Method for producing water-absorbent resin powder

By employing a twin-screw kneader and gel crushing at elevated temperatures, the method achieves a water-absorbent resin powder with improved water absorption speed and efficiency, addressing size and adherence issues in existing production methods.

JP7595080B2Active Publication Date: 2024-12-05NIPPON SHOKUBAI CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022552033
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-25
Filing Date
2021-09-22
Publication Date
2024-12-05
Estimated Expiration
2041-09-22

AI Technical Summary

Technical Problem

Existing methods for producing water-absorbent resin powder struggle to achieve the desired particle size and water absorption speed, leading to inefficiencies and equipment size issues, with hydrogel adherence causing maintenance challenges and inadequate performance in applications like disposable diapers.

Method used

The method involves using a twin-screw kneader to produce a particulate hydrogel crosslinked polymer, followed by gel crushing at 50°C or higher to achieve a particle size of 3 mm or less, ensuring excellent water absorption rates through continuous pulverization and drying processes.

Benefits of technology

This approach results in a water-absorbent resin powder with enhanced water absorption speed and efficiency, suitable for high-performance applications such as disposable diapers, while minimizing equipment size and maintenance challenges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595080000004
    Figure 0007595080000004
  • Figure 0007595080000005
    Figure 0007595080000005
  • Figure 0007595080000006
    Figure 0007595080000006
Patent Text Reader

Abstract

[Problem] To provide a method for producing a water-absorbing resin powder having an excellent water absorption rate. [Solution] The method for producing a water-absorbing resin powder, according to the present invention, comprises: a polymerization step for polymerizing a monomer aqueous solution to obtain a hydrogel-like crosslinked polymer; a gel pulverization step, after the polymerization step, for pulverizing the hydrogel-like crosslinked polymer using a gel pulverizer to obtain a particulate hydrogel-like crosslinked polymer; and a drying step for drying the particulate hydrogel-like crosslinked polymer to obtain a dried product. The gel pulverizer includes an input port, a discharge port, and a main body having a plurality of rotating shafts. Each of the rotating shafts has a pulverization means, and in the gel pulverization step, the hydrogel-like crosslinked polymer is continuously input from the input port, the hydrogel-like crosslinked polymer is continuously pulverized at 50°C or more by the pulverization means, a particulate hydrogel-like crosslinked polymer is continuously taken out from the discharge port, the polymerization rate of the hydrogel-like crosslinked polymer input into the input port is 90% by mass or more, and the mass average particle diameter d1 in terms of solid content of the particulate hydrogel-like crosslinked polymer discharged from the discharge port is 3 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a water-absorbent resin powder. [Background technology]

[0002] Super absorbent polymers (SAPs) are water-swellable, water-insoluble polymer gelling agents that are widely used in a variety of fields, including absorbent articles such as disposable diapers and sanitary napkins, agricultural and horticultural water retention agents, and industrial water-stopping agents.

[0003] The above-mentioned water absorbent resins use many monomers and hydrophilic polymers as raw materials, but from the viewpoint of water absorption performance, polyacrylic acid (salt)-based water absorbent resins using acrylic acid and / or its salt as a monomer are most widely produced industrially.

[0004] The above-mentioned water-absorbing resin is required to have various functions (higher physical properties) in accordance with the improvement of the performance of paper diapers, which are the main application of the water-absorbing resin. Specifically, in addition to the basic physical properties of water absorption capacity without pressure and water absorption capacity under pressure, various physical properties such as gel strength, water-soluble content, water absorption rate, liquid permeability, particle size distribution, urine resistance, antibacterial properties, damage resistance, powder flowability, deodorizing properties, coloring resistance, low dust, and low residual monomer are required of the water-absorbing resin. In particular, in the application of sanitary products such as paper diapers, further improvement of water absorption rate is desired in accordance with the thinning of products.

[0005]

[0113] A commercial production method of the above-mentioned powdery or particulate water absorbent resin typically includes a polymerization step, a gel crushing (fine grain) step carried out after or simultaneously with the polymerization, a drying step of the finely grained gel, a crushing step of the dried product, a classification step of the crushed product, a recovery step of fine powder generated by the crushing and classification, and a surface cross-linking step of the water absorbent resin powder after classification.

[0006] One of the methods for producing water-absorbent resins proposed so far is a production method in which a polymerization step and a gel crushing step are carried out simultaneously using a polymerization apparatus having a crushing mechanism. In this production method, as the polymerization reaction of the liquid monomer progresses, the generated hydrogel is crushed, and the finely granulated hydrogel is discharged from the polymerization apparatus. As specific examples of this method, methods using a batch kneader or a continuous kneader are shown in Patent Documents 1 to 3.

[0007] However, the size of gel particles obtained by these devices is about several mm to several cm, and in the recent situation where further improvement of the water absorption speed is required, the gel pulverization is insufficient, and an additional gel pulverization device is required. Patent Document 4 proposes a method of wet pulverizing using a batch kneader or a continuous kneader to a size smaller than the gel particles that will become the product particle size of the water absorbent resin, but this is not practical because the size of the device becomes excessively large.

[0008] Furthermore, since the polymerization process involves crushing a highly adhesive hydrous gel undergoing a monomer polymerization reaction, the hydrous gel is prone to adhere to component parts inside the device. If the reaction continues in this adhered state, the hydrous gel will harden, which can damage the component parts and require a lot of time for cleaning during maintenance. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Publication No. 57-34101 [Patent Document 2] Japanese Patent Application Publication No. 60-55002 [Patent Document 3] International Publication No. 2001 / 038402 Brochure [Patent Document 4] Japanese Patent Application Publication No. 05-112654 Summary of the Invention

[0010] In recent years, in order to obtain a water-absorbing resin having an excellent water absorption rate, which is particularly required, it is necessary to crush a hydrogel to a particle size smaller than that of the conventional method in a gel crushing step. However, in the conventional so-called kneader polymerization in which a polymerization step and a gel crushing step are simultaneously performed using a kneader having multiple shafts, it has not been possible to obtain a hydrogel having a desired particle size.

[0011] Therefore, an object of the present invention is to provide a water-absorbent resin having an excellent water absorption rate.

[0012] First, the present inventors discovered that, whereas a particulate hydrogel-like crosslinked polymer (hereinafter also referred to as "particulate hydrogel") is conventionally obtained by using an extruder (meat chopper) equipped with a perforated plate, a particulate hydrogel can be continuously obtained by grinding the gel using a multi-screw kneader (particularly a twin-screw kneader). Furthermore, they discovered that a water-absorbent resin powder having an excellent water absorption rate can be obtained by continuously grinding the hydrogel-like crosslinked polymer at 50°C or higher in this grinding means, and thus completed the present invention.

[0013] That is, the present invention is a method for producing a water-absorbent resin powder, comprising: a polymerization step of polymerizing an aqueous monomer solution to obtain a hydrogel-like crosslinked polymer; a gel crushing step of crushing the hydrogel-like crosslinked polymer using a gel crushing device after the polymerization step to obtain a particulate hydrogel-like crosslinked polymer; and a drying step of drying the particulate hydrogel-like crosslinked polymer to obtain a dried product, the gel crushing device having an inlet, an outlet, and a main body incorporating a plurality of rotating shafts, each of which has a crushing means, the hydrogel-like crosslinked polymer being continuously introduced from the inlet in the gel crushing step, the hydrogel-like crosslinked polymer being continuously crushed by the crushing means at 50° C. or higher, and the particulate hydrogel-like crosslinked polymer being continuously taken out from the outlet, the polymerization rate of the hydrogel-like crosslinked polymer introduced into the inlet being 90% by mass or more, and the particulate hydrogel-like crosslinked polymer discharged from the outlet having a mass average particle diameter d1 calculated based on the solid content of 3 mm or less. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a partially cutaway side view showing an example of a gel crushing device used in the manufacturing method according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of the gel grinding device of FIG. 1 (a top view of the center of the main body). [Diagram 3] FIG. 1 is a flow diagram for explaining a typical manufacturing process of a water-absorbent resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below, but the scope of the present invention is not limited to these descriptions, and in addition to the following examples, the present invention can be implemented by making appropriate modifications within the scope of the invention. Furthermore, the present invention is not limited to the following embodiments, and various modifications are possible within the scope of the claims. Other embodiments obtained by appropriately combining the technical means disclosed in each of the embodiments are also included in the technical scope of the present invention.

[0016] [1] Definitions of terms [1-1] “Water-absorbing resin” The term "water-absorbent resin" in the present invention refers to a water-swellable, water-insoluble polymer gelling agent that satisfies the following physical properties: That is, the term refers to a polymer gelling agent that has a CRC (centrifuge retention capacity) of 5 g / g or more as defined in ERT441.2-02 as a water-swellable property, and an Ext (water-soluble content) of 50 mass% or less as a water-insoluble property as defined in ERT470.2-02.

[0017] The water absorbent resin can be designed according to its use and purpose, and is not particularly limited, but is preferably a hydrophilic crosslinked polymer obtained by crosslinking an unsaturated monomer having a carboxyl group. In addition, the water absorbent resin is not limited to a form in which the entire amount is a crosslinked polymer, and may be a composition containing additives, etc., as long as each of the physical properties (CRC, Ext) satisfies the above numerical range.

[0018] The "water absorbent resin" in the present invention may be surface cross-linked (also called post-cross-linked or secondary cross-linked), or may not be surface cross-linked. In this specification, the "water absorbent resin powder" refers to a powdered water absorbent resin, and is preferably a water absorbent resin adjusted to a predetermined solid content rate (moisture content) and particle size (particle diameter). In addition, the water absorbent resin powder in which a predetermined surface cross-linking treatment has been completed may be separately referred to as a surface cross-linked (post-cross-linked) water absorbent resin powder or water absorbing agent.

[0019] [1-2] "Poly(meth)acrylic acid (salt)" The term "poly(meth)acrylic acid (salt)" in the present invention refers to poly(meth)acrylic acid and / or a salt thereof, and means a crosslinked polymer containing (meth)acrylic acid and / or a salt thereof (hereinafter also referred to as "(meth)acrylic acid (salt)") as a main component as a repeating unit and containing a graft component as an optional component.

[0020] The above "main component" means that the amount (content) of (meth)acrylic acid (salt) used is preferably 50 mol% to 100 mol%, more preferably 70 mol% to 100 mol%, even more preferably 90 mol% to 100 mol%, and particularly preferably substantially 100 mol%, based on the total monomers used in the polymerization (all monomers excluding the crosslinking agent).

[0021] Here, "poly(methacrylic acid) (salt) " may be unneutralized, but is preferably a partially or completely neutralized poly(meth)acrylate salt, more preferably a monovalent salt, even more preferably an alkali metal salt or ammonium salt, even more preferably an alkali metal salt, and particularly preferably a sodium salt.

[0022] [1-3] Definition of evaluation method "EDANA" is an abbreviation for European Disposables and Nonwovens Associations. "ERT" is an abbreviation for EDANA Recommended Test Methods, which is a European standard that specifies the evaluation method of water-absorbent resins. In the present invention, unless otherwise specified, the measurement methods described in the original ERT (revised in 2002) are measured in accordance with the ERT. Evaluation methods not described in are measured by the methods and conditions described in the Examples.

[0023] [1-3-1] “CRC” (ERT441.2-02) "CRC" is an abbreviation of Centrifuge Retention Capacity, and means the water absorption capacity of a water-absorbent resin under no pressure (sometimes called "water absorption capacity"). Specifically, it means the water absorption capacity (unit: g / g) after 0.2 g of a water-absorbent resin is placed in a nonwoven bag, immersed in a large excess of 0.9% by mass sodium chloride aqueous solution for 30 minutes to allow free swelling, and then drained with a centrifuge (250G) for 3 minutes. For the hydrogel after polymerization and / or gel crushing, 0.4 g of hydrogel is used, the measurement time is changed to 24 hours, and the CRC is obtained by correcting for the solid content.

[0024] [1-3-2] “Moisture Content” (ERT430.2-02) "Moisture Content" means the moisture content defined by the loss on drying of the water-absorbent resin. Specifically, it means a value (unit: mass%) calculated from the loss on drying when 4.0 g of the water-absorbent resin is dried at 105°C for 3 hours. In the present invention, the moisture content is defined by the loss on drying of 1.0 g of the water-absorbent resin at 180°C for 3 hours for the water-absorbent resin after drying, and the moisture content is defined by the loss on drying of 2.0 g of the water-containing gel at 180°C for 24 hours for the water-containing gel before drying.

[0025] [1-3-3] "PSD" (ERT420.2-02) "PSD" is an abbreviation of Particle Size Distribution, and means the particle size distribution of the water-absorbent resin measured by sieve classification. The mass-average particle size (D50) and the logarithmic standard deviation (σζ) of the particle size distribution are measured by the same method as that described in U.S. Pat. No. 7,638,570. In the present invention, the particle size distribution (PSD) of the particulate hydrogel is determined by wet sieve classification using the method described below. Furthermore, the particle size (μm) of the particulate hydrogel in terms of solid content is determined by the particle size (μm) of the particulate hydrogel and its solid content (mass%) using the calculation method described below.

[0026] [1-3-4] “AAP” (ERT442.2-02) "AAP" is an abbreviation for Absorption Against Pressure, and means the water absorption capacity of a water-absorbent resin under pressure. Specifically, 0.9 g of a water-absorbent resin is subjected to a large excess of a 0.9% by mass aqueous sodium chloride solution at 2.06 kPa (21 g / cm) for 1 hour. 2 This refers to the water absorption capacity (unit: g / g) after swelling under a load of 4.83 kPa (approximately 49 g / cm 2 , equivalent to approximately 0.7 psi).

[0027] [1-3-5] "Vortex" In this specification, the term "vortex" is an index representing the water absorption speed of a water absorbent resin, and means the time (unit: seconds) required for 2 g of a water absorbent resin to absorb 50 ml of a 0.9 mass % aqueous sodium chloride solution to a predetermined state.

[0028] [1-4] "Gel crushing" In this specification, the term "gel crushing" refers to an operation of reducing the size and increasing the surface area of ​​a hydrogel-like crosslinked polymer (hereinafter also simply referred to as "hydrogel") obtained in a polymerization step (preferably aqueous solution polymerization, unstirred aqueous solution polymerization (static aqueous solution polymerization), particularly preferably belt polymerization) by applying shear and compression forces to the polymer to facilitate drying.

[0029] The shape of the hydrogel obtained may vary depending on the type of the polymerization machine. For example, the shape of the hydrogel obtained by static polymerization (particularly belt polymerization) is sheet-like or block-like. Here, the sheet-like refers to a polymer having a thickness in a plane, and the thickness is preferably 1 mm to 30 cm, particularly preferably 0.5 to 10 cm. The sheet-like hydrogel is typically obtained by belt polymerization, drum polymerization, and batch thin film polymerization. The length and width of the sheet-like hydrogel are appropriately determined depending on the size of the polymerization apparatus used. In the case of continuous polymerization (continuous belt polymerization or continuous drum polymerization), a sheet-like hydrogel having an endless length is obtained, and its width is the width of the belt or drum of the polymerization apparatus, preferably 0.1 to 10 m, more preferably 1 to 5 m. This endless sheet-like hydrogel may be appropriately cut in the length direction after polymerization and used. Furthermore, a block-like hydrogel is obtained by tank polymerization or the like. This block-like hydrogel may be appropriately crushed into several cm to several m squares after polymerization. In contrast, in the case of kneader polymerization, polymerization and gel crushing are performed continuously in the same apparatus in the polymerization step, so that a hydrogel that is finely granulated to some extent is obtained. However, the hydrogel particles obtained by kneader polymerization are not finely granulated to the particle size level obtained by the production method according to the present invention. In addition, in order to crush the hydrogel to the particle size level obtained by kneader polymerization in the present invention, an excessively large apparatus is required, which is not practical as an industrial production method. Therefore, gel crushing in such a polymerization step is not included in the concept of "gel crushing" in the present invention. In addition, in the present invention, the polymerization step is considered to be completed when the polymerization rate reaches the range described below. The operation of crushing the hydrogel that has been finely granulated to some extent by a method such as kneader polymerization to the particle size level required in the present invention is included in the concept of "gel crushing" in the present invention.

[0030] [1-5] Others In this specification, the range "X to Y" means "X or more and Y or less." In addition, unless otherwise noted, the unit of mass "t (ton)" means "metric ton," and "ppm" means "ppm by mass" or "ppm by weight." Furthermore, "mass" and "weight," "parts by mass" and "parts by weight," "% by mass" and "% by weight" are treated as synonyms. In addition, "acid (salt)" means "acid and / or its salt," and "(meth)acrylic" means "acrylic and / or methacrylic."

[0031] [2] Method for producing water-absorbent resin powder The method for producing a water absorbent resin powder according to the present invention includes a polymerization step, a gel crushing step and a drying step that are separate from the polymerization step. Preferably, the production method further includes a cooling step, a crushing step of the dried product, a classification step, a surface cross-linking step, and a sizing step after the surface cross-linking step (see FIG. 3). In addition, the method may include a step of adjusting an aqueous monomer solution, a step of adding various additives, a fine powder removal step, a fine powder recycling step (fine powder recovery step), and a filling step. Furthermore, various known steps may be included depending on the purpose.

[0032] According to the production method of the present invention, a hydrogel-like crosslinked polymer having a polymerization rate of 90% by mass or more is gel-pulverized using a multi-shaft kneader (particularly a twin-shaft kneader), and the particulate hydrogel having a mass average particle diameter d1 calculated as solid content of 3 mm or less is subjected to a drying step, thereby producing an absorbent resin with excellent water absorption rate.

[0033] Each step will now be described in detail.

[0034] [2-1] Preparation of monomer aqueous solution This step is an optional step of preparing an aqueous solution containing an acid group-containing unsaturated monomer as a main component (hereinafter referred to as "aqueous monomer solution"). Although a slurry liquid of the monomer can be used within a range in which the water absorption performance of the obtained water absorbent resin is not deteriorated, the aqueous monomer solution will be described in this section for convenience.

[0035] The above-mentioned "main component" means that the amount (content) of the acid group-containing unsaturated monomer used is usually 50 mol % or more, preferably 70 mol % or more, and more preferably 90 mol % or more (upper limit: 100 mol %) based on the total monomers (excluding the internal crosslinking agent) to be subjected to the polymerization reaction of the water absorbent resin.

[0036] (Acid group-containing unsaturated monomer) The acid group defined in the present invention is not particularly limited, but examples thereof include a carboxyl group, a sulfone group, and a phosphoric acid group. Examples of the acid group-containing unsaturated monomer include (meth)acrylic acid, (anhydrous) maleic acid, itaconic acid, cinnamic acid, vinyl sulfonic acid, allyl toluene sulfonic acid, vinyl toluene sulfonic acid, styrene sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, 2-(meth)acryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, and 2-hydroxyethyl (meth)acryloyl phosphate. From the viewpoint of water absorption performance, preferred are (meth)acrylic acid, (anhydrous) maleic acid, itaconic acid, and cinnamic acid, more preferred are (meth)acrylic acid, and particularly preferred is acrylic acid.

[0037] (Monomers other than acid group-containing unsaturated monomers) The monomer other than the acid group-containing unsaturated monomer may be any compound that can be polymerized to form a water-absorbing resin, such as (meth)acrylamide, N-ethyl(meth)acrylamide, and N,N-dimethyl(meth)acrylamide. , N,N-Dimethylaminopropyl(meth)acrylamide Amide group-containing unsaturated monomers such as N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, etc. To et al. mercapto group-containing unsaturated monomers; phenolic hydroxyl group-containing unsaturated monomers; and lactam group-containing unsaturated monomers such as N-vinylpyrrolidone.

[0038] (Neutralizing salt) In the present invention, a neutralized salt in which a part or all of the acid groups contained in the acid group-containing unsaturated monomer are neutralized can be used. In this case, the salt of the acid group-containing unsaturated monomer is preferably a salt with a monovalent cation, more preferably at least one selected from an alkali metal salt, an ammonium salt, and an amine salt, even more preferably an alkali metal salt, even more preferably at least one selected from a sodium salt, a lithium salt, and a potassium salt, and particularly preferably a sodium salt.

[0039] ( Neutralizer ) The neutralizing agent used to neutralize the acid group-containing unsaturated monomer is not particularly limited, but may be appropriately selected from inorganic salts such as sodium hydroxide, potassium hydroxide, sodium carbonate, and ammonium carbonate, and basic substances such as amine-based organic compounds having an amino group or an imino group. Inorganic salts and Basic substances Two or more types selected from In addition, the monomer in the present invention is a concept including a neutralized salt, unless otherwise specified.

[0040] (neutralization rate) From the viewpoint of water absorption performance, the number of moles of the neutralized salt relative to the total number of moles of the acid group-containing unsaturated monomer and its neutralized salt (hereinafter referred to as "neutralization rate") is preferably 40 mol% or more, more preferably 40 mol% to 80 mol%, even more preferably 45 mol% to 78 mol%, and particularly preferably 50 mol% to 75 mol%.

[0041] The method for adjusting the neutralization rate includes a method of mixing an acid group-containing unsaturated monomer with its neutralized salt, a method of adding a known neutralizing agent to an acid group-containing unsaturated monomer, a method of using a partially neutralized salt of an acid group-containing unsaturated monomer (i.e., a mixture of an acid group-containing unsaturated monomer and its neutralized salt) that has been adjusted to a predetermined neutralization rate in advance, etc. These methods may also be combined.

[0042] The neutralization rate may be adjusted before the start of the polymerization reaction of the acid group-containing unsaturated monomer, during the polymerization reaction of the acid group-containing unsaturated monomer, or on the hydrogel-like crosslinked polymer obtained after the completion of the polymerization reaction of the acid group-containing unsaturated monomer. The neutralization rate may be adjusted at one of the stages before the start of the polymerization reaction, during the polymerization reaction, or after the completion of the polymerization reaction, or at multiple stages. In applications where the polymer may come into direct contact with the human body, such as absorbent articles such as paper diapers, the neutralization rate may be adjusted preferably before the start of the polymerization reaction and / or during the polymerization reaction, more preferably before the start of the polymerization reaction.

[0043] (Internal crosslinking agent) In the method for producing a water-absorbent resin powder, an internal crosslinking agent is preferably used, which adjusts the water-absorbent performance and gel strength of the obtained water-absorbent resin when absorbing water.

[0044] The internal crosslinking agent may have a total of two or more unsaturated bonds or reactive functional groups in one molecule. For example, examples of internal crosslinking agents having a plurality of polymerizable unsaturated groups (copolymerizable with monomers) in the molecule include N,N-methylenebis(meth)acrylamide, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin (meth)acrylate, glycerin acrylate methacrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol hexa(meth)acrylate, triallyl cyanurate, triallyl isocyanurate, and triallyl phosphate. Examples of internal crosslinking agents having multiple reactive functional groups (which can react with the functional groups of the monomer (e.g., carboxyl groups)) in the molecule include triallylamine, polyallyloxyalkane, (poly)ethylene glycol diglycidyl ether, glycerol diglycidyl ether, ethylene glycol, polyethylene glycol, propylene glycol, glycerin, 1,4-butanediol, pentaerythritol, ethylenediamine, ethylene carbonate, propylene carbonate, and polyethyleneimine. do.Furthermore, examples of internal crosslinking agents having a polymerizable unsaturated group and a reactive functional group in the molecule include glycidyl (meth)acrylate, etc. Among these, two or more kinds may be used in combination.

[0045] Among these internal crosslinking agents, from the viewpoint of the effect of the present invention, a compound having a plurality of polymerizable unsaturated groups in the molecule is preferable, a compound having a (poly)alkylene structural unit in the molecule is more preferable, a compound having a polyethylene glycol structural unit is even more preferable, and an acrylate compound having a polyethylene glycol structural unit is particularly preferable. The hydrogel obtained by using these internal crosslinking agents has low adhesion. By drying this hydrogel having low adhesion, it is preferable because it can reduce fusion and aggregation during drying.

[0046] The amount of the internal crosslinking agent used is appropriately set depending on the type of monomer and the internal crosslinking agent. From the viewpoint of gel strength of the obtained water absorbent resin, the amount is preferably 0.001 mol% or more, more preferably 0.005 mol% or more, and even more preferably 0.01 mol% or more, based on the monomer. From the viewpoint of improving the water absorption performance of the water absorbent resin, the amount is preferably 5 mol% or less, more preferably 2 mol% or less. Note that, under polymerization conditions where the self-crosslinking reaction of the monomer is effective, the internal crosslinking agent may not be used.

[0047] (Polymerization inhibitor) The monomer used in the polymerization preferably contains a small amount of a polymerization inhibitor from the viewpoint of polymerization stability. A preferred polymerization inhibitor is p-methoxyphenol. The amount of the polymerization inhibitor contained in the monomer (particularly acrylic acid and its salts) is usually 1 ppm to 250 ppm, preferably 10 ppm to 160 ppm, and more preferably 20 ppm to 80 ppm.

[0048] (Other substances) In the production method according to the present invention, the following substances (hereinafter referred to as "other substances") may be added to the aqueous monomer solution within the scope of achieving the object of the present invention.

[0049] Specific examples of other substances include chain transfer agents such as thiols, thiolic acids, secondary alcohols, amines, and hypophosphites; foaming agents such as carbonates, bicarbonates, azo compounds, and bubbles; chelating agents such as ethylenediaminetetra(methylenephosphinic acid) and metal salts thereof, ethylenediaminetetraacetic acid and metal salts thereof, and diethylenetriaminepentaacetic acid and metal salts thereof; hydrophilic polymers such as polyacrylic acid (salts) and crosslinked products thereof (for example, recycled water-absorbent resin fine powder), starch, cellulose, starch-cellulose derivatives, and polyvinyl alcohol. The other substances may be used alone or in combination of two or more.

[0050] The amount of other substances used is not particularly limited, but in the case of recycled fine powder, it is 30% by mass or less relative to the monomer, and in the case of other than fine powder, the total concentration of other substances is preferably 10% by mass or less relative to the monomer, more preferably 0.001% by mass to 5% by mass, and particularly preferably 0.01% by mass to 1% by mass.

[0051] (Monomer aqueous solution (monomer concentration in In this process, the monomer aqueous solution The monomer concentration in the water absorbent resin (=total monomer amount / (total monomer amount+total polymerization solvent amount (usually water)) is preferably 10 mass % to 90 mass %, more preferably 20 mass % to 80 mass %, further preferably 30 mass % to 70 mass %, particularly preferably 40 mass % to 60 mass %, from the viewpoint of physical properties and productivity of the water absorbent resin. Hereinafter, the monomer concentration may be referred to as "monomer concentration".

[0052] (Polymerization initiator) The polymerization initiator used in the present invention is not particularly limited since it is appropriately selected depending on the polymerization form, etc., but examples thereof include a thermally decomposable polymerization initiator, a photodecomposable polymerization initiator, or a combination of these, or a redox-based polymerization initiator combined with a reducing agent that promotes the decomposition of the polymerization initiator. Specifically, one or more of the polymerization initiators disclosed in U.S. Pat. No. 7,265,190 are used. From the viewpoint of the handling of the polymerization initiator and the physical properties of the water-absorbing resin, preferably a peroxide or an azo compound, more preferably a peroxide, and even more preferably a persulfate is used.

[0053] The amount of the polymerization initiator used is preferably 0.001 mol % to 1 mol %, more preferably 0.001 mol % to 0.5 mol %, based on the monomer. When redox polymerization is performed as necessary, the amount of the reducing agent used in combination with the oxidizing agent is preferably 0.0001 mol % to 0.02 mol %, based on the monomer.

[0054] (dissolved oxygen) The dissolved oxygen in the aqueous monomer solution before polymerization may be reduced by raising the temperature or by replacing the solution with an inert gas. For example, the dissolved oxygen is preferably reduced to 5 ppm or less, more preferably 3 ppm or less, and particularly preferably 1 ppm or less.

[0055] It is also possible to disperse bubbles (particularly the above-mentioned inert gases) in the aqueous monomer solution, in which case the polymerization reaction will result in foaming polymerization.

[0056] [2-2] Polymerization process This step is a step of polymerizing the aqueous monomer solution to obtain a hydrogel-like crosslinked polymer, preferably a hydrogel that is a crosslinked body mainly composed of poly(meth)acrylic acid (salt).

[0057] In addition to the method of carrying out a polymerization reaction by adding the polymerization initiator, there is a method of irradiating with active energy rays such as radiation, electron beams, ultraviolet rays, etc. In addition, irradiation with active energy rays may be carried out in combination with the addition of a polymerization initiator.

[0058] (polymerization form) The polymerization form is a batch or continuous aqueous solution polymerization. It may also be belt polymerization or kneader polymerization. Furthermore, continuous aqueous solution polymerization is more preferable, and both continuous belt polymerization and continuous kneader polymerization are applicable. As specific polymerization forms, continuous belt polymerization is disclosed in U.S. Pat. Nos. 4,893,999, 6,241,928, and U.S. Patent Application Publication No. 2005 / 215734, and continuous kneader polymerization is disclosed in U.S. Pat. Nos. 6,987,151 and 6,710,141. By adopting these continuous aqueous solution polymerizations, the production efficiency of the water absorbent resin is improved.

[0059] In addition, examples of the preferred form of the continuous aqueous solution polymerization include "high-temperature initiated polymerization" and "high-concentration polymerization." "High-temperature initiated polymerization" refers to a form in which polymerization is initiated at a temperature of the aqueous monomer solution of preferably 30°C or higher, more preferably 35°C or higher, even more preferably 40°C or higher, and particularly preferably 50°C or higher (upper limit is the boiling point), and "high-concentration polymerization" refers to a form in which polymerization is performed at a monomer concentration of preferably 30% by mass or higher, more preferably 35% by mass or higher, even more preferably 40% by mass or higher, and particularly preferably 45% by mass or higher (upper limit is the saturated concentration). These polymerization forms can also be used in combination.

[0060] (Polymerization rate of hydrogel) The polymerization rate of the hydrogel crosslinked polymer obtained in the polymerization step is 90% by mass or more. It is preferably 95% by mass or more, more preferably 98% by mass or more, and particularly preferably 99% by mass or more. When gel pulverization is performed in a state where the polymerization rate is low (i.e., in a state where the polymerization rate is less than 90% by mass) (for example, when polymerization and gel pulverization are performed simultaneously as in kneader polymerization), a large amount of unreacted monomer contained in the pulverized gel particles is polymerized and adheres the pulverized gel particles to each other, so that gel particles with a large particle size are generated again. Therefore, when gel pulverization is performed during the polymerization step, it is necessary to pulverize the regenerated large particle size gel particles again, which increases the energy required for pulverization and causes the polymerization device to become excessively large. In addition, when a hydrogel with a low polymerization rate is pulverized after the polymerization step and a drying step is performed in a state containing a large amount of unreacted monomer, a polymerization reaction proceeds during drying, and large particle size hydrogel particles are regenerated from small particle size gel particles, which causes problems such as a decrease in the water absorption rate of the obtained water absorbent resin and an increase in the particle size of the dried product. The upper limit of the polymerization rate is not particularly limited, and 100% by mass is ideal, but a long polymerization time or strict polymerization conditions are required for a high polymerization rate, which may lead to a decrease in productivity and physical properties, so the upper limit is 99.95% by mass, further 99.9% by mass, and usually about 99.8% by mass. Typically, the polymerization rate of the hydrogel crosslinked polymer obtained in the polymerization step is 98 to 99.99% by mass.

[0061] [2-3] Shredding process The shredding step is an optional step of cutting or roughly crushing the hydrogel crosslinked polymer into a size that can be put into a gel crusher after the polymerization step and before the gel crushing step. In particular, when the polymerization step is belt polymerization and a sheet-like or block-like hydrogel is obtained, this shredding step is preferably carried out. Therefore, in one embodiment of the present invention, the hydrogel crosslinked polymer obtained after the polymerization step is in the form of a sheet, and a shredding step of shredding the sheet-like hydrogel crosslinked polymer before the gel crushing step is further included. The means for cutting or roughly crushing the hydrogel in the shredding step is not particularly limited, and a rotary cutter, a roller cutter, a guillotine cutter, or the like is used. The size of the shredded hydrogel is not particularly limited as long as it is within the range that can be put into a gel crusher described later, but the size of the shredded hydrogel is preferably 1 mm to 3 m, more preferably 5 mm to 2.5 m, and particularly preferably 1 cm to 2 m. If the object of the present invention is achieved, the shredding step may not be carried out.

[0062] [2-4] Gel crushing process This step is a step of obtaining a particulate hydrogel-like crosslinked polymer (hereinafter, "particulate hydrogel") by pulverizing the hydrogel-like crosslinked polymer obtained in the polymerization step after the above polymerization. The particle size of the particulate hydrogel is adjusted to a preferred range described later so that a (surface-crosslinked) water-absorbent resin powder having the desired shape and performance can be obtained in high yield. Note that this step may be carried out two or more times to obtain a particulate hydrogel having a predetermined particle size.

[0063] (Gel crusher) In the production method according to the present invention, as shown in Fig. 1 and Fig. 2, a gel crushing device having an inlet, a main body incorporating multiple rotating shafts, and an outlet is used in the gel crushing step after the polymerization step. Each rotating shaft has a crushing means. In this gel crushing device, the hydrogel crosslinked polymer continuously fed into the main body from the inlet is crushed at 50°C or higher by the crushing means of each rotating shaft, and is continuously taken out from the outlet as a particulate hydrogel crosslinked polymer. In the present invention, the main body means the body part (reference numeral 208 in Fig. 1) in which the multiple rotating shafts and crushing means are installed, and is also called a barrel, trough, casing, etc.

[0064] The gel grinding device used in the production method according to the present invention may be a vertical type (the hydrogel travels vertically) or a horizontal type (the hydrogel travels horizontally or horizontally) as long as it is a continuous type. In addition, the vertical and horizontal gel grinding devices may have an inclination of 0° to 90° with respect to the horizontal direction. For example, in the case of the horizontal continuous grinding device shown in FIG. 1, an appropriate inclination is provided as necessary, and the inclination may be downward or upward from the inlet to the outlet (i.e., with respect to the hydrogel travel direction). Usually, the inclination angle is 0° to 10°, preferably 0° to 1°, and particularly preferably 0°.

[0065] In the case of an extruder (meat chopper) used for gel crushing in a conventional manufacturing method, the hydrogel is substantially crushed near the die installed at the extrusion port, and gel crushing is hardly performed in the screw portion related to the transport of the hydrogel. In contrast, the gel crushing device (particularly, the kneader) used in the manufacturing method according to the present invention is characterized in that the hydrogel introduced is crushed to a particle size of 3 mm or less by the crushing means of the rotating shaft before it reaches the discharge port.

[0066] In detail, in this gel crushing device, the hydrogel fed from the feed port is crushed to the desired particle size before being discharged from the discharge port. Therefore, in this gel crushing device, unlike conventional extruders (meat choppers), it is not necessary to extrude from a die, and particulate hydrogel adjusted to the desired particle size is taken out from the discharge port. In the production method according to the present invention, by using this gel crushing device, a water-absorbent resin with an excellent water absorption rate can be obtained.

[0067] From the viewpoint of continuously crushing the gel at 50°C or higher, the gel crushing device preferably has a heating means and / or a heat-retaining means. The heating means and / or the heat-retaining means are not particularly limited, but from the viewpoint of preventing adhesion and aggregation of the hydrous gel and particulate hydrous gel, a heating means using direct heat transfer by convection and / or indirect heat transfer by heat conduction from the heating surface (contact surface with the hydrous gel, heat source part) of the gel crushing device heated by a heat medium is preferred. More preferred heating means are a ventilation heating type for direct heat transfer and an outer wall heating type for indirect heat transfer.

[0068] From the viewpoint of reducing damage to the hydrogel, preferably, the outer surface of the main body is provided with a heating means and / or a heat-retaining means, more preferably a heating means. As the heat-retaining means, for example, a method of covering a part or the whole surface of the outer surface of the main body (preferably 50% or more of the outer surface (area) of the main body, more preferably 80% or more, particularly preferably the whole surface) with a heat insulating material can be mentioned. In addition, as the heating means, an electric trace, a steam trace, a jacket heated by a heat medium, and the like, which are installed so as to cover a part or the whole surface of the outer surface of the main body (preferably 50% or more of the outer surface (area) of the main body, more preferably 80% or more, particularly preferably the whole surface), can be mentioned. The particle size of the particulate hydrogel required in the present invention is much smaller than that of the conventional one. Therefore, it was found that the variation in the adhesiveness and fluidity of the hydrogel particles due to the temperature change is larger than that expected in the range of the conventional technology. As a result, it was clarified by the study in the present invention that the energy required for crushing the hydrogel and the cohesiveness between the crushed gel particles vary greatly depending on the temperature. By providing the gel crushing device with the above heating means and / or heat-retaining means, the gel crushing process can be carried out in a more preferable temperature range. In addition, it is possible to prevent deterioration of the gel crushing quality due to the influence of temperature differences such as the seasons and day and night. Furthermore, it is possible to smoothly guide the gel crushing device to stable operation when starting up.

[0069] As long as the effects of the present invention can be obtained, the type of the pulverizing means of each rotating shaft is not particularly limited. For example, disks of various shapes can be mentioned as those having a shearing effect on the hydrous gel. The disks may be called chips, paddles, elements, kneading, rotors, etc. The shape of the disks is not particularly limited and is appropriately selected from disks, ellipses, approximately triangular shapes, etc. It is also possible to use a combination of disks of different shapes, and the arrangement is appropriately adjusted from the viewpoint of the particle diameter of the target particulate hydrous gel and the energy required for pulverization. In addition, arms, vanes, blades, cut disks (CD), etc. may be used in combination as the pulverizing means.

[0070] For example, when each rotating shaft has a circular or elliptical disk as a crushing means, the ratio of the effective length L (length) inside the main body to the maximum diameter D (diameter; when multiple disks with different diameters are used, the diameter of the largest disk) of the disk is defined as L / D. This L / D is preferably 5 to 40, more preferably 6 to 30, and even more preferably 6.5 to 20. The effective length L means the axial length (total length) of the main body (barrel) part including the inlet and outlet, as shown in FIG. 1.

[0071] In addition, the distance (clearance) between the disk and the main body (barrel) may vary depending on the location. When the minimum clearance C is the shortest distance between the outer periphery of the disk and the inner wall of the main body (barrel), the minimum clearance C is preferably 20% or less, more preferably 15% or less, even more preferably 10% or less, and particularly preferably 5% or less, of the maximum diameter D of the disk. If it is equal to or less than the upper limit, the shear force between the barrel and the disk during gel crushing becomes strong, and the gel crushing efficiency becomes good. In addition, the minimum clearance C is preferably 0.2% or more, more preferably 0.5% or more, and even more preferably 1% or more, of the maximum diameter D of the disk. If it is equal to or more than the lower limit, contact between the disk and the inner wall of the main body (barrel) is suppressed, and the intrusion of metal foreign matter due to wear is suppressed. In a preferred embodiment of the present invention, the minimum clearance C is 0.2 to 20% of the maximum diameter D of the disk.

[0072] As described later, in this gel crushing device, the hydrogel is crushed to a predetermined particle size by the rotation of multiple rotating shafts having crushing means. The rotation speed of the multiple rotating shafts may be uniform or non-uniform and is set appropriately depending on the device, but is preferably in the range of 1 rpm to 1000 rpm, more preferably 3 rpm to 500 rpm, and even more preferably 5 rpm to 300 rpm. In addition, when the rotation speeds of the rotating shafts are different, the ratio of the rotation speed of one rotating shaft to the rotation speed of the other rotating shafts is usually in the range of 1 to 10, and preferably in the range of 1 to 2.

[0073] In addition, when the multiple rotating shafts have disks as the crushing means, the peripheral speed (V) of the disks defined by the following (Equation 3) may be uniform or non-uniform and is appropriately set depending on the device, but is preferably 0.05 m / s to 5 m / s, more preferably 0.1 m / s to 5 m / s, even more preferably 0.15 m / s to 3 m / s, and particularly preferably 0.2 m / s to 2 m / s. If it exceeds the above range, the shear force of the hydrogel becomes excessive, which is not preferable because it causes deterioration of the physical properties of the hydrogel particles after crushing and excessive compaction. If it is below the above range, it is not preferable because the processing amount per unit time in the gel crushing process decreases. In addition, when the peripheral speeds of the disks of each rotating shaft are different, the ratio of the peripheral speed of one rotating shaft to the peripheral speed of the other rotating shaft is usually in the range of 1 to 10, and preferably in the range of 1 to 2.

[0074] Circumferential speed (V) (m / s)=πD×n / 60 (Formula 3) In equation (3), V is the peripheral speed of the disk (unit: m / s), D is the maximum diameter of the disk (unit: m), and n is the number of rotations of the disk per unit time (unit: rpm).

[0075] The rotation direction of the multiple rotating shafts may be a unidirectional type in which each rotating shaft rotates in the same direction, or a counter-directional type in which each rotating shaft rotates in the opposite direction. A unidirectional type device is expected to have self-cleaning properties, while a counter-directional type device is expected to have strong shearing forces. The rotation direction of each rotating shaft is appropriately selected in combination with the arrangement (disk pattern) of the grinding means described above.

[0076] This gel crushing device is preferably provided with a function of supplying water and / or water vapor into the main body. By performing gel crushing while supplying water and / or water vapor (preferably water and water vapor), a water-absorbent resin powder having a superior water absorption rate can be obtained. Therefore, according to one embodiment of the present invention, water and / or water vapor is supplied into the main body in the gel crushing step. In another preferred embodiment, water and water vapor are supplied into the main body in the gel crushing step. As a means for supplying water and / or water vapor, the gel crushing device may be provided with a plurality of inlets. The inlets for water and / or water vapor may be installed at any position, but are preferably installed on the side of the inlet for the hydrogel. Moreover, water and water vapor may be supplied from different inlets.

[0077] The method of adding water vapor is not particularly limited, but for example, a gas such as air, dry air, or nitrogen may be mixed with water vapor and added as a mixed gas. The pressure of the water vapor to be added is not particularly limited, but is preferably 0.2 to 0.8 MPa, more preferably 0.3 to 0.7 MPa. The temperature of the water and / or water vapor (including the mixed gas) is not particularly limited, but is preferably 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, and particularly preferably 80°C or higher. From the viewpoint of suppressing excessive temperature rise and drying of the hydrogel, it is preferably 200°C or lower, more preferably 170°C or lower, even more preferably 150°C or lower, even more preferably 120°C or lower, and particularly preferably 100°C or lower. In a preferred embodiment, the temperature of the water and / or water vapor supplied to the inside of the main body is 50 to 120°C. It is also possible to adjust the temperature of the hydrogel and particulate hydrogel in the gel crushing device by the temperature and the amount of water and / or water vapor (including the mixed gas) used. In this case, the water vapor and / or the mixed gas acts as a heat medium for direct heat transfer, and the water-containing gel and the particulate water-containing gel inside the main body are heated or kept at a predetermined temperature. The water and / or water vapor (including the mixed gas) to be added may contain additives such as a gel fluidizing agent, a crosslinking agent, an oxidizing agent, a reducing agent, and a polymerization initiator, which will be described later.

[0078] The amount of water and / or water vapor supplied is preferably 0.1% by mass to 50% by mass, more preferably 0.5% by mass to 40% by mass, and further preferably 1% by mass to 30% by mass, based on the mass of the hydrogel calculated as solid content.

[0079] The gel grinding device used in the manufacturing method according to the present invention is preferably equipped with a heating means and / or a heat-retaining means on the outer surface of the main body, and a liquid heat medium such as hot water or oil may be introduced into a jacket or the like installed on the outer surface of the main body, or a heated gas (hot air) may be introduced as a heat medium. These heat mediums act as heat mediums for indirect heat transfer. From the viewpoint of the heating efficiency and / or heat-retaining efficiency of indirect heat transfer, the temperature of the heat medium is preferably 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, and particularly preferably 80°C or higher. On the other hand, from the viewpoint of suppressing excessive temperature rise and drying of the hydrogel, the temperature of the heat medium is preferably 200°C or lower, more preferably 170°C or lower, even more preferably 150°C or lower, even more preferably 130°C or lower, and particularly preferably 110°C or lower. A particularly preferred heat medium is hot water or steam. The temperature of the heat medium may be a constant temperature, or may be appropriately changed during gel grinding.

[0080] More preferably, before the hydrous gel is introduced into the gel crusher, the temperature inside (inner surface) of the main body is preferably heated to 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, and even more preferably 80°C or higher. This reduces adhesion of the hydrous gel to the inner surface of the main body. This also further improves the water absorption rate of the obtained water-absorbent resin powder. That is, in the production method according to the present invention, it is preferable that the inner surface of the main body is heated to the above-mentioned temperature or higher before the hydrous gel is introduced and at the start of gel crushing. More preferably, it is preferable that the inner surface of the main body and the outer surfaces of the multiple rotating shafts and the crushing means of each rotating shaft are heated to the above-mentioned temperature or higher. On the other hand, from the viewpoint of suppressing excessive heating and drying of the hydrous gel, the heating temperature inside (inner surface) of the main body is preferably 200°C or lower, more preferably 170°C or lower, even more preferably 150°C or lower, even more preferably 130°C or lower, and particularly preferably 110°C or lower before the hydrous gel is introduced into the gel crusher. For example, the temperature inside the main body (inner surface) can be adjusted to a desired range by circulating a heat medium inside the jacket provided on the main body. From the viewpoint of maintaining the temperature in the gel crushing step at 50°C or higher, it is preferable that the temperature inside the main body (inner surface) is maintained within the above range in the gel crushing step.

[0081] Here, "continuously crushing the hydrogel-like crosslinked polymer at 50°C or higher" means continuously crushing the hydrogel-like crosslinked polymer while maintaining the temperature of the hydrogel-like crosslinked polymer at 50°C or higher in the section shown in (A) of FIG. 1, that is, in the section from the inlet to the outlet. In other words, "continuously crushing the hydrogel-like crosslinked polymer by a crushing means at 50°C or higher" means "continuously crushing the hydrogel-like crosslinked polymer by a crushing means while maintaining the hydrogel-like crosslinked polymer at 50°C or higher." For example, if the temperature T1 of the hydrogel-like crosslinked polymer fed into the inlet of the gel crushing device is set to 50°C or higher and the heat medium temperature of the jacket installed on the outside of the device body is set to 50°C or higher, the temperature of the hydrogel-like crosslinked polymer can be maintained at 50°C or higher in the section shown in (A) of FIG. 1, and the hydrogel-like crosslinked polymer can be continuously crushed at 50°C or higher. Also included is a case where, even if the temperature T1 of the hydrogel-like crosslinked polymer fed into the inlet of the gel grinding device is 50°C or lower, the temperature of the hydrogel-like crosslinked polymer is rapidly raised by supplying high-temperature water and / or steam to the inlet portion or setting the jacket heat medium temperature of the device body to a high temperature, thereby raising the temperature to 50°C or higher in part (A) and continuously grinding the polymer.

[0082] The temperature at which the hydrogel crosslinked polymer is continuously pulverized is 50° C. or higher, preferably 60° C. or higher, more preferably 70° C. or higher, and further preferably 80° C. or higher.

[0083] The upper limit of the temperature for continuously grinding the hydrogel crosslinked polymer is not particularly limited, but from the viewpoint of suppressing excessive heating and drying of the hydrogel, it is preferably 200°C or less, more preferably 170°C or less, even more preferably 150°C or less, even more preferably 130°C or less, and particularly preferably 110°C or less.

[0084] Furthermore, in the case of a large-sized gel grinding device, it is preferable to circulate a heat medium inside the multiple rotating shafts as a heating means and / or a heat retention means. This can shorten the time it takes to heat up the inside of the main body when starting up the gel grinding device.

[0085] As long as the hydrogel is adjusted to a desired particle size, the average residence time of the hydrogel in the gel crusher is not particularly limited, but from the viewpoint of reducing mechanical damage to the hydrogel, it is preferably 30 seconds to 30 minutes. In the gel crusher, the average residence time of the hydrogel is adjusted by the rotation speed of the rotating shaft and the input speed of the hydrogel.

[0086] In the gel crushing device used in the manufacturing method according to the present invention, it is most preferable not to use a die (die plate), but as long as the effect of the present invention can be obtained, a die may be installed at the outlet. When a die is used, the opening rate of the die is preferably 25% or more, more preferably 50% or more, even more preferably 60% or more, even more preferably 70% or more, and particularly preferably 80% or more. There is no particular upper limit to the opening rate. An opening rate of 100% is synonymous with the case where a die is not used. The die (die plate) is a plate having (multiple) through holes for discharging the material inside the main body, and is installed near the outlet of the crushing device. The opening rate refers to the ratio of the total planar area of ​​all the through holes to the planar area of ​​the die. The larger the opening rate, the less likely the material inside the main body is to be blocked and the easier it is to be discharged, so that the effect of the present invention becomes more pronounced.

[0087] Figures 1 and 2 show an example of a gel crusher 200 used in the production method according to the present invention. Figure 1 is a partially cutaway side view of the gel crusher 200, and Figure 2 is an enlarged view of the gel crusher 200 (a top view of the center of the main body). The basic configuration and method of use of the gel crusher 200 will be described below with reference to Figures 1 and 2.

[0088] As shown in the figure, the gel crusher 200 includes an inlet 204, a main body 208, two rotating shafts 206, an outlet 210, a driving device 214, and a gas inlet 216. The main body 208 is also called a barrel. In FIG. 1, two rotating shafts 206 are provided along a direction perpendicular to the paper surface. The rotating shafts 206 extend in the length direction of the main body 208. One end of the rotating shaft 206 penetrates the main body 208 and is connected to the driving device 214. Although not shown in the figure, in the gel crusher 200, the other end of the rotating shaft 206 is ,shaft Support bearing At the rear of the main body 208 The rotating shaft 206 is supported so as to be freely rotatable. That is, the rotating shaft 206 is held at both ends. However, the gel grinding device in the manufacturing method according to the present invention is not limited to such a double-shaft supported form, and may have a so-called single-shaft supported structure without a bearing behind the outlet 210 as long as the object of the present invention is achieved. The inlet 204, the gas inlet 216, and the outlet 210 are each fixed to the main body 208 and communicate with the inside of the main body 208. The left-right direction in FIG. 1 is the length direction of the main body 208 and the axial direction of the rotating shaft 206. Although not shown, the main body 208 has a jacket structure.

[0089] FIG. 2 shows a part of the main body 208 of the gel crusher 200. FIG. 2 is an enlarged view of the gel crusher of FIG. 1 (a view of the center of the main body from above). As shown in the figure, in this gel crusher 200, two rotating shafts 206 are built into the main body 208. A crushing means 212 is provided on the outer periphery of each of the two rotating shafts 206. That is, the crushing means 212 and the rotating shaft 206 are configured as separate bodies. In this embodiment, the rotating shaft 206 has a plurality of disks as the crushing means 212. The up-down direction in FIG. 2 is the width direction of the main body 208. The left-right direction in FIG. 2 is the length direction of the main body 208 and the axial direction of the rotating shaft 206.

[0090] In a preferred embodiment of the gel crushing process using this gel crushing device 200, a heat medium is first circulated through a jacket (not shown) to heat the main body 208. Then, each of the rotating shafts 206 is rotated by a driving device 214 (e.g., a motor). With the rotation of the rotating shafts 206, the rotating shafts 206 and the multiple disks that are the crushing means 212 rotate.

[0091] Next, the hydrous gel is continuously fed into the feed port 204. At this time, water and / or water vapor may be fed into the feed port 204 at the same time. Also, water vapor and / or water may be fed into the gas feed port 216. The hydrous gel and the main body 208 are heated by the water and / or water vapor and kept at a predetermined temperature.

[0092] The hydrogel introduced into the main body 208 moves toward the outlet 210 .

[0093] The hydrous gel comes into contact with the crushing means 212 (i.e., a plurality of disks) in the main body 208. The hydrous gel is broken down into fine particles by the shearing action of the rotating disks. The hydrous gel moves toward the discharge port 210 while being crushed by the shearing action of the crushing means 212. At the discharge port 210, particulate hydrous gel adjusted to a predetermined particle size is taken out.

[0094] The rotating shaft of the gel crushing device has multiple disks. The shapes of the multiple disks may be the same or different, but are preferably different. The combination of disks is appropriately changed depending on the physical properties of the hydrogel, the size of the crushed gel to be obtained, etc., with reference to, for example, patent documents (JP Patent Publication No. 2005-35212).

[0095] An example of a gel grinding device having such a basic configuration is a multi-shaft kneader having two or more shafts. Specifically, a two-shaft, three-shaft, four-shaft or eight-shaft kneader can be mentioned. From the viewpoint of production efficiency, a continuous type is preferably used for this gel grinding device. Specifically, examples of the gel grinding device include a CKH type continuous kneader (Honda Iron Works Co., Ltd.), a twin-screw extruder TEX (The Japan Steel Works, Ltd.), a twin-screw extruder TEXαIII (The Japan Steel Works, Ltd.), a continuous kneader (CONTINUOUS KNEADER, Dalton Co., Ltd.), a KRC hybrid reactor (KRC HYBRID REACTER, Kurimoto Iron Works Co., Ltd.), a KRC kneader (KURIMOTO-READCO CONTINUOUS KNEADER, Kurimoto Iron Works Co., Ltd.), a KEX extruder (KEX EXTRUDER, Kurimoto Iron Works Co., Ltd.), a KEXD extruder (KEXD Examples include the twin-screw extruder TEX-SSG (Toshiba Machine Co., Ltd.), twin-screw extruder TEX-CS (Toshiba Machine Co., Ltd.), twin-screw extruder TEX-SX (Toshiba Machine Co., Ltd.), twin-screw extruder TEX-DS (Toshiba Machine Co., Ltd.), twin-screw extruder TEX-A (Toshiba Machine Co., Ltd.), twin-screw extruder TEX-B (Toshiba Machine Co., Ltd.), twin-screw extruder TEX-BS (Toshiba Machine Co., Ltd.), 4-screw, 8-screw extruder WDR series (Technovel Co., Ltd.), etc. Therefore, in a preferred embodiment of the present invention, the gel crushing device is a continuous double-screw kneader.

[0096] (Gel crushing energy) Gel grinding energy (GGE) is described in International Publication No. 2011 / 126079 (corresponding to U.S. Patent Application Publication No. 2013 / 026412 and U.S. Patent Application Publication No. 2016 / 332141), and means the mechanical energy per unit mass (unit mass of hydrous gel) required by a gel grinding device when grinding a hydrous gel, and is calculated by the following formula (5) when the gel grinding device is driven by three-phase AC power.

[0097] Gel crushing energy [J / g] = {3 1 / 2 × voltage × current × power factor × motor efficiency} / {mass of hydrous gel fed into the gel grinder per second} (Equation 5) Here, the power factor and motor efficiency are values ​​specific to the device that change depending on the operating conditions of the gel grinding device, and take values ​​from 0 to 1. When the gel grinding device is driven by single-phase AC power, the power factor and motor efficiency in the above formula are 1 / 2 is calculated by changing to 1. In the above (Equation 5), the unit of voltage is [V], the unit of current is [A], and the unit of mass of the hydrogel is [g]. The gel grinding energy (GGE) applied in the present invention is preferably 15 J / g or more, more preferably 25 J / g or more, more preferably 40 J / g or more, even more preferably 50 J / g or more, even more preferably 100 J / g or more, and most preferably 120 J / g or more. The upper limit is 200 J / g or less.

[0098] (gel temperature) From the viewpoint of continuously pulverizing the hydrogel crosslinked polymer at 50° C. or more, the temperature T1 of the hydrogel crosslinked polymer fed into the inlet of the gel crushing device in the gel crushing step (hereinafter also referred to as the "gel temperature T1 at the inlet" or simply the "gel temperature T1") is preferably 50° C. or more. This gel temperature T1 is preferably measured by a thermometer installed at the inlet. From the viewpoint of preventing adhesion between the gel-pulverized hydrogels, this gel temperature T1 is preferably 60° C. or more, and from the viewpoint of further improving the water absorption rate of the water-absorbent resin powder, it is more preferably 70° C. or more, and even more preferably 80° C. or more. From the viewpoint of suppressing excessive drying, the gel temperature T1 is preferably 130° C. or less, more preferably 110° C. or less, even more preferably 100° C. or less, and particularly preferably 90° C. or less. For the same reason, the gel temperature during crushing is preferably 130° C. or less. The gel temperature T1 can be adjusted within a desired range by keeping the hydrogel-like crosslinked polymer warm after the temperature of the hydrogel-like crosslinked polymer has increased due to the heat of polymerization before being fed into the gel crusher, or by heating the obtained hydrogel-like crosslinked polymer.

[0099] From the viewpoint of suppressing aggregation of the gel-pulverized hydrogels, the temperature T2 of the particulate hydrogel crosslinked polymer discharged from the gel crusher (hereinafter also referred to as "gel temperature T2 at the outlet" or simply "gel temperature T2") is preferably 60°C to 140°C, more preferably 70°C to 130°C, even more preferably 80°C to 125°C, even more preferably 85°C to 120°C, particularly preferably 90°C to 115°C, and most preferably 100°C to 115°C. Preferably, the temperature T2 is set in the relevant temperature range, and the temperature T1 is set in the above-mentioned temperature range. This gel temperature T2 is preferably measured by a thermometer installed at the outlet. The gel temperature T2 can be adjusted within a desired range by appropriately adjusting the set temperature of the heating means and / or the warming means of the gel crusher, and further the residence time of the hydrogel crosslinked polymer inside the gel crusher.

[0100] From the viewpoint of further improving the water absorption rate of the water absorbent resin powder, the gel temperature T2 at the discharge port is preferably higher than the gel temperature T1 at the input port. The difference ΔT=(T2-T1) is preferably 5°C or more, more preferably 8°C or more, and even more preferably 10°C or more. The difference ΔT=(T2-T1) is preferably 60°C or less, more preferably 50°C or less, even more preferably 40°C or less, and particularly preferably 35°C or less. It is preferable that the difference ΔT=(T2-T1) is within the relevant temperature range, and the temperature T1 and the temperature T2 are set to be within the above-mentioned temperature range. Incidentally, ΔT can be adjusted within a desired range by adjusting T1 and T2, respectively, as described above.

[0101] (gel solid content) In the gel crushing step, the solid content of the hydrogel fed into the inlet of the gel crusher (hereinafter referred to as gel solid content) is determined by the measurement method described in the Examples below. From the viewpoints of the degree of aggregation between the gel-crushed hydrogels, the energy required for crushing, the drying efficiency, and the absorption performance, the gel solid content is preferably 25% by mass to 75% by mass, more preferably 30% by mass to 70% by mass, further preferably 35% by mass to 65% by mass, and particularly preferably 40% by mass to 60% by mass.

[0102] (Gel fluidizer) In the production method according to the present invention, the gel fluidizer is preferably added before and / or during the gel crushing step. As a result, the particulate hydrogel containing the gel fluidizer is taken out from the outlet. The addition of the gel fluidizer suppresses strong adhesion or adhesion between finely crushed gel particles, and has the effect of improving the water absorption rate of the obtained water absorbent resin. In addition, the load in the crushing step after the drying step and the crushing step in the sizing step described below is reduced, and the amount of fine powder generated is reduced. From the viewpoint that each particle of the obtained particulate hydrogel contains the gel fluidizer uniformly, addition during the gel crushing step is more preferable, and addition simultaneously with the introduction of the hydrogel is even more preferable.

[0103] The amount of the gel fluidizer to be added is appropriately set depending on the solid content of the hydrogel or particulate hydrogel and the type of the gel fluidizer. The amount of the gel fluidizer to be added is preferably 0.001% by mass to 5% by mass, more preferably 0.01% by mass to 3% by mass, still more preferably 0.02% by mass to 2% by mass, and particularly preferably 0.03% by mass to 1% by mass, based on the solid content of the hydrogel.

[0104] Examples of the gel fluidizing agent include anionic, cationic, nonionic and amphoteric surfactants, as well as low molecular weight or high molecular weight surfactants thereof, polymer lubricants, etc. Among these, surfactants are preferred.

[0105] (Surfactant) Specifically, surfactants used in gel fluidizing agents include: (1) sucrose fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene glycerin fatty acid esters, sorbitol fatty acid esters, polyoxyethylene sorbitol fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, alkylaryl formaldehyde condensed polyoxyethylene ethers, polyoxyethylene polyoxypropylene block copolymers, polyoxyethylene polyoxypropyl alkyl ethers, polyethylene glycol fatty acid esters, alkyl glucosides, N-alkyl gluconamides, polyoxyethylene fatty acid amides, polyoxyethylene alkylamines, phosphate esters of polyoxyethylene alkyl ethers, and phosphate esters of polyoxyethylene alkyl allyl ethers. Nonionic surfactants such as esters, (2) alkyl dimethyl amino acetic acid betaines such as capryl dimethyl amino acetic acid betaine, lauryl dimethyl amino acetic acid betaine, myristyl dimethyl amino acetic acid betaine, and stearyl dimethyl amino acetic acid betaine, alkyl amidopropyl betaines such as lauric acid amidopropyl betaine, coconut oil fatty acid amidopropyl betaine, and palm kernel oil fatty acid amidopropyl betaine, alkyl hydroxysulfobetaines such as lauryl hydroxysulfobetaine, and alkyl carboxymethyl hydroxyethyl imidazolinium betaine such as 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, (3) anionic surfactants such as alkyl amino diacetate monoalkali metals such as lauryl amino diacetate monosodium, lauryl amino diacetate potassium, and myristyl amino diacetate sodium, and (4) cationic surfactants such as long-chain alkyl dimethyl amino ethyl quaternary salts. Two or more of these may be used in combination. Among these, from the viewpoint of further improving the water absorption rate of the water absorbent resin powder, amphoteric surfactants are preferred, and alkyldimethylaminoacetate betaine is more preferred.

[0106] (polymer lubricant) In the production method according to the present invention, the polymer lubricants exemplified below can be added to the aqueous monomer solution or hydrous gel as long as the object of the present invention is achieved.

[0107] Specific examples of the polymer lubricant include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-modified ethylene-propylene-diene terpolymer (EPDM), maleic anhydride-modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, polyalkylene oxide such as ethyl cellulose, ethylhydroxyethyl cellulose, polyethylene glycol, and polysiloxane modified with side chain and / or terminal polyether. The molecular weight (weight average molecular weight) of these is preferably selected appropriately within the range of 2 to 2,000,000, more preferably 4 to 1,000,000. Two or more of these may be used in combination.

[0108] In addition, the above-mentioned polymer lubricant may be used in combination with the above-mentioned surfactant as a gel fluidizing agent. When the surfactant and the polymer lubricant are used in combination, the total amount added is appropriately set according to the polymerization form, the composition of the monomer aqueous solution, and the water content of the hydrogel. When added to the monomer aqueous solution, it is set as a concentration relative to the monomer component, when added to the hydrogel, it is set relative to the solid content, and when added to both, it is set as the sum of the above.

[0109] The total amount of the surfactant and polymer lubricant added is preferably 5% by mass or less, more preferably 3% by mass or less, and is preferably 0.001% by mass or more, particularly preferably 0.01% by mass or more, based on the solid content of the hydrogel.

[0110] (surface tension) The type and amount of the gel fluidizer are appropriately adjusted in consideration of the suppression of aggregation of the particulate hydrogel in the gel crushing step and the drying step. From the amount of return in the actual use of the obtained water-absorbent resin powder in an absorbent article (diaper), the type and amount of the gel fluidizer that does not excessively reduce the surface tension of the water-absorbent resin of the final product are preferred. For example, the type and amount of the gel fluidizer are selected so that the surface tension of the water-absorbent resin (surface tension of the dispersion of the water-absorbent resin in physiological saline) is preferably 55 mN / m or more, more preferably 60 mN / m or more, and even more preferably 65 mN / m or more. This surface tension is measured by the method described in WO2015 / 129917. An example of a gel fluidizer that can keep the surface tension within this range is an amphoteric surfactant.

[0111] (Other additives) During the gel crushing step, or during the transition from the gel crushing step to the subsequent drying step, a surface crosslinking agent as described in [2-7-1] or other additives as described in [2-10] may be added.

[0112] (Particle size of particulate hydrogel) In the manufacturing method according to the present invention, from the viewpoint of the absorption speed of the manufactured water absorbent resin powder, the particulate hydrogel crosslinked polymer discharged from the outlet of the gel crusher has a mass average particle diameter d1 calculated as a solid content of 3 mm or less. When d1 exceeds 3 mm, the polymer cannot be subjected to a post-process, and therefore a water absorbent resin powder cannot be obtained (Experimental Example 5 described later). d1 is preferably 1 μm to 3 mm, more preferably 10 μm to 3 mm, even more preferably 30 μm to 2 mm, even more preferably 50 μm to 1 mm, and particularly preferably 100 μm to 200 μm. The mass average particle diameter d1 of the particulate hydrogel crosslinked polymer discharged from the outlet of the gel grinder in terms of solid content can be controlled, for example, by the temperature of the hydrogel crosslinked polymer during grinding (for example, controlled by the temperature inside the grinder body or the temperature of water and / or steam supplied inside the body), the minimum clearance relative to the maximum disk diameter of the gel grinder, the feeding speed of the hydrogel, the rotation speed of the rotating shaft of the gel grinder, the gel crushing energy (GGE), etc. The mass average particle diameter d1 of the particulate hydrogel in terms of solid content is specified by the physical property measurement methods (g) and (h) described later.

[0113] The particle size distribution of the particulate hydrogel is preferably 10% by mass or more, more preferably 25% by mass or more, and even more preferably 40% by mass or more, of the particles in the range of less than 150 μm, calculated as solid content. The particle size distribution of the particulate hydrogel is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, of the particles in the range of less than 850 μm, calculated as solid content, with the upper limit being 100% by mass. The logarithmic standard deviation (σζ) of the particle size distribution is 0.2 to 1.0, more preferably 0.2 to 0.8, and even more preferably 0.2 to 0.7.

[0114] (Solid content of particulate hydrogel) The solid content of the particulate hydrogel discharged from the outlet of the gel grinding device is preferably 25% by mass to 75% by mass, more preferably 30% by mass to 70% by mass, further preferably 35% by mass to 65% by mass, and particularly preferably 40% by mass to 60% by mass. By subjecting the particulate hydrogel having a solid content in the above range to the drying step, a particulate dried product having a high CRC and little damage due to drying (such as an increase in water-soluble content) can be obtained.

[0115] (Polymerization rate of particulate hydrogel) The polymerization rate of the particulate hydrogel discharged from the gel crusher is within the range of the polymerization rate before being introduced into the gel crusher, and the polymerization may be further advanced in the gel crushing step. The degree of progress of the polymerization is appropriately adjusted by the heating and residence time in the gel crusher, the remaining amount of the polymerization initiator in the hydrogel after polymerization, the amount of any polymerization initiator added later, and the like. The polymerization rate after the gel crushing step is specified by the physical property measurement method described later, similar to the polymerization rate before gel crushing. The polymerization rate of the particulate hydrogel after gel crushing is 90% by mass or more, preferably 95% by mass or more, more preferably 98 to 99.99% by mass, and ideally 100%. In the particulate hydrogel having a polymerization rate within the above range, aggregation and adhesion during drying are avoided.

[0116] [2-5] Drying process This step is a step of drying a particulate hydrogel crosslinked polymer, preferably a particulate hydrogel crosslinked polymer containing a gel fluidizer, to a desired solid content to obtain a dried product. The "solid content" refers to a value calculated from the loss on drying (the mass change when 1.0 g of a sample is dried at 180°C for 3 hours).

[0117] The solid content of the dried product after the drying step is preferably 80% by mass or more, more preferably 85% by mass to 99.8% by mass, even more preferably 90% by mass to 99.7% by mass, even more preferably 92% by mass to 99.5% by mass, particularly preferably 96% by mass to 99.5% by mass, and extremely preferably 98% by mass to 99.5% by mass. If the solid content after drying is excessively high, not only will long-term drying be required, but there is also a risk of deterioration of physical properties and coloring after drying. In addition, if the solid content after drying is low, there may be cases where the productivity in the sizing step described below decreases and the water absorption capacity (CRC) decreases. When the surface crosslinking step described below is performed after the drying step, it is preferable to dry to the above solid content, since the physical properties are further improved. The moisture content (=100-solid content) of the dried product is calculated from the above solid content.

[0118] The drying method in the drying step of the present invention is not particularly limited, and may be appropriately selected from stationary drying, stirring drying, fluidized bed drying, etc. In addition, various drying methods may be used, such as heat drying, hot air drying, reduced pressure drying, infrared drying, microwave drying, drum dryer drying, azeotropic dehydration drying with a hydrophobic organic solvent, and high humidity drying using high-temperature water vapor.

[0119] (drying equipment) The drying device used in the drying step is not particularly limited, and one or more of a heat transfer conduction type dryer, a radiation heat transfer type dryer, a hot air heat transfer type dryer, a dielectric heating type dryer, etc. may be appropriately selected. It may be a batch type or a continuous type. It may also be a direct heating type or an indirect heating type. For example, heat transfer type dryers such as a ventilation band type, a ventilation circuit type, a ventilation vertical type, a parallel flow band type, a ventilation tunnel type, a ventilation stirring type, a ventilation rotation type, a fluidized bed type, and an air flow type may be mentioned.

[0120] The heating means is not particularly limited, but from the viewpoint of drying efficiency and reducing thermal damage to the water-absorbent resin, the heating means for the particulate hydrogel is preferably a heating means for direct heat transfer by convection and / or indirect heat transfer by heat conduction from the heating surface (contact surface with the particulate hydrogel, heat source part) of the dryer heated by a heat medium. More preferred heating means are a ventilation heating type for direct heat transfer, and an outer wall heating type or a tubular heating type for indirect heat transfer.

[0121] In the drying step, a gas may be introduced into the dryer. The gas is not particularly limited, but examples thereof include air, dry air, nitrogen, water vapor, and a mixture thereof. The gas acts as a carrier gas and promotes drying by discharging water vapor generated during drying to the outside of the dryer. Furthermore, when a heated gas is used, the gas also acts as a heat medium, which further promotes drying. Preferably, nitrogen, water vapor, and a mixture of these with air are used. When a mixed gas containing water vapor (hereinafter also referred to as a high-humidity mixed gas) is used, the inside of the dryer becomes a low-oxygen state, and oxidation and deterioration during drying are suppressed. As a result, the performance of the water-absorbent resin can be improved and low coloring can be achieved. In addition, the moving direction of this gas may be parallel or countercurrent to the moving direction of the particulate hydrous gel to be dried, or a mixture of these may be used.

[0122] The drying conditions are appropriately selected depending on the type of drying device and the solid content of the particulate hydrogel, and the drying temperature is preferably 100°C to 300°C, more preferably 150°C to 250°C, even more preferably 160°C to 220°C, and particularly preferably 170°C to 200°C. If the drying temperature is below the above range, the drying time becomes excessively long, which is uneconomical. If the drying temperature is above the above range, the physical properties of the water-absorbent resin deteriorate and significant coloring occurs, which is undesirable. In addition, the drying time is preferably 1 minute to 10 hours, more preferably 5 minutes to 2 hours, even more preferably 10 minutes to 120 minutes, and particularly preferably 20 minutes to 60 minutes. If the drying temperature is below the above range, the drying temperature needs to be excessively high, which is undesirable because the physical properties of the water-absorbent resin deteriorate and significant coloring occurs. If the drying temperature is above the above range, the dryer becomes large and the processing capacity decreases, which is uneconomical.

[0123] [2-6] Crushing and classification process This step is a step of crushing and / or classifying the dried product obtained in the drying step to obtain a water absorbent resin powder having a specific particle size. Note that this step differs from the above (2-4) gel crushing step in that the material to be crushed is subjected to a drying step.

[0124] This step is carried out before and / or after the surface cross-linking step [2-7], preferably before the surface cross-linking step [2-7], and may be carried out at least twice before and after the surface cross-linking step [2-7].

[0125] Examples of the equipment (crusher) used in the crushing step of the present invention include high-speed rotary crushers such as roll mills, hammer mills, screw mills and pin mills, vibration mills, knuckle-type crushers and cylindrical mixers, which may be used in combination as necessary.

[0126] (particle size) The weight average particle diameter (D50) of the water absorbent resin powder before surface crosslinking is preferably 200 μm or more, more preferably 200 μm to 600 μm, further preferably 250 μm to 550 μm, and particularly preferably 300 μm to 500 μm, from the viewpoints of water absorption speed, water absorption capacity under pressure, and the like.

[0127] Further, the content of fine particles having a particle diameter of less than 150 μm as defined by standard sieve classification is preferably as small as possible, and is preferably 0 to 5 wt %, more preferably 0 to 3 wt %, and further preferably 0 to 2 wt %, based on the entire water absorbent resin powder.

[0128] Furthermore, the smaller the amount of coarse particles having a particle diameter of 850 μm or more as defined by standard sieve classification, the better. From the viewpoint of water absorption speed, etc., the amount is preferably 0 to 5 wt %, more preferably 0 to 3 wt %, and further preferably 0 to 1 wt % based on the entire water absorbent resin powder.

[0129] Further, the ratio of particles having a particle diameter of 150 μm or more and less than 850 μm is preferably 90 weight % or more, more preferably 95 weight % or more, further preferably 98 weight % or more, and particularly preferably 99 weight % or more (upper limit is 100 weight %), based on the entire water absorbent resin powder, from the viewpoint of water absorption speed, water absorption capacity under pressure, etc.

[0130] [2-7] Surface crosslinking process This step is a step of adding a surface crosslinking agent that reacts with a functional group (particularly a carboxyl group) of the water absorbent resin powder obtained through the crushing and classification steps [2-6] to cause a crosslinking reaction, and is also called a post-crosslinking step. In the production method according to the present invention, in this step, the surface crosslinking agent is added to the water absorbent resin powder, and then the water absorbent resin powder is heated to cause a crosslinking reaction. This step includes a surface crosslinking agent adding step and a heat treatment step, and may include a cooling step after the heat treatment step as necessary.

[0131] [2-7-1] Surface cross-linking agent addition process This step is a step of preparing a water absorbent resin powder containing a surface cross-linking agent to be subjected to a surface cross-linking step by mixing the water absorbent resin powder with a surface cross-linking agent.

[0132] (Surface cross-linking agent) As the above surface cross-linking agent, a surface cross-linking agent capable of reacting with a plurality of functional groups (preferably a plurality of carboxyl groups) of the water absorbent resin, preferably a surface cross-linking agent capable of forming a covalent bond or an ionic bond, further a covalent bond, is used. Specifically, polyhydric alcohol compounds such as ethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,3-propanediol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerin, polyglycerin, 2-butene-1,4-diol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,2-cyclohexanol, trimethylolpropane, diethanolamine, triethanolamine, polyoxypropylene, oxyethylene-oxypropylene block copolymer, pentaerythritol, and sorbitol; ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol Epoxy compounds such as cerol polyglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol polyglycidyl ether, glycidol, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, trimethylolpropane polyglycidyl ether, neopentyl glycol diglycidyl ether, and 1,6-hexanediol diglycidyl ether; polyamine compounds and inorganic or organic salts thereof such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and polyethyleneimine; polyisocyanate compounds such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; aziridine compounds such as polyaziridine; polyoxazoline compounds such as 1,2-ethylenebisoxazoline, bisoxazoline, and polyoxazoline; carbonic acid derivatives such as urea, thiourea, guanidine, dicyandiamide, and 2-oxazolidinone;1,3-dioxolan-2-one (ethylene carbonate), 4-methyl-1,3-dioxolan-2-one, 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, 4-ethyl-1,3-dioxolan-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, 4,6-dimethyl-1,3-dioxan-2-one, 1,3-dioxo Examples of suitable surface crosslinking agents include alkylene carbonate compounds such as pan-2-one; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin, and polyvalent amine adducts thereof; oxetane compounds; silane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane; and polyvalent metal compounds such as hydroxides, chlorides, sulfates, nitrates, or carbonates of zinc, calcium, magnesium, aluminum, iron, and zirconium. Two or more of these may be used in combination. Among the above surface crosslinking agents, one or more selected from polyvalent metal ions, epoxy compounds, oxazoline compounds, and alkylene carbonate compounds are preferred.

[0133] (Surface cross-linking agent solution) The amount of the surface cross-linking agent added is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, still more preferably 1% by mass or less, and particularly preferably 0.1% by mass or less, based on the solid content of the water absorbent resin. The lower limit is preferably 0.001% by mass or more, more preferably 0.01% by mass or more.

[0134] The surface cross-linking agent may be added as it is, but is preferably added as a solution dissolved in water or an organic solvent from the viewpoint of ease of addition. The concentration of the surface cross-linking agent solution is preferably 1% by mass or more, more preferably 2% by mass or more. The total amount of the solvent selected from water and an organic solvent is preferably 0 to 10% by mass, more preferably 0.1% by mass to 8% by mass, and even more preferably 0.5% by mass to 5% by mass, based on the solid content of the water absorbent resin. When water and an organic solvent are used in combination, it is preferable that water is the main component.

[0135] When it is added as an aqueous solution, it is preferable because the concentration of the aqueous solution can be adjusted depending on the water content of the water absorbent resin powder at the time of contacting with the surface crosslinking agent. When the solubility of the surface crosslinking agent in water is low and the surface crosslinking agent does not become a solution, it is preferable to appropriately add a hydrophilic solvent such as alcohol to make the surface crosslinking agent into a uniform solution.

[0136] [2-6-2] Heat treatment process This step is a step of heat-treating a water-absorbent resin powder containing a surface-crosslinking agent to obtain a surface-crosslinked dried product.

[0137] (Surface crosslinking temperature) In this step, a water absorbing agent is obtained by heating the water absorbent resin powder containing a surface cross-linking agent to 100° C. or higher. The preferred maximum temperature, which varies depending on the type of the surface cross-linking agent, is 100° C. to 250° C., more preferably 120° C. to 230° C., and further preferably 150° C. to 210° C.

[0138] (time) The heat treatment process time is ,grain The heating time may be appropriately set based on the moisture content of the dried product, the type of surface crosslinking agent, the thermal efficiency of the heating device, etc. As a rough guide, heating may be performed until the moisture content becomes 10% by mass or less, and the heating time is in the range of 10 minutes to 120 minutes, and preferably 30 minutes to 90 minutes.

[0139] (Heating form) The heating device used in the surface crosslinking step is not particularly limited, but from the viewpoint of preventing uneven heating, a heating device having a stirring mechanism and using a conductive heat transfer method through solid-solid contact is preferably used.

[0140] [2-7] Cooling process Preferably, after the above-mentioned drying step or surface crosslinking step, and before the sizing step described below, a cooling step is provided in which the dried product or the surface crosslinked dried product is forcibly cooled to a desired temperature. The cooling step can be carried out using a conventionally known cooling means. The cooling temperature can be appropriately adjusted.

[0141] [2-8] Sizing process This step is a step for adjusting the particle size of the surface-crosslinked dried material. By this particle size regulation step, a water-absorbent resin powder in which the particle size or particle size distribution is more actively controlled can be obtained.

[0142] Preferably, the sizing step includes a crushing step and / or a classification step. The crushing step is a step of adjusting the particle size by crushing the granular dried material loosely aggregated after the surface treatment step with a crusher. The classification step is a step of removing coarse particles and fine powder from the surface-crosslinked granular dried material or the crushed product thereof with a classifier.

[0143] The crusher is not particularly limited, and examples thereof include a vibration mill, a roll granulator, a knuckle type crusher, a roll mill, a high-speed rotary crusher (pin mill, hammer mill, screw mill), a cylindrical mixer, etc. Those that cause little damage to the dried material or the surface-crosslinked dried material are preferred, and specific examples thereof include a roll granulator (Matsubo Corporation), a granulator (Kurimoto Iron Works, Ltd.), and a Randel Mill (Tokuju Corporation). As a classifier, a vibrating or rocking sieve classifier using a sieve net is used.

[0144] [2-9] Fine powder recycling process The "fine powder recycling step" refers to a step in which the fine powder removed in the classification step is fed to any step as is or after granulating the fine powder. Preferably, it is a step in which the fine powder or the fine powder granules are fed to a step before the drying step for reuse. The steps before the drying step are , heavy Monomer before synthesis water Examples of such processes include a crushing process for a solution, a hydrogel during polymerization, or a hydrogel after polymerization, and a drying process for a granular hydrogel. In these processes, the fine powder may be added as is, or may be added after swelling and gelling with water or granulating. In addition, water, a crosslinking agent, a binder other than water (e.g., water-soluble polymer, thermoplastic resin), a polymerization initiator, a reducing agent, a chelating agent, a coloring inhibitor, etc. may be added together with the fine powder.

[0145] The preferred amount of fine powder to be collected is appropriately determined depending on the target particle size.

[0146] [2-10] Other processes In addition to the steps described above, the production method according to the present invention may further include a grinding step, a classification step, a rewetting step, a granulation step, a transportation step, a storage step, a packaging step, a keeping step, and the like, as necessary.

[0147] (Other additives) In addition to the above-mentioned surface cross-linking agent and gel fluidizing agent, conventionally known components such as polymer powders (e.g., starches such as tapioca starch acetate), inorganic fine particles, dust inhibitors, dried water-absorbent resins (fine powder), liquid permeability improvers, and reducing agents (e.g., sodium sulfite) can be further added as other additives before or after drying.

[0148] [3] Physical properties of water-absorbent resin powder as a product Regarding the water absorbent resin powder (particularly, a surface-crosslinked water absorbent resin powder is also referred to as a water absorbing agent) obtained by the production method according to the present invention, when the water absorbent resin powder or the water absorbing agent is used in an absorbent article, particularly a paper diaper, it is desired that at least one, preferably two or more, more preferably three or more, and further preferably all of the physical properties listed in the following (3-1) to (3-7) are controlled within a desired range. When all of the following physical properties do not satisfy the following ranges, the effect of the present invention cannot be sufficiently obtained, and particularly, there is a possibility that the water absorbing agent does not exhibit sufficient performance in a so-called high-concentration paper diaper in which a large amount of the water absorbing agent is used per paper diaper.

[0149] [3-1] CRC (centrifuge holding capacity) The CRC (centrifuge retention capacity) of the water absorbent resin powder (water absorbent) of the present invention is usually 5 g / g or more, preferably 15 g / g or more, more preferably 25 g / g or more. The upper limit is not particularly limited, and a higher CRC is preferable, but from the viewpoint of the balance with other physical properties, it is preferably 70 g / g or less, more preferably 50 g / g or less, and even more preferably 40 g / g or less.

[0150] If the CRC is less than 5 g / g, the absorption amount is small and the material is not suitable for use as an absorbent for absorbent articles such as paper diapers. If the CRC is more than 70 g / g, the speed at which the material absorbs body fluids such as urine and blood decreases, making the material unsuitable for use in paper diapers with high water absorption rates. The CRC can be controlled by changing the type and amount of the internal crosslinking agent or surface crosslinking agent.

[0151] [3-2] Moisture content and solid content The moisture content of the surface-crosslinked water-absorbent resin powder (water-absorbing agent) is preferably more than 0% by mass and 20% by mass or less, more preferably 1% by mass to 15% by mass, even more preferably 2% by mass to 13% by mass, and particularly preferably 2% by mass to 10% by mass. By setting the moisture content within the above range, a water-absorbing agent having excellent powder characteristics (e.g., fluidity, transportability, damage resistance, etc.) can be obtained. In addition, the solid content of the surface-crosslinked water-absorbent resin powder (water-absorbing agent) is preferably 80% by mass or more, more preferably 85% by mass to 99% by mass, even more preferably 87% by mass to 98% by mass, and particularly preferably 90% by mass to 98% by mass.

[0152] [3-3] Particle size The mass median particle diameter d3 (D50) of the water-absorbent resin powder (water-absorbing agent) is preferably 200 μm or more, more preferably 200 μm to 600 μm, even more preferably 250 μm to 550 μm, and particularly preferably 300 μm to 500 μm. The ratio of particles having a particle diameter of less than 150 μm is preferably 10 mass% or less, more preferably 8 mass% or less, and even more preferably 6 mass% or less. The ratio of water-absorbent resin particles having a particle diameter of more than 850 μm is preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 1 mass% or less. This water-absorbing agent contains particles having a particle diameter of 150 μm to 850 μm in an amount of preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 97 mass% or more, and especially preferably 99 mass% or more. Ideally, it is 100 mass%. The logarithmic standard deviation (σζ) of the particle size distribution is preferably 0.20 to 0.50, more preferably 0.25 to 0.40, and further preferably 0.27 to 0.35.

[0153] [3-4] AAP (absorption capacity under pressure) The AAP (absorption capacity under pressure) of the water absorbent resin powder (water absorbent) is preferably 15 g / g or more, more preferably 20 g / g or more, further preferably 23 g / g or more, particularly preferably 24 g / g or more, and most preferably 25 g / g or more. The upper limit is not particularly limited, but is preferably 30 g / g or less.

[0154] If the AAP is less than 15 g / g, the amount of liquid returning when pressure is applied to the absorbent (sometimes called "Re-Wet") increases, making it unsuitable for use as an absorbent in absorbent articles such as disposable diapers. The AAP can be controlled by adjusting the particle size, changing the surface cross-linking agent, etc.

[0155] [3-5] Vortex (water absorption speed) The Vortex (water absorption speed) of the water absorbent resin powder (water absorbent) is preferably 65 seconds or less, more preferably 60 seconds or less, even more preferably 50 seconds or less, even more preferably 40 seconds or less, particularly preferably 30 seconds or less, and most preferably 25 seconds or less. The lower limit is not particularly limited, but is preferably 5 seconds or more, more preferably 10 seconds or more.

[0156] By setting the Vortex within the above range, it becomes possible to absorb a given amount of liquid in a short time. When used in the absorbent body of an absorbent article such as a disposable diaper, the time that the user feels the skin is wet is shortened, which reduces discomfort and reduces the amount of leakage.

[0157] [4] Uses of water-absorbent resin powder (water absorbent) The use of the water-absorbent resin powder (water-absorbing agent) is not particularly limited, but it is preferably used as an absorbent for absorbent articles such as paper diapers, sanitary napkins, and incontinence pads. In particular, it can be used as an absorbent for high-concentration paper diapers. Furthermore, since the water-absorbing agent has an excellent water absorption time and a controlled particle size distribution, a remarkable effect can be expected when it is used in the upper layer of the absorbent.

[0158] In addition, as the raw material of the absorbent, an absorbent material such as pulp fiber can be used together with the water absorbing agent. In this case, the content (core concentration) of the water absorbing agent in the absorbent is preferably 30% by mass to 100% by mass, more preferably 40% by mass to 100% by mass, even more preferably 50% by mass to 100% by mass, even more preferably 60% by mass to 100% by mass, particularly preferably 70% by mass to 100% by mass, and most preferably 75% by mass to 95% by mass.

[0159] By setting the core concentration within the above range, when the absorbent is used in the upper layer of an absorbent article, the absorbent article can be maintained in a clean white state. Furthermore, since the absorbent has excellent diffusibility of body fluids such as urine and blood, efficient liquid distribution is achieved, and an improvement in the absorption amount can be expected. EXAMPLES

[0160] The present invention will be described in more detail with reference to the following experimental examples. However, the present invention is not limited to these explanations, and experimental examples obtained by appropriately combining the technical means disclosed in each experimental example are also included in the scope of the present invention.

[0161] In addition, the term "water-absorbent resin" described below means a granular dried material that has been subjected to a drying process, a surface-crosslinked granular dried material or a water-absorbent resin powder, and a surface-crosslinked water-absorbent resin powder, and the term "water-containing gel" means a water-containing gel-like crosslinked polymer or a particulate water-containing gel-like crosslinked polymer that has not been subjected to a drying process.

[0162] In addition, unless otherwise noted, electric devices (including devices for measuring the physical properties of the water-absorbent resin) used in the experimental examples were powered by a 60 Hz, 200 V or 100 V power source. In addition, unless otherwise noted, the various physical properties of the water-absorbent resin and the hydrous gel described below were measured under the conditions of room temperature (20°C to 25°C) and a relative humidity of 50% RH ± 10%.

[0163] For convenience, "liter" may be expressed as "l" or "L", and "mass%" or "weight%" as "wt%". When measuring trace components, amounts below the detection limit may be expressed as ND (Non Detected).

[0164] [Physical property measurement method] (a) Centrifuge Retention Capacity (CRC) of water absorbent resin powder The CRC (centrifuge retention capacity) of the water absorbent resin powder was measured in accordance with the EDANA method (ERT441.2-02).

[0165] (b) Moisture content and solid content of water-absorbent resin powder The moisture content of the water absorbent resin powder was measured in accordance with the EDANA method (ERT430.2-02). In the measurement, the mass of the sample was changed to 1.0 g, the drying temperature was changed to 180° C., and the moisture content and solid content of the water absorbent resin powder were calculated from the loss on drying when the sample was dried for 3 hours.

[0166] (c) Mass average particle diameter (d3) of the water absorbent resin powder The mass median particle diameter (d3) of the water absorbent resin powder was measured in accordance with the method described in columns 27 and 28 of US Pat. No. 7,638,570.

[0167] (d) Conversion rate of hydrogel 1.00 g of the sampled hydrogel was added to 1000 g of ion-exchanged water at room temperature (the polymerization reaction was substantially stopped at this point), and the mixture was stirred at 300 rpm for 2 hours, followed by filtration to remove insoluble matter. The amount of monomer extracted in the filtrate obtained by the above operation was measured using a liquid chromatograph. When the amount of the monomer was taken as the residual monomer amount m (g), the polymerization rate C (mass%) of the hydrogel was calculated according to the following (Equation 8). It is preferable to measure the polymerization rate immediately after sampling the hydrogel, but if it takes time from sampling to measurement, it is necessary to perform a polymerization termination operation by forced cooling (contact with dry ice, liquid nitrogen, ice water, etc.).

[0168] C (mass%)=100×{1-m / (M×α / 100)} (Formula 8) In the formula (8), M is the mass (g) of the water-containing gel, and α is the solid content (mass%) of the water-containing gel.

[0169] (e) Solid content of hydrous gel The water content of the hydrous gel was measured according to the EDANA method (ERT430.2-02). In the measurement, the mass of the sample was changed to 2.0 g, the drying temperature to 180 ° C, and the drying time to 24 hours. Specifically, 2.0 g of the hydrous gel was placed in an aluminum cup with a bottom diameter of 50 mm, and then the total mass W1 (g) of the sample (hydrous gel and aluminum cup) was accurately weighed. Next, the sample was placed in an oven with an atmospheric temperature set to 180 ° C. After 24 hours, the sample was removed from the oven and the total mass W2 (g) was accurately weighed. When the mass of the hydrous gel used in this measurement was M (g), the solid content α (mass%) of the hydrous gel was calculated according to the following (Equation 10).

[0170] α (mass%)=100-{(W1-W2) / M}×100 (Equation 10).

[0171] (f) Particle size of particulate hydrogel The mass average particle diameter (D50) of the particulate hydrogel was measured in accordance with the method described in WO2016 / 204302.

[0172] That is, 20 g of a hydrogel (solid content α (mass%)) at a temperature of 20 to 25°C was added to 1,000 g of a 20 mass% aqueous sodium chloride solution (hereinafter referred to as "aqueous EMAL solution") containing 0.08 mass% EMAL 20C (surfactant, manufactured by Kao Corporation) to prepare a dispersion, and the mixture was stirred at 300 rpm for 16 hours using a stirrer tip with a length of 50 mm and a diameter of 7 mm (a cylindrical polypropylene container with a height of 21 cm and a diameter of 8 cm, approximately 1.14 L, was used).

[0173] After stirring, the above dispersion was poured into the center of a JIS standard sieve (inner diameter 20 cm, sieve openings: 8 mm / 4 mm / 2 mm / 1 mm / 0.60 mm / 0.30 mm / 0.15 mm / 0.075 mm) placed on a rotating plate. After washing out all the hydrous gel onto the sieve using 100 g of an aqueous solution of EMAL, 6,000 g of the aqueous solution of EMAL was poured from above using a shower (72 holes, liquid volume: 6.0 [L / min]) from a height of 30 cm, while rotating the sieve by hand (20 rpm). 2The hydrous gel was classified by pouring the water evenly over the sieve four times so that the water was distributed over the entire sieve. The hydrous gel on the first sieve was drained for about 2 minutes and then weighed. The second and subsequent sieves were classified in the same manner, and the hydrous gel remaining on each sieve after draining was weighed. The type of sieve was appropriately changed depending on the particle size of the hydrous gel. For example, when the particle size of the hydrous gel is fine and clogging occurs in sieves with 0.15 mm or 0.075 mm openings, JIS standard sieves with larger diameters (diameter 30 cm, openings 0.15 mm and 0.075 mm) were used.

[0174] The proportion (mass%) of the hydrogel in the total hydrogel was calculated from the mass of the hydrogel remaining on each sieve using the following formula (11). The mesh size of the sieve after draining was determined according to the following formula (12), and the particle size distribution of the hydrogel was plotted on logarithmic probability paper. The particle size at which the cumulative sieve %R of the plot corresponds to 50 mass% was taken as the mass average particle size (D50) of the hydrogel with solid content α (mass%).

[0175] X(%)=(w / W) × 100 (Equation 11) R(α)(mm)=(20 / W) 1 / 3 × r... (Equation 12) In addition, here, X: Mass percentage (%) of the hydrous gel remaining on each sieve after classification and draining w: Mass (g) of the hydrogel remaining on each sieve after classification and draining W: Total mass of the hydrogel remaining on each sieve after classification and draining (g) R(α): Sieve opening (mm) when converted into a hydrous gel with solid content α (mass%) r: The mesh size (mm) of the sieve used to classify the hydrous gel swollen in a 20% by mass sodium chloride aqueous solution.

[0176] (g) Mass average particle diameter (d1) of the particulate hydrogel converted into solid content In accordance with WO2016 / 204302, the particle size d1 of the particulate hydrogel converted into solid content (mass average particle size of the particulate hydrogel converted into solid content in a dried product) was calculated from the solid content α (mass%) of the particulate hydrogel obtained in (e) above and the mass average particle size (D50) of the hydrogel having the solid content α (mass%) obtained in (f) above, according to the following (Equation 14). SolidD50(d1)=GelD50×(α / 100) 1 / 3 ... (Equation 14) In addition, here, GelD50: Mass average particle size (μm) of particulate hydrogel with solid content α (mass%) α: solid content of particulate hydrogel (mass%) SolidD50 (d1): Mass average particle size (μm) converted into the solid content of the hydrous gel.

[0177] (h) Vortex (absorption time) of water-absorbent resin powder The Vortex (water absorption time) of the water absorbent resin powder was measured according to the following procedure. First, 0.02 parts by mass of edible blue No. 1 (brilliant blue), which is a food additive, was added to 1000 parts by mass of previously prepared physiological saline (0.9% by mass aqueous sodium chloride solution), and the liquid temperature was then adjusted to 30°C.

[0178] Next, 50 ml of the physiological saline was measured out into a 100 ml beaker, and 2.0 g of the water absorbent resin powder was added while stirring at 600 rpm using a stirrer tip with a length of 40 mm and a diameter of 8 mm. The time from the time of adding the water absorbent resin powder to the time when the water absorbent resin powder absorbed the physiological saline and covered the stirrer tip was measured as a Vortex (absorption time) (unit: seconds).

[0179] (i) AAP (absorbency under pressure) of water-absorbent resin powder The AAP (absorption capacity under pressure) of the water absorbent resin powder was measured in accordance with the EDANA method (ERT442.2-02). Note that the load condition was changed to 4.83 kPa (0.7 psi) during the measurement.

[0180] (j) Average residence time The average residence time (seconds) of the hydrogel in the gel crusher was determined according to the following method.

[0181] First, in Production Example 1 described later, Monomer Water Add 1% by weight (based on the amount of Blue No. 1) to the solution. Monomer Water Polymerization was carried out in the same manner, except that a blue-colored hydrogel (solution) was added, to separately prepare a hydrogel colored blue. Next, the uncolored hydrogel was added to the gel crusher at a predetermined feeding speed to allow stable operation. Without changing the feeding speed of the hydrogel, the blue-colored hydrogel was added instead of the hydrogel for 2±5 seconds, and then the uncolored hydrogel was added at the same speed to continue gel crushing. The particulate hydrogel discharged from the gel crusher was sampled every 5 seconds, with the start of the feeding of the blue hydrogel being set as 0 seconds.

[0182] 15 g of the sampled hydrous gel was placed in a polyethylene bag with a zipper (size A, manufactured by Nippon Seisakusho Co., Ltd., length 70 mm, width 50 mm, thickness 0.04 mm), and then a weight (15 kg) with a square bottom of length and width 80 mm was placed on top of the bag for 5 seconds to form it into a sheet. At that time, care was taken not to trap air inside the bag. Next, the b value of the obtained sheet-like sample was measured using a spectrophotometer SZ-Σ80 COLOR MEASURING SYSTEM (manufactured by Nippon Denshoku Industries Co., Ltd.) under the measurement conditions of reflection measurement / standard white board No. 1 / 30φ projector pipe. Five measurements were taken for each sample, and the average value was calculated. Note that a weight was placed on the sample after each measurement to adjust the shape of the sample. The b value was calculated in the same manner for the hydrous gel sampled every 5 seconds. The stronger the blueness of the hydrous gel, the smaller the b value (less than 0 and larger absolute value). The sampling time of the hydrogel with the strongest blue color (minimum b value) was defined as the average residence time (min). When the gel crushing process was carried out multiple times, the average residence time was measured for each time, and the sum of these was defined as the average residence time (min).

[0183] [Production Example 1] An aqueous monomer solution was prepared consisting of 300 parts by mass of acrylic acid, 100 parts by mass of 48% by mass sodium hydroxide aqueous solution, 0.61 parts by mass of polyethylene glycol diacrylate (average n number 9), 16.4 parts by mass of 0.1% by mass aqueous solution of trisodium diethylenetriaminepentaacetate, and 273.2 parts by mass of deionized water.

[0184] Next, the above-mentioned monomer aqueous solution adjusted to 38°C was continuously fed by a metering pump, and then 150.6 parts by mass of a 48% by mass aqueous sodium hydroxide solution was continuously mixed by line mixing. At this time, the liquid temperature of the monomer aqueous solution rose to 87°C due to heat of neutralization.

[0185] Furthermore, 14.6 parts by mass of a 4% by mass aqueous solution of sodium persulfate was continuously mixed by line mixing, and then the mixture was transferred to a continuous polymerization machine having a flat polymerization belt equipped with weirs on both ends. The monomer solution is The mixture was continuously fed so that the thickness was 10 mm. Thereafter, polymerization was continuously performed for a polymerization time of 3 minutes to obtain a strip-shaped (sheet-shaped) hydrogel crosslinked polymer (1a). The obtained strip-shaped hydrogel (1a) was cut in accordance with the processing speed and feeding interval of a gel crusher described later to obtain a strip-shaped hydrogel (1b) having a width of several centimeters. For example, when the processing speed of the gel crusher is 0.64 kg / min and the strip-shaped hydrogel is fed at intervals of 2.5 seconds, the mass of each strip-shaped hydrogel is 0.0267 kg. The polymerization rate of the strip-shaped hydrogel (1b) was 98.5% by mass and the solid content rate was 53% by mass.

[0186] [Experimental Example 1] <Gel crushing> As a gel crushing device, a twin-shaft kneader equipped with a main body (barrel) containing two rotating shafts rotating in the same direction was used to crush the strip-shaped hydrogel (1b). Each rotating shaft was equipped with a circular disk, which was the main crushing means. The barrel had a jacket structure, and had a gas inlet penetrating the jacket to inject water vapor into the main body.

[0187] First, a heat medium at 60°C was circulated inside the jacket to maintain the temperature inside the main body (barrel) at 60°C. Then, the rotation speed was set to 40 rpm, and the rectangular hydrogel (1b) heated to 60°C was fed into the inlet of the twin-screw kneader at a rate of 0.64 kg / min. At that time, water at 60°C was fed from the inlet simultaneously with the hydrogel (1b), and steam at 0.6 MPa was fed from the gas inlet. The amount of water fed at 60°C was 11.8% by mass relative to the solid content of the rectangular hydrogel (1b). The amount of steam fed at 0.6 MPa was 9.7% by mass relative to the solid content of the rectangular hydrogel (1b). The diameter D of the disks used for gel crushing was as shown in Table 1, and the minimum clearance between the barrel and the disk was 6 mm (15% of the disk diameter D). The gel crushing conditions are shown in Table 1. The properties of the particulate hydrogel (A) obtained by crushing are shown in Table 2. The GGE during gel crushing was 19 J / g.

[0188] <Drying / Surface treatment> The obtained particulate hydrogel (A) was dried using a hot air dryer. This dryer was equipped with a basket (bottom size 30 cm x 20 cm) made of a wire mesh with an opening of 1.2 mm. 500 g of the particulate hydrogel (A) was spread almost uniformly on the bottom surface of the basket, and hot air of 190 ° C. was blown from below for 30 minutes to obtain a dried product. Thereafter, the cooled dried product was fed to a roll mill and pulverized, and classified using JIS standard sieves with openings of 850 μm and 150 μm. The component that passed through the 850 μm sieve and did not pass through the 150 μm sieve was collected to obtain a water-absorbent resin powder (AP1).

[0189] Next, a surface cross-linking agent solution consisting of 0.025 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of ethylene carbonate, 0.5 parts by mass of propylene glycol, and 2.0 parts by mass of deionized water was sprayed and mixed into 100 parts by mass of the water absorbent resin powder (AP1). This mixture was heat-treated at 200°C for 35 minutes to obtain a surface-cross-linked water absorbent resin powder (AP2). The physical properties of the surface-cross-linked water absorbent resin powder (AP2) are shown in Table 3.

[0190] [Experimental Example 2] Particulate hydrogel (B) was obtained in the same manner as in Experimental Example 1, except that the minimum clearance between the barrel and the disk was changed to 2 mm (4.16% of the disk diameter D). The disk arrangement pattern was the same as in Experimental Example 1, and the GGE during gel crushing was 41 J / g. The gel crushing conditions are shown in Table 1. The properties of the particulate hydrogel (B) obtained by crushing are shown in Table 2.

[0191] The particulate hydrogel (B) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (BP1) and a surface-crosslinked water-absorbent resin powder (BP2). The physical properties are shown in Table 3.

[0192] [Experimental Example 3] The heating temperature of the rectangular hydrous gel (1b) (gel temperature T1 fed into the inlet of the gel crusher) was changed to 80°C, and a 10% by mass aqueous solution of lauryl dimethyl amino acetate betaine was fed from the inlet simultaneously with the rectangular hydrous gel (1b). The temperature of the water fed was changed to 90°C, the rotation speed of the rotating shaft was changed to 100 rpm, the heat medium temperature of the jacket was changed to 105°C (i.e., the temperature inside the main body was kept at 105°C), and the minimum clearance between the barrel and the disk was changed to 1 mm (2% of the disk diameter D). Except for this, a particulate hydrous gel (C) was obtained in the same manner as in Experimental Example 1. The amount of lauryl dimethyl amino acetate betaine fed as a solid content was 0.15% by mass relative to the solid content of the rectangular hydrous gel (1b). The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (C) obtained by crushing are shown in Table 2. The GGE during gel crushing was 125 J / g.

[0193] The particulate hydrogel (C) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (CP1) and a surface-crosslinked water-absorbent resin powder (CP2). The physical properties are shown in Table 3.

[0194] [Experimental Example 4] A particulate hydrous gel (D) was obtained in the same manner as in Experimental Example 1, except that the heating temperature of the strip-shaped hydrous gel (1b) (gel temperature T1 fed into the inlet of the gel crusher) was changed to 70°C, water and steam were not supplied, the rotation speed of the rotating shaft was changed to 100 rpm, the heat medium temperature of the jacket was changed to 80°C (i.e., the temperature inside the main body was maintained at 80°C), and the minimum clearance between the barrel and the disk was changed to 1 mm (2% of the disk diameter D). The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (D) obtained by crushing are shown in Table 2. The GGE during gel crushing was 54 J / g.

[0195] The particulate hydrogel (D) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (DP1) and a surface-crosslinked water-absorbent resin powder (DP2). The physical properties are shown in Table 3.

[0196] [Experimental Example 5] The heating temperature of the strip-shaped hydrous gel (1b) (gel temperature T1 fed into the inlet of the gel crusher) was changed to 80°C, the speed of the strip-shaped hydrous gel (1b) was changed to 0.45 kg / min, the temperature of the water to be fed was changed to 90°C, the minimum clearance between the barrel and the disk was changed to 1 mm (2% of the disk diameter D), the rotation speed of the rotating shaft was changed to 70 rpm, and the heat medium temperature of the jacket was changed to 105°C. Except for this, a particulate hydrous gel (E) was obtained in the same manner as in Experimental Example 1. The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (E) obtained by crushing are shown in Table 2. The GGE during gel crushing was 10 J / g.

[0197] When the particulate hydrogel (E) was subjected to a drying treatment in the same manner as in Experimental Example 1, the drying of the coarse gel particles of about 10 mm present in the particulate hydrogel (E) was insufficient, and the dried product was not suitable for the subsequent roll mill grinding process.

[0198] [Experimental Example 6] The same operation as in Experimental Example 4 was performed except that the temperature of the rectangular hydrous gel (1b) was changed to room temperature (20°C), water and steam were not supplied, and the heat medium temperature of the jacket was changed to room temperature (20°C) (i.e., the temperature inside the main body was kept at room temperature (20°C)). As a result, the device stopped due to overload. After the stoppage, the barrel was opened to check the contents, and it was found that the hydrous gel (F) had integrated into a mochi-like shape and was not suitable for the subsequent manufacturing process.

[0199] [Experimental Example 7] Particulate hydrous gel (G) was obtained in the same manner as in Experimental Example 4, except that 90°C water was supplied from the inlet simultaneously with the strip-shaped hydrous gel (1b). The disk pattern was the same as in Experimental Example 4, but the GGE during gel crushing was 48 J / g. The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (G) obtained by crushing are shown in Table 2.

[0200] The particulate hydrogel (G) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (GP1) and a surface-crosslinked water-absorbent resin powder (GP2). The physical properties are shown in Table 3.

[0201] [Experimental Example 8] Particulate hydrogel (H) was obtained in the same manner as in Experimental Example 3, except that 0.6 MPa water vapor was not supplied. The disk pattern was the same as in Experimental Example 3, but the GGE during gel crushing was 157 J / g. The gel crushing conditions are shown in Table 1. The properties of the particulate hydrogel (H) obtained by crushing are shown in Table 2.

[0202] The particulate hydrogel (H) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (HP1) and a surface-crosslinked water-absorbent resin powder (HP2). The physical properties are shown in Table 3.

[0203] [Experimental Example 9] Particulate hydrous gel (I) was obtained in the same manner as in Experimental Example 3, except that the heat medium temperature of the jacket was changed to 60°C (i.e., the temperature inside the main body was maintained at 60°C). The disk pattern was the same as in Experimental Example 3, but the GGE during gel crushing was 135 J / g. The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (I) obtained by crushing are shown in Table 2.

[0204] The particulate hydrogel (I) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (IP1) and a surface-crosslinked water-absorbent resin powder (IP2). The physical properties are shown in Table 3.

[0205] [Experimental Example 10] A particulate hydrous gel (J) was obtained in the same manner as in Experimental Example 2, except that a 10% by mass aqueous solution of polyethylene glycol 2000 (manufactured by Tokyo Chemical Industry Co., Ltd., weight average molecular weight 2,000) was supplied from the inlet simultaneously with the strip-shaped hydrous gel (1b). The amount of polyethylene glycol 2000 supplied as a solid content was 0.8% by mass relative to the solid content of the strip-shaped hydrous gel (1b). The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (J) obtained by crushing are shown in Table 2. The GGE during gel crushing was 38 J / g.

[0206] The particulate hydrogel (J) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (JP1) and a surface-crosslinked water-absorbent resin powder (JP2). The physical properties are shown in Table 3.

[0207] [Experimental Example 11] A particulate hydrous gel (K) was obtained in the same manner as in Experimental Example 2, except that a 10% by mass aqueous solution of KF-354L (Shin-Etsu Chemical Co., Ltd., side-chain polyether-modified polysiloxane) was supplied from the inlet simultaneously with the strip-shaped hydrous gel (1b). The amount of KF-354L supplied as a solid content was 0.05% by mass relative to the solid content of the strip-shaped hydrous gel (1b). The gel crushing conditions are shown in Table 1. The properties of the particulate hydrous gel (K) obtained by crushing are shown in Table 2. The GGE during gel crushing was 36 J / g.

[0208] The particulate hydrogel (K) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (KP1) and a surface-crosslinked water-absorbent resin powder (KP2). The physical properties are shown in Table 3.

[0209] [Experimental Example 12] The heating temperature of the rectangular hydrous gel (1b) (gel temperature T1 fed into the inlet of the gel crushing device) was changed to 80°C, the processing speed of the rectangular hydrous gel (1b) was changed to 0.36 kg / min, and the powder of tapioca acetate starch BK-V (manufactured by Tokai Starch Co., Ltd.) was fed from the inlet simultaneously with the rectangular hydrous gel (1b), the rotation speed of the rotating shaft was set to 50 rpm, the amount of water fed was set to 52.2% by mass relative to the solid content of the rectangular hydrous gel (1b), and the heat medium temperature of the jacket was changed to 90°C (i.e., the temperature inside the main body was maintained at 90°C). Except for this, the particulate hydrous gel (L) was obtained in the same manner as in Experimental Example 7. The amount of tapioca acetate starch BK-V fed as a solid content was 25% by mass relative to the solid content of the rectangular hydrous gel (1b). The gel crushing conditions are shown in Table 1. The properties of the particulate hydrogel (L) obtained by pulverization are shown in Table 2. The GGE when the gel was pulverized was 30 J / g.

[0210] The particulate hydrogel (L) was dried / surface-treated in the same manner as in Experimental Example 1 to obtain a water-absorbent resin powder (LP1) and a surface-crosslinked water-absorbent resin powder (LP2). The physical properties are shown in Table 3.

[0211] In Table 1, gel temperature T1 represents the gel temperature at the inlet of the gel crusher, and gel temperature T2 represents the gel temperature at the outlet of the gel crusher. In Table 2, d1 represents the mass average particle diameter of the particulate hydrogel in terms of solid content. In Table 3, d3 represents the mass average particle diameter of the water absorbent resin powder. Except for Example 6 In all the Examples, the hydrogel crosslinked polymer was continuously pulverized by the pulverizing means at 50° C. or higher. Except for Example 6 In all the examples, the inside of the main body was heated to 50° C. or higher before the hydrogel was poured in.

[0212] [Table 1]

[0213] [Table 2]

[0214] [Table 3]

[0215] In the production method according to the present invention, the hydrogel crosslinked polymer obtained in the polymerization step was gel-pulverized using a kneader having multiple axes to obtain a gel pulverized product that can be used in the subsequent steps. Furthermore, the obtained water-absorbent resin powder also showed an excellent absorption rate (Experimental Examples 1 to 4, 7 to 12).

[0216] Comparing Experimental Examples 1 and 2, it was confirmed that by reducing the clearance between the barrel and the disk, the particle size of the particulate hydrous gel was reduced, and further the water absorption rate of the water-absorbent resin powder was improved.

[0217] Comparing Experimental Examples 4 and 7, it was confirmed that by crushing the gel while supplying water into the main body, the particle size of the particulate hydrous gel increases, but the water absorption rate of the water-absorbent resin powder increases.

[0218] From a comparison of Experimental Examples 3, 8 and 9, it was confirmed that the water absorption rate of the water absorbent resin powder was improved by carrying out gel crushing at high temperatures (100°C or higher) while supplying water vapor into the main body.

[0219] From a comparison of Experimental Examples 2, 10, and 11, it was confirmed that by adding a gel fluidizing agent simultaneously with a hydrous gel and carrying out gel crushing, the particle size of the particulate hydrous gel increases, but the water absorption rate of the water absorbent resin powder is improved. [Industrial Applicability]

[0220] The water-absorbent resin powder obtained by the present invention is suitable for use as an absorbent for sanitary products such as disposable diapers.

[0221] This application is based on Japanese Patent Application No. 2020-161054, filed on September 25, 2020, the disclosure of which is incorporated herein by reference in its entirety. [Explanation of symbols]

[0222] 200 Gel crushing device 204...Inlet 206 Rotating shaft 208... Body (barrel) 210...Discharge port 212... Crushing means 214 Drive unit 216 Gas inlet

Claims

1. a polymerization step of polymerizing the aqueous monomer solution to obtain a hydrous gel-like crosslinked polymer; a gel crushing step of crushing the hydrogel crosslinked polymer using a gel crushing device after the polymerization step to obtain a particulate hydrogel crosslinked polymer; A drying step of drying the particulate hydrogel crosslinked polymer to obtain a dried product, The gel crushing device includes an inlet, an outlet, and a main body incorporating a plurality of rotating shafts, each of which has a crushing means; the hydrogel-like cross-linked polymer advances from the inlet toward the outlet in a direction in which the multiple rotation shafts extend, In the gel crushing step, the hydrogel crosslinked polymer is continuously fed through the inlet, the hydrogel crosslinked polymer is continuously crushed by the crushing means at 50° C. or higher, and a particulate hydrogel crosslinked polymer is continuously taken out through the outlet, The polymerization rate of the hydrogel crosslinked polymer to be introduced into the introduction port is 90% by mass or more, The method for producing a water-absorbent resin powder, wherein the particulate hydrogel-like crosslinked polymer discharged from the discharge port has a mass average particle diameter d1 calculated as a solid content of 3 mm or less.

2. 2. The method according to claim 1, wherein the hydrogel crosslinked polymer fed into the feed port has a gel temperature T1 of 50° C. or higher.

3. The method according to claim 1 or 2, wherein the gel crushing device is a continuous double-shaft kneader.

4. The method according to any one of claims 1 to 3, wherein the gel grinding device has a heating and / or heat retention means.

5. The manufacturing method according to any one of claims 1 to 4, wherein the gel temperature T2 at the outlet of the gel crusher is higher than the gel temperature T1 at the inlet.

6. A method for producing a water-absorbent resin powder as described in any one of claims 1 to 5, wherein the hydrous gel-like cross-linked polymer advances in the axial direction of the multiple rotating shafts from the inlet toward the outlet while being pulverized by the pulverizing means.

7. A method for producing an absorbent resin powder according to any one of claims 1 to 6, wherein in the gel crushing device, the inlet is provided near one end of the rotating shaft and the outlet is provided near the other end of the rotating shaft.

8. A method for producing a water-absorbent resin powder according to any one of claims 1 to 7, wherein in the gel crushing device, the discharge outlet is provided near the rear of the main body.

9. The method according to any one of claims 1 to 8, wherein the aqueous monomer solution contains an acid group-containing unsaturated monomer as a main component.

10. A manufacturing method described in any one of claims 1 to 9, wherein the crushing means possessed by each of the rotating shafts is at least one selected from a disk, a chip, a paddle, an element, a kneading, and a rotor.

11. The manufacturing method described in claim 10, wherein the minimum clearance C of the gel crushing device is 0.2 to 20% of the maximum diameter D of the disk.

12. A manufacturing method as described in claim 10 or 11, wherein the ratio L / D of the effective length L (Length) inside the main body to the maximum diameter D of the disk is 5 to 40.

13. The method according to any one of claims 1 to 12, wherein the gel temperature T2 at the outlet of the gel crusher is 60 to 140 ° C.

14. The method according to any one of claims 1 to 13, wherein the inside of the body is heated to 50°C or higher before the hydrogel crosslinked polymer is introduced through the inlet.

15. The hydrogel crosslinked polymer obtained after the polymerization step is in a sheet form, and the method further comprises a shredding step of shredding the sheet-like hydrogel crosslinked polymer before the gel crushing step. The method according to any one of claims 1 to 14.

16. The manufacturing method according to any one of claims 1 to 15, wherein water and / or water vapor is supplied to the inside of the body in the gel crushing step.

17. The method according to claim 16, wherein the temperature of the water and / or steam supplied to the inside of the body is 50 to 120°C.

18. The method according to claim 16 or 17, wherein the pressure of the steam supplied to the inside of the body is 0.2 to 0.8 MPa.

19. The method according to any one of claims 1 to 18, wherein the solid content of the hydrogel crosslinked polymer fed into the feed port is 25 to 75 mass%.

20. The method according to any one of claims 1 to 19, wherein the particulate hydrogel crosslinked polymer discharged from the outlet has a solid content of 25 to 75 mass%.

21. The method according to any one of claims 1 to 20, wherein the hydrogel crosslinked polymer is a crosslinked body mainly composed of poly(meth)acrylic acid (salt).

Citation Information

Patent Citations

  • Novel polymerization process

    JP1982034101A

  • Novel continuous polymerization

    JP1985055002A

  • Producti0n of water-containing gelatinous polymer particle and water-absorbing resin

    JP1993112654A

  • Production of hydrophilic resin

    JP1999188727A

  • Cracking method for hydrous gel of water-soluble (METH)acrylic acid polymer

    JP2004002562A