Method for separating As and Sb

The Sb precipitation process with controlled redox potential and pH conditions effectively separates Sb from As in metal smelting solutions, achieving high Sb recovery with minimal As loss.

JP7594930B2Active Publication Date: 2024-12-05DOWA METALS & MINING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021022307
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-16
Publication Date
2024-12-05
Estimated Expiration
2041-02-16

AI Technical Summary

Technical Problem

Existing methods fail to effectively separate arsenic (As) and antimony (Sb) from solutions produced in metal smelting due to their mixture in precipitates, necessitating a separate process.

Method used

A method involving an Sb precipitation process that includes a reduction step followed by a neutralization step, with specific redox potential (ORP) and pH conditions, optionally with a Cu source addition, to selectively precipitate Sb while leaving As in solution.

Benefits of technology

Achieves high Sb removal rates while maintaining low As removal rates, ensuring efficient separation and recovery of both elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594930000001
    Figure 0007594930000001
  • Figure 0007594930000002
    Figure 0007594930000002
Patent Text Reader

Abstract

To selectively deposit Sb between As and Sb, thereby separating Sb from As.SOLUTION: A method for separating Sb from As includes an Sb deposition process for depositing Sb from a solution that contains Cu, As, and Sb, with the dissolved Sb having concentration of 1.0 g / L or more, a concentration ratio Cu / As of 0.10 or more and a concentration ratio Cu / Sb of 0.10 or more. The Sb deposition process includes an Sb reduction step and a neutralization step in the stated order. At the finish of the Sb reduction step, ORP (3.3M KCl-Ag / AgCl) is 70-210 mV. There are also provided techniques relating thereto.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for separating As and Sb, and more particularly to a method for separating As and Sb from a solution produced in metal smelting. [Background technology]

[0002] Patent Document 1 describes a method for separating arsenic and antimony in an aqueous arsenic acid solution, which comprises: a step (A) of blowing sulfur dioxide gas into an aqueous arsenic acid solution containing antimony to reduce the arsenic and antimony and obtain a precipitate containing arsenous acid (As2O3) and diantimony trioxide (Sb2O3); and a step (B) of adding the precipitate to warm water having a temperature of 70 to 100°C to dissolve the arsenous acid in the precipitate and obtain an aqueous arsenous acid solution and an undissolved residue containing antimony.

[0003] Patent Document 2 describes a method for recovering bismuth, which comprises neutralizing an acidic solution containing bismuth to precipitate bismuth salts, reducing a solution containing the precipitates, and separating and recovering bismuth from coexisting metals, in which the neutralization is carried out in two stages at room temperature, adjusting the pH of the bismuth-containing solution to 0.5-1.5 over 60 minutes or more in the first neutralization to precipitate coexisting metals that precipitate in that pH range, filtering out the precipitate, and then adjusting the pH of the filtrate to 2-3 in the second neutralization to produce a precipitate containing bismuth, recovering this bismuth-containing precipitate and dissolving it in hydrochloric acid, and reducing the solution with iron to recover the precipitated metallic bismuth. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-167442 A [Patent Document 2] JP 2013-155432 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the case of the method described in Patent Document 1, As and Sb are mixed in the precipitate, so a separate process for separating As and Sb is required. The main point of the method described in Patent Document 2 is a method for recovering bismuth.

[0006] An object of the present invention is to separate As and Sb by selectively precipitating Sb from As and Sb. [Means for solving the problem]

[0007] The first aspect of the present invention is The method includes a step of precipitating Sb from a solution containing Cu, As, and Sb, the solution having a concentration of dissolved Sb of 1.0 g / L or more, a concentration ratio of Cu / As of 0.10 or more, and a concentration ratio of Cu / Sb of 0.10 or more, The Sb precipitation step includes an Sb reduction step and a neutralization step in this order, The ORP (3.3M KCl-Ag / AgCl) at the start of the neutralization process is 70 to 210 mV. This is a method for separating As and Sb.

[0008] The second aspect of the present invention is the method according to the first aspect, The above solution is the solution at the start of the Sb reduction process.

[0009] A third aspect of the present invention relates to a method for producing a composition according to the second aspect, A Cu source addition step is included before the Sb reduction step.

[0010] A fourth aspect of the present invention is any one of the first to third aspects, The pH at the start of the neutralization step is 0.9 to 3.0.

[0011] A fifth aspect of the present invention is any one of the first to fourth aspects, The ORP at the end of the neutralization process is 130 to 350 mV.

[0012] A sixth aspect of the present invention is any one of the first to fifth aspects, The pH at the start of the Sb reduction step is 0.5 to 2.0.

[0013] A seventh aspect of the present invention is any one of the first to sixth aspects, The ORP at the start of the Sb reduction process is 100 to 700 mV. Effect of the Invention

[0014] According to the present invention, it is possible to separate As and Sb by selectively precipitating Sb out of As and Sb. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] This embodiment relates to a method for separating As and Sb. In this specification, "~" indicates a value greater than or equal to a predetermined value and less than or equal to a predetermined value. In this embodiment, element symbols such as "As" and "Sb" indicate metal elements or ions. Hereinafter, concentration ratio means wt ratio, and % means wt%.

[0016] The solution to be treated in this embodiment is, for example, a solution generated in metal smelting (particularly zinc smelting). "Separating As and Sb" specifically means precipitating Sb from the solution while leaving As in the solution.

[0017] In this embodiment, an Sb precipitation step is performed to precipitate Sb from a solution. The Sb precipitation step includes, in this order, a reduction step to reduce Sb in a solution, and a neutralization step to neutralize the solution after the reduction step to precipitate reduced Sb. Hereinafter, the solution before the start of the reduction step is also referred to as a pre-treatment solution, the solution after the start of the reduction step or before the end of the neutralization step is also referred to as a treatment solution, and the solution after the end of the neutralization step is also referred to as a treatment solution.

[0018] [Aspect 1] In this embodiment, a case where Cu is previously present in the pre-treatment solution will be exemplified.

[0019] The pre-treatment solution in this embodiment should have the following characteristics: Contains Cu, As, and Sb. - The concentration of dissolved Sb is 1.0g / L or more. The concentration ratio Cu / As is 0.10 or more, and the concentration ratio Cu / Sb is 0.10 or more.

[0020] Preferably, Cu, As, and Sb in the pre-treatment solution are all ionized (including complex ions) and dissolved in the solution.

[0021] The concentration of Sb dissolved in the pre-treatment solution is 1.0 g / L or more, and the pre-treatment solution of this embodiment is different from the solution described in Patent Document 2 which is intended for the recovery of bismuth.

[0022] The lower limit of the concentration of Sb dissolved in the pre-treatment solution may be 1.5 g / L or 2.0 g / L, and the upper limit of the concentration may be 20 g / L, 15 g / L, or 10 g / L.

[0023] The concentration of As dissolved in the pre-treatment solution is not limited, but the lower limit of the concentration may be 1 g / L, 10 g / L, or 20 g / L, and the upper limit of the concentration may be 200 g / L or 100 g / L.

[0024] The concentration of Cu dissolved in the pre-treatment solution is not limited, but the lower limit of the concentration may be 10 g / L, 20 g / L, or 25 g / L, and the upper limit of the concentration may be 150 g / L, 100 g / L, or 80 g / L.

[0025] However, the concentration ratio Cu / As in the solution before treatment is 0.10 or more, and the concentration ratio Cu / Sb is 0.10 or more.

[0026] The lower limit of the Cu / As concentration ratio in the pre-treatment solution may be 1, 3, or 5. The upper limit of the Cu / As concentration ratio may be 50 or 30.

[0027] The lower limit of the concentration ratio Cu / Sb in the pre-treatment solution may be 0.3 or 0.5, and the upper limit of the concentration ratio Cu / Sb may be 5, 3, or 2.

[0028] The lower limit of the concentration ratio As / Sb in the pre-treatment solution may be 0.1, 1, or 5. The upper limit of the concentration ratio As / Sb may be 50, 30, or 20.

[0029] The lower limit of the concentration ratio Cu / (Sb+As) in the pre-treatment solution may be 0.1. The upper limit of the concentration ratio Cu / (Sb+As) may be 5.

[0030] The above-mentioned concentration settings for As and Sb in the pre-treatment solution include the concentration values ​​of As and Sb in the solution produced in metal smelting (particularly zinc smelting). On the other hand, if the above-mentioned concentration setting for Cu in the pre-treatment solution is not met in the solution produced in metal smelting (particularly zinc smelting), a Cu source may be added separately to the pre-treatment solution (Cu source addition step). The Cu source to be added separately is preferably water-soluble, for example, copper sulfate (CuSO4) (hydrates can also be used). In this case, divalent copper ions will be present in the pre-treatment solution.

[0031] An example of the composition of the pre-treatment solution is as follows: As: 0.2-100g / L Sb: 0.05-10g / L Cu: 0.1-100g / L Heavy metals other than those mentioned above (Cd, Co, Ni, Pb, Zn, etc.): 1g / L or less

[0032] The lower limit of the pH of the pre-treatment solution may be 0.5 or may exceed 1.0. The upper limit of the pH of the pre-treatment solution may be 3.0 or 2.0. As these numerical ranges indicate, the pre-treatment solution is acidic. The pH value in this specification is the value in a state where the change has settled (for example, the change in 10 minutes is within 0.1). The pH of the pre-treatment solution may be rephrased as the pH at the start of the Sb reduction process.

[0033] In this specification, ORP (3.3M KCl-Ag / AgCl) is +199 mV (vs. SHE, 25°C) against a standard electrode, which is the so-called oxidation-reduction potential (vsAg / AgCl). Hereinafter, ORP will have the same definition. In addition, the ORP value in this specification is the value in a state where the change has settled (for example, the change in 10 minutes is within 10 mV). The ORP of the pre-treatment solution may be rephrased as the ORP at the start of the Sb reduction process.

[0034] The lower limit of the ORP of the pre-treatment solution may be 100 mV, 150 mV, or 200 mV. The upper limit of the ORP of the pre-treatment solution may be 700 mV or 600 mV.

[0035] The pre-treatment solution is subjected to a reduction process of Sb. Specifically, a reducing agent is added to the pre-treatment solution. There is no limitation on the reducing agent, but examples include at least one of sulfur dioxide (SO2) (gas injection can also be used) and sodium sulfite (NaHSO3).

[0036] The temperature of the solution during the Sb reduction step may be 40 to 95° C. The reaction time of the Sb reduction step may be 30 to 150 minutes.

[0037] The lower limit of the pH of the solution being treated after the Sb reduction step may be 0.9, 1.0, more than 1.0, 1.5, or 2.0. The upper limit of the pH of the solution being treated after the Sb reduction step may be 3.0 or 2.5. The pH of the solution being treated after the Sb reduction step may be rephrased as the pH at the start of the neutralization step.

[0038] The ORP of the solution being treated after the Sb reduction step is set to 70 to 210 mV. This allows sufficient Sb precipitation after the neutralization step. In other words, it is possible to improve the value (Sb removal rate) obtained by subtracting the percentage of the concentration of Sb dissolved in the solution after the neutralization step (after separation of precipitated Sb) from 100 relative to the concentration of Sb dissolved in the solution before treatment.

[0039] The lower limit of the ORP of the solution being treated after the Sb reduction step may be 100 mV, 110 mV, or 130 mV. The upper limit of the ORP of the solution being treated after the Sb reduction step may be 190 mV or 170 mV. The ORP of the solution being treated after the Sb reduction step may be rephrased as the ORP at the start of the neutralization step.

[0040] Regarding the concentration ratios Cu / As, Cu / Sb, As / Sb, and Cu / (Sb+As) in the in-process solution after the Sb reduction step, since almost no As or Sb precipitates in the Sb reduction step of the present invention and no solid-liquid separation step is performed on the in-process solution, the same concentration ratios as in the pre-processing solution can be applied.

[0041] The reduction rates (particularly the reduction rate of the As concentration) from the concentrations of As, Sb, and Cu dissolved in the pre-treatment solution before the Sb reduction step and the concentration ratios of each element dissolved in the pre-treatment solution, Cu / As, Cu / Sb, As / Sb, and Cu / (Sb+As), to the concentrations and concentration ratios of each element dissolved in the treatment solution after the Sb reduction step may be 2% or less, or 1% or less.

[0042] The solution in process after the Sb reduction step is subjected to a neutralization step to precipitate the reduced Sb. There is no limitation on the additives as long as they can increase the pH of the solution in process after the reduction step, but for example, an alkali (one example being at least one of calcium carbonate (CaCO3) and sodium hydroxide (NaOH)) may be added. Gypsum (CaSO4) is also an example of such an additive.

[0043] The temperature of the solution during the neutralization step may be 40 to 95° C. The reaction time of the neutralization step may be 30 to 150 minutes.

[0044] The pH of the post-processing solution after the neutralization step may be higher than the pH of the processing solution after the reduction step and before the neutralization step. In addition, the lower limit of the pH of the post-processing solution after the neutralization step is preferably 2.5 or 3.0. The upper limit of the pH of the post-processing solution after the neutralization step is preferably 4.0.

[0045] The lower limit of the ORP of the treated solution after the neutralization step may be 50 mV, 80 mV, 100 mV, 130 mV. The upper limit of the ORP of the treated solution after the neutralization step may be 350 mV, 300 mV, 280 mV.

[0046] If the pH and ORP of the treated solution after the neutralization step are in the above-mentioned ranges, Sb can be sufficiently precipitated and As can be sufficiently left in the treated solution. In other words, the value obtained by subtracting the percentage of the As concentration (after separation of precipitated As) dissolved in the treated solution after the neutralization step relative to the As concentration dissolved in the pre-treatment solution from 100 (As removal rate) can be kept low, while the Sb removal rate can be improved.

[0047] The As removal rate in the solution after solid-liquid separation of the treated solution is 33% or less, preferably 25% or less. The Sb removal rate in the solution after solid-liquid separation is 75% or more, preferably 80% or more. However, it is preferable that both the As removal rate and the Sb removal rate are adequately good. Therefore, the lower limit of the value of (100-As removal rate) x Sb removal rate may be 6600, 7000, 7500, or 8000.

[0048] The Cu removal rate in the solution after solid-liquid separation may be 25% or less, or 15% or less. The Cu removal rate in the solution after solid-liquid separation may be 25% or less, or 15% or less. In addition, the Cu removal rate in the solution after solid-liquid separation may be 25% or less, or 15% or less.

[0049] There is no limitation on the concentration ratio Cu / As in the solution after solid-liquid separation of the treated solution, but the lower limit may be 0.2, 0.6, 1.0, or 1.4, and the upper limit may be 2.0 or 1.6.

[0050] There is no limitation on the concentration ratio Cu / Sb in the solution after solid-liquid separation of the treated solution, but the lower limit may be 10 or 60, and the upper limit may be 20,000, 2,000, 600, 200, 100, or 70.

[0051] There is no limitation on the concentration ratio As / Sb in the solution after solid-liquid separation of the treated solution, but the lower limit may be 40 and the upper limit may be 25,000, 800, or 600.

[0052] Agitation may be performed during the reduction and neutralization steps, for example using a stirrer or tilted paddle.

[0053] In this embodiment, the neutralization step is started after the reduction step is completed, but the present invention is not limited thereto. For example, the neutralization step may be started just before the reduction step is completed. In this case, the above-mentioned definitions of the pH and ORP of the solution being treated are applicable to the pH and ORP values ​​at the start of the neutralization step.

[0054] The method for separating As and Sb described in this embodiment can also be applied to a method for separating and recovering Sb and As. For example, a solid-liquid separation process can be performed on the treated solution after the neutralization process, and Sb can be recovered from the solid (residue). In other words, the present invention can also be used as a method for recovering Sb (a method for producing Sb). In addition, the As remaining in the solution after the solid-liquid separation can be used as arsenous acid used in zinc smelting.

[0055] The solid-liquid separation step in this specification may be carried out by a known method, for example, filtration, centrifugation, or the like.

[0056] [Aspect 2] The Cu source may be added to the in-process solution after the reduction step and before the neutralization step, and the Cu concentration may be set to satisfy the above-mentioned concentration setting for Cu in the pre-processing solution in the above-mentioned embodiment 1. Example 5 described later corresponds to embodiment 2.

[0057] In this embodiment, the pre-treatment solution does not contain Cu, or even if it does contain Cu, the above-mentioned concentration setting for Cu is not satisfied. Instead, the pre-treatment solution after the reduction step and before the neutralization step only needs to satisfy the above-mentioned concentration setting for Cu in the pre-treatment solution. The other provisions may be the same as those in the above-mentioned embodiment 1.

[0058] In this specification, the following expressions are used to include both embodiment 1 and embodiment 2. "The method includes a step of precipitating Sb from a solution containing Cu, As, and Sb, the concentration of dissolved Sb being 1.0 g / L or more, the concentration ratio Cu / As being 0.10 or more, and the concentration ratio Cu / Sb being 0.10 or more, The Sb precipitation step includes an Sb reduction step and a neutralization step in this order, The ORP (3.3M KCl-Ag / AgCl) at the end of the Sb reduction process is 70-210mV. This is a method for separating As and Sb. The above expression includes the case where the solution that is the target of the Sb deposition step satisfies the requirement before the Sb reduction step, and the case where the solution satisfies the requirement after the Sb reduction step and before the neutralization step. EXAMPLES

[0059] The present invention will now be described in detail with reference to examples. The present invention is not limited to the following examples. Note that the contents not described below are the same as those described in the present embodiment.

[0060] <Example 1> Residues produced during zinc smelting were dissolved in sulfuric acid to obtain pre-treatment solution X. Details of pre-treatment solution X are as follows. For each example other than Example 1, the following details are shown in Table 1 below. Volume: 400mL ·As concentration: 20g / L ·Sb concentration: 2.0g / L ·Cu concentration: 33g / L Heavy metals other than those mentioned above (Cd, Co, Ni, Pb, Zn, etc.): 1g / L or less pH: 0.69 ORP (3.3M KCl-Ag / AgCl, omitted below): 430mV ·Concentration ratio Cu / As:1.6 ·Concentration ratio Cu / Sb:17 ·Concentration ratio As / Sb:10 In this example, since the pre-treatment solution X already satisfied the regulations regarding the Cu concentration (the concentration ratio Cu / As is 0.10 or more and the concentration ratio Cu / Sb is 0.10 or more), no Cu source was added.

[0061] The reduction process was carried out on the untreated solution X of this example. Specifically, the liquid temperature was set to 60°C, and a predetermined amount of NaHSO3 was added as a reducing agent to the untreated solution X. Then, the solution was stirred for 120 minutes with three inclined paddles (without baffles). Then, an in-process solution was obtained after the reduction process and before the neutralization process. Details of the in-process solution are as follows. For each example other than Example 1, the following details are listed in Table 1 below. pH: 1.6 ORP: 137mV

[0062] Regarding the concentration ratios Cu / As, Cu / Sb, As / Sb, and Cu / (Sb+As) in the solution during treatment, since almost no As or Sb precipitates in the Sb reduction process in the present invention and since no solid-liquid separation process is performed on the solution during treatment, the values ​​were the same as those of solution X before treatment.

[0063] The neutralization process was carried out on the in-process solution of this example. Specifically, the liquid temperature was set to 60°C, and a predetermined amount of CaCO3 was added to the in-process solution as a neutralizing agent. Then, the solution was stirred for 120 minutes with a three-blade inclined paddle (without baffles). Then, a post-processed solution was obtained after the neutralization process. Details of the post-processed solution are as follows. For each example other than Example 1, the following details are listed in Table 1 below. pH: 3.7 ORP: 146mV

[0064] The treated solution was subjected to a solid-liquid separation process using filter paper. Details of the solution after solid-liquid separation are as follows. For each example other than Example 1, the following details are shown in Table 2 below. ·As removal rate: 21% ·Sb removal rate: 99% ·Cu removal rate: 5% ·Concentration ratio Cu / As:1.9 ·Concentration ratio Cu / Sb:1412 ·Concentration ratio As / Sb:726

[0065] [Table 1] [Table 2]

[0066] <Examples 2 to 4> Each example was carried out after changing each setting from Example 1 as shown in Table 1. Details of the solution after solid-liquid separation are shown in Table 2 above.

[0067] <Example 5> In this example, pre-treatment solution Y was prepared using a reagent instead of a smelting residue.

[0068] Specifically, 0.72 g of Sb2O3 was added to 150 mL of pure water heated to 50°C, and sulfuric acid was added to adjust the pH to below 1. Then, a 60% arsenic acid solution was added so that the concentration of As dissolved in the pre-treatment solution Y was about 40 g / L.

[0069] After that, H2O2 was further added to bring the ORP to about 530 mV and the mixture was stirred for about 1 hour using a magnetic stirrer with a thermostatic bath.

[0070] After stirring, 150 mL of the solution obtained was measured and diluted 2-fold with pure water, and the diluted solution was heated to 60° C. to obtain pre-treatment solution Y. (This solution is also the pre-treatment solution according to Comparative Example 1.)

[0071] In Example 5, CuSO4 (flakes) was added to and dissolved in pre-treatment solution Y to prepare a pre-treatment solution with a predetermined Cu concentration.

[0072] Each example was carried out after changing each setting from Example 1 as shown in Table 1. Details of the solution after solid-liquid separation are shown in Table 2 above.

[0073] <Example 6> In Example 6, pre-treatment solution Y was used. Starting from pre-treatment solution Y, the solution was changed to an in-treatment solution after the Sb reduction step and before the neutralization step, and CuSO4 (flakes) was added and dissolved to prepare an in-treatment solution with a specified Cu concentration. In addition, each setting was changed from Example 1 as described in Table 1 above, and each example was carried out. Details of the solution after solid-liquid separation are described in Table 2 above.

[0074] <Comparative Example 1> In Comparative Example 1, pre-treatment solution Y was used. Other than that, each setting was changed from Example 1 as shown in Table 1 above, and each example was carried out. Details of the solution after solid-liquid separation are shown in Table 2 above. The copper concentration of the solution during treatment was 0 g / L.

[0075] <Comparative Examples 2 and 3> Each example was carried out after changing each setting from Example 1 as shown in Table 1. Details of the solution after solid-liquid separation are shown in Table 2. The same pre-treatment solution as in Example 1 was used.

[0076] <Comparative Example 4> In Comparative Example 4, pre-treatment solution Y was used. Starting from pre-treatment solution Y, the solution was changed to an in-treatment solution after the Sb reduction step and before the neutralization step, and CuSO4 (flakes) was added and dissolved to prepare an in-treatment solution with a predetermined Cu concentration. Each example was carried out after changing each setting from Example 1 as shown in Table 1 above. Details of the solution after solid-liquid separation are shown in Table 2 above.

[0077] <Summary> In each Example, a high Sb removal rate was achieved while a low As removal rate was shown. In particular, in Examples 1 to 3 and 5, in which the ORP of the treated solution after the neutralization step was in the range of 80 to 350 mV, a low As removal rate and a high Sb removal rate were achieved in a well-balanced manner.

Claims

1. The method includes a step of precipitating Sb from a solution containing Cu, As, and Sb, the solution having a concentration of dissolved Sb of 1.0 g / L or more, a concentration ratio of Cu / As of 0.10 or more, and a concentration ratio of Cu / Sb of 0.10 or more, The Sb precipitation step includes an Sb reduction step and a neutralization step in this order, A method for separating As and Sb, in which the ORP (3.3M KCl-Ag / AgCl) at the start of the neutralization process is 70 to 210 mV.

2. The method for separating As and Sb according to claim 1 , wherein the solution is a solution at the start of an Sb reduction step.

3. The method for separating As and Sb according to claim 2 , further comprising a step of adding a Cu source before the step of reducing Sb.

4. The method for separating As and Sb according to any one of claims 1 to 3, wherein the pH at the start of the neutralization step is 0.9 to 3.

0.

5. The method for separating As and Sb according to any one of claims 1 to 4, wherein the ORP at the end of the neutralization step is 130 to 350 mV.

6. The method for separating As and Sb according to any one of claims 1 to 5, wherein the pH at the start of the Sb reduction step is 0.5 to 2.

0.

7. The method for separating As and Sb according to any one of claims 1 to 6, wherein the ORP at the start of the Sb reduction step is 100 to 700 mV.

Citation Information

Patent Citations

  • Technological method for separating antimony and arsenic from antimony and arsenic soot

    CN109957660A

  • Method for leaching and separating antimony and tellurium from copper anode mud through controlling potential

    CN110578059A

  • Method for separating arsenic and antimony in arsenic acid aqueous solution

    JP2009167442A

  • Method for producing aqueous arsenous acid solution of high purity from copper removal slime

    JP2010059035A

  • METHOD OF RECOVERING Ir FROM PLATINUM GROUP-CONTAINING SOLUTION

    JP2012167334A