of the residue is 20% to 40% by mass of the initial mass of the raw manganese It is preferable to implement this.

[0023] According to the sublimation method, impurities with a higher vapor pressure than manganese are cooled in the cooling section of the refining device. The manganese is condensed in a region at a lower temperature than the region where the manganese is condensed. Impurities at low pressure remain as residues of the raw manganese. In this way, the purity is improved. Therefore, high purity manganese can be obtained.

[0024] Here, the first heat treatment in the method for producing high purity manganese in this embodiment is carried out. By this, the surface of the raw manganese is oxidized and a manganese oxide film is formed. When manganese raw material is heated to generate manganese vapor without the formation of an oxide film, Some of the boron contained as an impurity in the raw manganese is released into the manganese vapor as an impurity. By forming an oxide film on the surface of the raw manganese by the above heat treatment, The boron in the manganese feed is captured by the oxide film. As a result, the boron mixed in the manganese vapor is can be reduced.

[0025] In the process for obtaining high purity manganese in the above embodiment, raw manganese is heated. Manganese vapor is generated by sublimation using a gas, and then the manganese vapor is cooled to obtain high-purity manganese. Oxygen, which is contained as an impurity in the raw manganese, has a strong affinity with manganese. Manganese oxide is formed and remains in the residue, and is separated from the manganese vapor. As a result, oxygen contained as an impurity in the raw manganese is absorbed into the manganese vapor. It is possible to prevent the raw manganese from being mixed in as a pure substance. By generating manganese vapor using this method, the oxygen and boron concentrations are sufficiently reduced, resulting in high-purity manganese vapor. Manganese can be obtained.

[0026] Next, a modified example of the method for producing high purity manganese according to the first embodiment will be described. 30) In the process of obtaining high purity manganese, the raw manganese is heated to sublimate it. Instead of generating manganese vapor by heating the manganese raw material, Gun steam may be produced (hereinafter, also referred to as distillation purification method).

[0027] An example of the above-mentioned distillation purification method will be specifically described. As with the sublimation method, The raw manganese is placed in a crucible in the refining apparatus. The crucible is evacuated to remove the manganese from the crucible. The inner space is evacuated. Preheating may be performed as in the sublimation method. Next, the inside of the crucible is heated. While maintaining a vacuum state, the raw manganese is kept at a temperature range of 1250℃ to 1300℃. By carrying out the evaporation process, the raw manganese melts and becomes liquid manganese. Manganese vapor is produced by the evaporation of liquid manganese. The manganese vapor is cooled in the cooling section of the refining equipment and condensed to form a solid, high-purity manganese. If the evaporation temperature is less than 1250°C, manganese can be obtained. If the evaporation temperature exceeds 1300°C, the gun may not melt sufficiently. In this case, the inner wall of the refining device reacts with the manganese vapor, causing impurities to be added to the manganese vapor. Therefore, the processing temperature in the evaporation process should be 1250°C or higher. The temperature is preferably 300° C. or less. The degree of vacuum during the evaporation process is 10 -3 Pa The distillation purification method is preferably carried out under a pressure of 10 Pa or less. The evaporation process can be performed at a vacuum level of 10 Pa or more. If the evaporation rate is too low, it may take a long time to obtain high-purity manganese. The mass of the manganese feed residue is 10% to 40% by mass of the initial mass of the manganese feed It is preferable to carry out the evaporation treatment until the above-mentioned

[0028] In the refinery, areas that liquid manganese may come into contact with must be protected from manganese oxide, such as alumina. It is desirable to protect the liquid manganese with a material that does not react easily with the metal. Even if the material adheres to the inner wall of the manufacturing equipment, it reduces the introduction of impurities into the high purity manganese. can be done.

[0029] According to the above-mentioned distillation purification method, impurities with a higher vapor pressure than manganese are removed by cooling in the purification equipment. The manganese in the cooling section is condensed in a region that is lower in temperature than the region where the manganese is condensed. Impurities with low vapor pressure remain as residues of the raw manganese. In the above-mentioned distillation purification method, liquid manganese can be obtained. When the liquid is generated, the less dense oxides of manganese are deposited on the surface of the liquid. Boron contained as an impurity in the gun is captured by the oxide. This can reduce the amount of boron that gets mixed into the gun steam.

[0030] In the process for obtaining high purity manganese in the above embodiment, raw manganese is heated. Manganese vapor is then evaporated by a gas to produce manganese vapor, which is then cooled to produce high-purity manganese. This distillation purification method can obtain high-purity manganese in a shorter time than the sublimation method. Therefore, high purity manganese can be obtained at a lower cost.

[0031] (Embodiment 2) Next, a second embodiment of the method for producing high purity manganese according to the present invention will be described. The method for producing high purity manganese in the second embodiment is basically the same as the method for producing the first embodiment. However, in the second embodiment, the step (S10) Instead of the above, a step of preparing a raw material (S40), a step of purifying the aqueous manganese chloride solution (S5 0) and the step (S60) of obtaining electrolytic manganese. The following mainly describes the differences from the first embodiment. .

[0032] Referring to FIG. 2, in the method for producing high purity manganese in the second embodiment, first, In step (S40), a step of preparing a raw material is carried out. In this embodiment, manganese A raw material containing at least one of manganese chloride and manganese dioxide is prepared. Next, in step (S50), a step of purifying the aqueous manganese chloride solution is carried out. An example of a process for purifying an aqueous manganese chloride solution will now be described in detail. First, the above raw material is dissolved in hydrochloric acid. The manganese chloride solution is prepared by dissolving manganese in water. The manganese concentration is, for example, 1 The manganese chloride solution is then mixed with an aqueous ammonia solution. Then, for example, a manganese chloride aqueous solution having a pH of 2 to 7 is prepared. A step of contacting the aqueous manganese chloride solution with a chelating resin is carried out. More specifically, The manganese chloride solution is then poured into a glass or vinyl chloride column packed with a chelating resin. The solution is passed through the filter. The chelating resin in this embodiment is an iminodiacetic acid type chelating resin. The flow rate of the aqueous manganese chloride solution through the column is, for example, 1 SV (Space Velocity) or more and less than 10SV. Iron (Fe), aluminum, Metal impurities of aluminum (Al) and chromium (Cr) are adsorbed by iminodiacetic acid type chelating resin. This makes it possible to reduce the amount of the metal impurities contained in the raw material. Such a step of purifying the aqueous manganese chloride solution may be carried out repeatedly.

[0033] When the pH of the manganese chloride solution is less than 2, it is difficult to react with iminodiacetic acid type chelating resin. However, there is a risk that the adsorption rate of the metal impurities iron, aluminum, and chromium contained in the above-mentioned If the pH of the manganese chloride solution exceeds 7, manganese hydroxide may precipitate. For this reason, the pH of the manganese chloride aqueous solution is preferably 2 or more and 7 or less. When the flow rate of the manganese aqueous solution through the column is less than 1SV, the purified chloride It takes a long time to obtain the manganese solution. If the SV exceeds 0 SV, the above metal impurities may be difficult to adsorb to the chelating resin. Therefore, the flow rate of the manganese chloride solution is 1SV or more and 10SV or less. It is preferable that

[0034] Next, in step (S60), a step of obtaining electrolytically won manganese is carried out. In the method, manganese is electrolytically deposited using the purified aqueous manganese chloride solution as an electrolyte. An example of the electrolytic treatment is described below. An electrolyte solution is prepared by adding ammonium chloride as a buffer to the above-mentioned manganese chloride aqueous solution. The concentration of manganese in the electrolytic solution is, for example, 5 g / L or more and 60 g / L or less. The concentration of ammonium chloride in the electrolyte is, for example, 80 g / L or more and 150 g / L or less. Next, electrolysis is carried out using the electrolytic solution. The current density in the electrolysis is, for example, 50mA / cm 2 More than 120mA / cm 2 In the above electrolytic treatment, an appropriate amount By adding an aqueous ammonia solution to the electrolyte, the pH is kept between 4 and 7. In this way, smooth plate-shaped electrolytic manganese is formed. If the pH of the electrolyte used is less than 4, the electrolytic manganese is likely to be re-eluted into the electrolyte. If the pH exceeds 7, manganese hydroxide is likely to precipitate in the electrolyte. Therefore, the pH of the electrolytic solution in the electrolytic treatment is preferably 4 or more and 7 or less. By carrying out the electrolytic treatment as described above, the alkali metals and alkaline earth metals contained in the raw materials are Metal impurities can be reduced.

[0035] The electrolytically won manganese obtained by the above process is used as raw manganese, and the process (S20) and The steps (S30) and (S31) are carried out in the same manner as in the first embodiment. Similarly to the first embodiment, the oxygen concentration and the boron concentration are sufficiently low by the manufacturing method of the silicon nitride. Thus, reduced high purity manganese can be obtained.

[0036] In the above embodiment, manganese, manganese chloride and and manganese dioxide. However, this is not limited to this, and any manganese raw material with a purity of 99.9% by mass (3N) or more can be used. Alternatively, raw manganese having an oxygen concentration of 570 mass ppm or less may be used. The oxygen concentration of the manganese feed is preferably 535 mass ppm or less, more preferably 50 By using such raw manganese, the high purity manganese The oxygen and boron concentrations in the silicon substrate can be further reduced. EXAMPLES

[0037] A sample was prepared by the method for producing high purity manganese disclosed above, and the oxygen concentration and HO were measured. An experiment was conducted to confirm the effect of reducing uric acid concentration. The procedure for the experiment was as follows.

[0038] (Examples 1 to 3) Electrolytic manganese with an oxygen concentration of 490 mass ppm and a boron concentration of 20 mass ppm was used as the raw material. Manganese was prepared as manganese. The raw manganese was pretreated by washing it with water and alcohol. Next, the partial pressure of oxygen is 8×10 4 In an atmosphere adjusted to 1 Pa, the raw manganese The first heat treatment was carried out at a temperature of 50° C. for 15 hours. 10 kg of the treated manganese raw material was placed in a crucible and preheated. Vacuum degree 10 -4 ~10 -3 The experiment was carried out under the conditions of heating to 500°C in the range of 1 Pa and holding for 1 hour. After the preheating, the raw manganese that had been subjected to the first heat treatment was heated to about 1080°C. The sublimation process was carried out for 30 hours. The manganese vapor was cooled in a high-purity alumina cooling section, and a sample weighing approximately 6 kg ( Example 1) was produced. The partial pressure of oxygen in the first heat treatment was 3.5 × 10 4 Pa, processing temperature A sample (Example 2) was prepared in the same manner as in Example 1, except that the temperature was 150° C. and the treatment time was 3 hours. The partial pressure of oxygen in the first heat treatment was 2×10 4 Pa, processing temperature 45℃, processing time A sample (Example 3) was prepared in the same manner as in Example 1, except that the heating time was 36 hours.

[0039] (Examples 4 to 6) Electrolytic manganese with an oxygen concentration of 490 mass ppm and a boron concentration of 20 mass ppm was used as the raw material. Manganese was prepared by washing the raw manganese with pure water and dissolving it in hydrochloric acid. The manganese chloride aqueous solution was prepared by adding ammonium chloride and pure water to the manganese chloride aqueous solution. To prepare an aqueous solution of manganese chloride and ammonium chloride, The manganese concentration in the aqueous solution of ammonium chloride and ammonium chloride is 50 g / L. The concentration of manganese chloride and ammonium chloride was adjusted to pH 6. The pH of the manganese chloride and manganese chloride solution was adjusted by adding an appropriate amount of ammonia solution. The aqueous solution of ammonium chloride and iminodiacetic acid type chelating resin (manufactured by Unitika, product name "UR The aqueous solution of manganese chloride and ammonium chloride was passed through a column packed with The solution was purified by column chromatography of aqueous solutions of manganese chloride and ammonium chloride. The flow rate was set to 5 SV. The column was packed with 7 L of iminodiacetic acid type chelating resin. was used.

[0040] Electrolysis was carried out using 30L of purified manganese chloride and ammonium chloride aqueous solution as the electrolyte. The current density in the electrolytic treatment was 100mA / cm 2 In electrolytic processing, In this case, an appropriate amount of aqueous ammonia was added to the electrolyte to maintain the pH at about 6. Thus, a smooth plate-like electrolytic manganese was formed. For 10 kg of manganese, the partial pressure of oxygen is 2.5 x 10 4 In an atmosphere adjusted to Pa The first heat treatment was carried out by heating the sample to 200° C. and holding the sample for 1 hour. The electrolytic manganese that had been treated was placed in a crucible and preheated. , degree of vacuum 10 -4 ~10 -3 The experiment was carried out under the conditions of heating to 500°C under a pressure of 1 Pa and holding for 1 hour. After the preheating, the electrolytic manganese that had been subjected to the first heat treatment was heated to about 1270°C. The mixture was then subjected to evaporation treatment (distillation purification method) for 6 hours. The generated manganese vapor is cooled in a high-purity alumina cooling section and about 7 kg of sample is The partial pressure of oxygen in the first heat treatment was 3×10 4 Pa, processing The sample (Example 5) was prepared in the same manner as in Example 4, except that the temperature was 60° C. and the treatment time was 20 hours. The partial pressure of oxygen in the first heat treatment was set to 4.5×10 4 Pa, processing temperature 80℃ A sample (Example 6) was prepared in the same manner as in Example 4, except that the treatment time was 12 hours. It was.

[0041] (Examples 7 to 9) For 10 kg of electrolytically won manganese produced by carrying out electrolytic treatment in the same manner as in Example 4, The partial pressure of oxygen is 4×10 4 Heat to 40°C in an atmosphere adjusted to 100 Pa for 48 hours. The electrolytic manganese that had been subjected to the first heat treatment was The same sublimation treatment as in Example 1 was carried out using the above material to prepare a sample (Example 7). 1 The partial pressure of oxygen during heat treatment is 6 x 10 4 Pa, treatment temperature 100℃, treatment time 6 hours A sample (Example 8) was prepared in the same manner as in Example 7, except that The partial pressure of oxygen is 1.5×10 4 The treatment temperature was 120°C and the treatment time was 10 hours. A sample (Example 9) was prepared in the same manner as in Example 7.

[0042] (Comparative Examples 1 and 2) The partial pressure of oxygen in the first heat treatment is 9×10 4Pa, treatment temperature 50℃, treatment time 15 hours A sample (Comparative Example 1) was produced in the same manner as in Example 1, except that the first heat treatment was performed as follows. The partial pressure of oxygen in 4 The treatment temperature was 150°C and the treatment time was 0.5 hours. Other than that, a sample (Comparative Example 2) was produced in the same manner as in Example 1.

[0043] (Comparative Examples 3 and 4) The partial pressure of oxygen in the first heat treatment is 2.5×10 4 Pa, treatment temperature 250℃, treatment time 1 A sample (Comparative Example 3) was produced in the same manner as in Example 4, except that the first heat treatment time was changed to 100 s. The partial pressure of oxygen in the 4 Pa, treatment temperature 35℃, treatment time 20 hours A sample (Comparative Example 4) was prepared in the same manner as in Example 4.

[0044] (Comparative Examples 5 and 6) The partial pressure of oxygen in the first heat treatment is 4×10 4 Pa, treatment temperature 40℃, treatment time 60 hours A sample (Comparative Example 5) was prepared in the same manner as in Example 7, except that the first heat treatment was performed as follows. The partial pressure of oxygen in 4 The treatment temperature was 100°C and the treatment time was 6 hours. A sample (Comparative Example 6) was prepared in the same manner as in Example 7.

[0045] (Oxygen and boron concentration measurements) The oxygen concentration and the HO concentration of the samples of Examples 1 to 9 and Comparative Examples 1 to 6 were The urinary concentration was measured. The oxygen concentration was measured by infrared absorption method. The LECO "ONH836" was used. The boron concentration was measured by the GDMS method. The above measurement device was "Element GD" manufactured by Thermo Scientific. was used. Table 1 shows the measurement results of the oxygen concentration and boron concentration of the samples of Examples 1 to 9 and Comparative Examples 1 to 6. In the purification method of Table 1, I represents the sublimation method. II represents the distillation purification method. III represents the electrolytic treatment. "I,III" indicates that the electrolytic treatment and the sublimation method are carried out as the purification method. Similarly, "II,III" indicates that the electrolytic treatment and the distillation purification method are carried out as the purification method. Table 2 shows the degree of possibility that the characteristics of the semiconductor device deteriorate in the samples of Examples 1 to 9 and Comparative Examples 1 to 6. In Table 2, A indicates that the possibility that the characteristics of the semiconductor device deteriorate is extremely low . B indicates that the possibility that the characteristics of the semiconductor device deteriorate is low. C indicates that the possibility that the characteristics of the semiconductor device deteriorate is high. D indicates that the possibility that the characteristics of the semiconductor device deteriorate is extremely high. The above A to D have a relationship of A < B < C < D with respect to the degree of possibility that the characteristics of the semiconductor device deteriorate.

[0046]

Table 1

[0047]

Table 2

[0048] Referring to Table 1, for the samples (Examples 1 to 9) where the partial pressure of oxygen in the first heat treatment is 1.5×10 4 Pa or more and 8×10 4 Pa or less, the treatment temperature is 40°C or more and 200°C or less, and the treatment time is 1 hour or more and 48 hours or less, in the samples (Comparative Examples) where the first heat treatment deviates from the above range ​​​​​​Compared with Example 1 to Comparative Example 6, the oxygen concentration and boron concentration can be reduced. In the samples (Examples 1 to 9) in which the heat treatment was performed within the above range, the oxygen concentration was kept at 3 ppm by mass or less. In addition, the boron concentration can be reduced to 3 mass ppm or less. In the sample of Example 9, it was confirmed that the oxygen concentration and the boron concentration were sufficiently reduced. can be.

[0049] In the samples (Examples 7 to 9) in which electrolysis and sublimation (sublimation method) were performed, In comparison with the samples (Examples 1 to 3) in which only the sublimation process was performed without the electrolysis process, In all cases, the oxygen concentration and boron concentration can be further reduced. It is preferable to use electrolytically extracted manganese as raw manganese. In the samples that underwent the fluorination treatment (Examples 7 to 9), the electrolysis treatment and the evaporation treatment (steaming) were performed. The oxygen concentration and boron concentration were higher than those of the samples (Examples 4 to 6) in which the distillation purification method was performed. Therefore, the method for producing high purity manganese is as follows: It is more preferable to carry out electrolysis and sublimation.

[0050] With reference to Table 2, in the samples of Example 1 to Example 9, the samples of Comparative Example 1 to Comparative Example 6 It is believed that the characteristics of semiconductor devices are less likely to deteriorate than in the case of electrolytic processing and The samples (Examples 7 to 9) in which the sublimation process was performed had characteristic semiconductor device properties. It is considered that it will be difficult for the

[0051] From the above experimental results, it can be seen that the method for producing high purity manganese according to the present disclosure not only improves the oxygen concentration but also It is confirmed that high purity manganese with a sufficiently reduced boron concentration can be obtained.

[0052] The embodiments disclosed herein are illustrative in all respects and are not restrictive in any respect. It should be understood that the scope of the invention is as set forth in the claims, not the above description. The scope of the claims is defined by the meaning and scope of the claims, and all modifications within the scope of the claims are within the scope of the claims. is intended to be included. [Industrial Applicability]

[0053] The method for producing high purity manganese disclosed herein is to adjust the oxygen concentration and boron concentration of high purity manganese. This is particularly advantageous when a reduction in

Claims

1. An additive for a wiring material for a semiconductor device, comprising high-purity manganese having an oxygen content of 3 ppm by mass or less and a boron content of 3 ppm by mass or less.

2. A copper wiring to which high-purity manganese having an oxygen content of 3 ppm by mass or less and a boron content of 3 ppm by mass or less has been added.

3. A sputtering target material using high purity manganese having an oxygen content of 3 ppm by mass or less and a boron content of 3 ppm by mass or less.

Citation Information

Patent Citations

  • High pure metallic manganese

    JP1977114512A

  • Production of high purity mn material, and high purity mn material for thin film formation

    JP1999152528A

  • Method for producing high purity manganese

    JP2002285373A

  • High-purity manganese and method for producing the same

    JP2013142184A

  • High purity manganese

    JP2016180184A