How to collect PGM

By adding base metal oxides to molten slag and employing oxidation smelting, the method addresses inefficiencies in PGM recovery from slag, achieving higher yields and reduced waste through enhanced separation and concentration of PGM alloys.

JP7595305B2Active Publication Date: 2024-12-06WASEDA UNIV +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021533916
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-14
Filing Date
2020-07-06
Publication Date
2024-12-06
Estimated Expiration
2040-07-06

AI Technical Summary

Technical Problem

Existing methods for recovering platinum group metals (PGM) from molten slag in the smelting process are inefficient, as PGM remains in the discharged slag, leading to waste and reduced recovery yields.

Method used

A method involving the addition of base metal oxides, such as copper, iron, tin, or nickel oxides, to the molten slag during the reduction smelting process, followed by oxidation smelting to separate and recover PGM alloys, with specific conditions on oxide addition amounts and holding times to enhance recovery.

Benefits of technology

The method effectively recovers PGM from molten slag by concentrating PGM in the alloy phase, improving recovery rates and reducing waste, with enhanced efficiency and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595305000004
    Figure 0007595305000004
  • Figure 0007595305000005
    Figure 0007595305000005
  • Figure 0007595305000006
    Figure 0007595305000006
Patent Text Reader

Abstract

A PGM recovery method wherein the following steps are performed in order to recover a PGM alloy: a reduction smelting step in which a PGM-including processing target, a base metal and / or a base metal oxide, a flux, and a reduction agent are inserted into a reduction kiln that is used for reduction smelting, and these are heated and melted to form a molten slag and a reduction kiln metal an extraction step in which the molten slag is extracted from the reduction kiln to obtain a PGM-including reduction kiln metal; and an oxidization smelting step in which the reduction kiln metal is transferred to an oxidization kiln that is used for oxidization smelting, the reduction kiln metal is oxidized and melted, and a base metal oxide slag and a PGM alloy are formed, then the base metal oxide slag is extracted to obtain a PGM alloy in which the PGM is concentrated. In this PGM recovery method, at least one type of base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide, and lead oxide is added to the molten slag.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering platinum group metals (sometimes referred to as "PGM" in the present invention) from materials containing PGM, such as used catalysts for purifying automobile exhaust gas, used electronic circuit boards and lead frames, used petrochemical catalysts, etc. [Background technology]

[0002] Conventionally, methods have been proposed for recovering PGMs from various PGM-containing materials, such as used automobile exhaust gas purification catalysts, that are treated as objects to be treated. For example, the applicant of the present invention has disclosed an efficient dry PGM recovery method in which a PGM-containing object to be treated is heated and melted together with a copper source material, and the PGMs are absorbed in the molten metal that is produced (see Patent Document 1).

[0003] In the dry recovery method of PGM according to Patent Document 1, a material to be treated containing PGM and a copper source material containing copper oxide are loaded into a closed reduction furnace together with a flux component and a reducing agent and melted. The PGM is concentrated in the molten metal that settles below the generated molten slag mainly composed of oxides and then recovered (sometimes referred to as the "reduction smelting process" in the present invention). Meanwhile, the molten slag with a reduced copper content is discharged from the reduction furnace, and a granular copper source material having a certain particle size is used as the copper source material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-24263 A Summary of the Invention [Problem to be solved by the invention]

[0005] The inventors of the present invention, not satisfied with the above results, have conducted research into a more efficient method for recovering PGMs from treated materials that contain PGMs. They have noticed that while the method of Patent Document 1 recovers PGMs from treated materials with high efficiency and high yield, PGMs remain in the molten slag discharged from the recovery process. The problem to be solved by the present invention is to provide a method for recovering the PGM remaining in this molten slag. [Means for solving the problem]

[0006] As a result of studying methods for recovering PGM remaining in molten slag, the inventors have come up with the idea that PGM can be recovered by adding base metal oxides to the molten slag.

[0007] That is, the first invention for solving the above-mentioned problems is: a reduction smelting process in which the PGM-containing workpiece, base metals and / or base metal oxides, flux and a reducing agent are placed in a reduction furnace used for reduction smelting, heated and melted to form molten slag and reduction furnace metal; extracting the molten slag from the reduction furnace to obtain reduction furnace metal containing PGM; a step of transferring the reduction furnace metal to an oxidation furnace for oxidation smelting, oxidizing and melting the metal to form a slag of base metal oxides and a PGM alloy, and then extracting the base metal oxide slag to obtain a PGM alloy enriched in PGM, This method for recovering PGM is characterized in that at least one base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide is added to the molten slag, and the PGM alloy contained in the molten slag is recovered. The second invention is The method for recovering PGM according to the first aspect of the present invention is characterized in that the base metal oxide is added in an amount of less than 35% by mass relative to the mass of the molten slag. The third invention is This is a method for recovering PGM according to either the first or second invention, characterized in that at least one base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide is added to the molten slag, and a holding time of at least two hours is set when recovering the PGM alloy contained in the molten slag. The fourth invention is The method for recovering PGM according to any one of the first to third aspects of the present invention is characterized in that the base metal oxide is added in an amount of 10 to 500 times the mass of the PGM contained in the molten slag. Effect of the Invention

[0008] According to the invention, PGM alloys can be recovered from the molten slag by adding base metal oxides to the molten slag. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a process flow diagram of a method for recovering PGM from molten slag according to the present invention. [Diagram 2] FIG. 1 is a process flow diagram of a method for recovering PGMs from molten slag according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a process flow diagram of a prior art PGM recovery process. [Figure 4] This is a graph in which the vertical axis represents the Pt concentration in the molten slag sample after the recovered metal is separated, and the horizontal axis represents the sampling time after the base metal oxide is added. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The PGM recovery method according to the present invention will be described with reference to the drawings (FIGS. 1 to 3) in the following order: [1] reduction smelting process, [2] oxidation smelting process, [3] problems with the reduction smelting process according to the conventional technology and solutions thereto, [4] the reduction smelting process according to the present invention, [5] the oxidation smelting process according to the present invention, and [6] an example of the PGM recovery method according to the present invention. FIG. 1 is a process flow diagram of a method for recovering PGMs from molten slag according to the present invention, FIG. 2 is a process flow diagram of a method for recovering PGMs from molten slag according to a different embodiment of the present invention, and FIG. 3 is a process flow diagram of a method for recovering PGMs according to the prior art. The raw materials, additives, products, waste materials and steps used in the process flows of these PGM recovery methods are given numbers, and raw materials etc. given the same numbers are similar.

[0011] That is, the first invention for solving the above-mentioned problems is: The PGM-containing material to be treated, the base metal and / or base metal oxide, the flux, and the reducing agent are placed in a reduction furnace used for reduction smelting and heated. of a reduction smelting step for melting the molten slag and reducing furnace metal; extracting the molten slag from the reduction furnace to obtain reduction furnace metal containing PGM; The reduction furnace metal is transferred to an oxidation furnace for oxidation smelting, where it is oxidized and melted to form a slag of base metal oxides and a PGM alloy. , base an oxidation smelting step to extract metal oxide slag and obtain a PGM-enriched alloy, From the top of the reduction furnace to the molten slag before the molten slag is extracted from the reduction furnace, or to the molten slag that is kept in a molten state using a reduction furnace separate from the reduction furnace; At least one base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide is added. The molten slag is allowed to settle. and recovering the PGM alloy contained in the molten slag. The second invention is The method for recovering PGM according to the first aspect of the present invention is characterized in that the base metal oxide is added in an amount of less than 35% by mass relative to the mass of the molten slag. The third invention is This is a method for recovering PGM according to either the first or second invention, characterized in that at least one base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide is added to the molten slag, and a holding time of at least two hours is set when recovering the PGM alloy contained in the molten slag. The fourth invention is The method for recovering PGM according to any one of the first to third aspects of the present invention is characterized in that the base metal oxide is added in an amount of 10 to 500 times the mass of the PGM contained in the molten slag.

[0012] [1] Reduction smelting process As shown in Fig. 3, the PGM-containing material to be treated (2), for example, crushed ceramic automobile catalyst, the extractant (3) such as base metals and / or base metal oxides, the flux (1) such as CaO and / or SiO2, and the reducing agent (4) such as a C (carbon)-containing material are loaded into a reduction furnace (5) for reduction smelting. Electricity is then applied to the electrodes in the furnace to heat and melt the loaded material.

[0013] In the present invention, the base metal refers to a metal having a higher ionization tendency than PGM. However, when considering using a base metal as the extractant (3), copper, iron, tin, nickel and lead are preferred from the viewpoints of ease of handling, cost, etc. Accordingly, preferred examples of the base metal oxide include copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide. For example, when copper is used as the base metal, copper oxide is also used as the base metal oxide, and when iron is used, iron oxide is also used. In view of increasing the efficiency of recovery of PGM, it is preferred to use the same metal for the base metal and the base metal oxide. Typically, it is particularly preferred to use copper as the base metal and copper oxide as the base metal oxide from the viewpoint of increasing the recovery rate of PGM.

[0014] Examples of the reducing agent (4) that can be used include C (carbon), SiC, CO gas, methane gas, propane gas, ammonia gas, and metals such as metallic Al and Ti that are more easily oxidized than the above-mentioned base metals. These reducing agents saturate the atmosphere with carbon, making it reducing, and reduce the copper oxide dissolved in the slag.

[0015] Then, in the reduction furnace (5) used for reduction smelting, reduction furnace metal (6), which is an alloy of base metals containing PGM, sinks below the molten slag (7) mainly composed of oxides (CaO-SiO2-Al2O3). At this time, PGM is concentrated in the reduction furnace metal (6) that has settled to the bottom. Thereafter, the molten slag (7), whose base metal content has been reduced to 3.0 mass% or less, is extracted and discharged from the reduction furnace (5) used for reduction smelting.

[0016] That is, in the present invention, the term "reduction furnace metal (6)" refers to a molten metal mainly composed of a copper alloy containing PGM, which is obtained by melting the crushed material (2), the reducing agent (4), the flux (1), and the extractant (3) in a reduction furnace (5) used for reduction smelting, and then extracting and discharging the molten slag (7) that is produced.

[0017] The process described above, in which the crushed material (2) and other materials charged in the reduction furnace (5) used for reduction smelting are melted, the molten slag (7) is extracted, separated and discharged, and the reduction furnace metal (6) is obtained, is the "reduction smelting process", which is similar to the method used in steel smelting, in which iron oxide ore is reduced in a blast furnace to obtain pig iron.

[0018] [2] Oxidation smelting process The reduction furnace metal (6) enriched with PGM obtained in the reduction smelting process is extracted from the reduction furnace (5) used for reduction smelting and transferred in a molten state to the oxidation furnace (9) used for oxidation smelting, where it is oxidized by blowing in air and / or oxygen. The reduction furnace metal (6) then separates into layers: base metal oxide slag (11) mainly composed of oxides of base metals, and PGM alloy (10) in which PGM is further enriched.

[0019] That is, in the present invention, the term "PGM alloy (10)" refers to an alloy material containing base metals and PGM as main components, which is obtained by blowing air and / or oxygen into reduction furnace metal (6) in an oxidation furnace (9) used for oxidation smelting, and then extracting the base metal oxide slag (11) that is produced.

[0020] The base metal oxide slag (11) formed on the surface of the PGM alloy (10) is discharged outside the oxidation furnace (9) used for oxidation smelting, and then air and / or oxygen is blown in again to separate the base metal oxide slag (11) mainly composed of oxides from the PGM alloy (10) in which the PGM is further concentrated. The base metal oxide slag (11) formed on the surface of the PGM alloy (10) is then discharged outside the oxidation furnace (9) again to be used for oxidation smelting.

[0021] The PGM content in the PGM alloy (10) is further concentrated by repeating the above-described oxidation treatment in the oxidation furnace (9) used for oxidation smelting and the treatment of discharging the base metal oxide slag (11).

[0022] The process of obtaining PGM alloy (10) containing concentrated PGMs in the oxidation furnace (9) used for the oxidation smelting described above is the "oxidation smelting process", which is similar to the process in steel smelting in which impurities such as carbon, silicon, and phosphorus are removed by oxidation from pig iron.

[0023] [3] Problems and solutions in the reduction smelting process related to conventional technology Research by the present inventors has revealed that the molten slag generated in the reduction smelting process according to the conventional technology contains PGM alloys. The molten slag generated in the conventional technology is extracted from the reduction furnace (5) used in the reduction smelting and further discharged as waste, while still containing the PGM alloys.

[0024] The inventors of the present invention have conducted research into the recovery of PGM alloys contained in molten slag, which ultimately becomes waste, as a problem in the reduction smelting process according to the prior art. As a result of this research, they have discovered that PGM alloys can be recovered by a simple method of adding base metal oxides to the molten slag generated in the reduction smelting process.

[0025] [4] Reduction smelting process according to the present invention The reduction smelting process according to the present invention is a process in which particles of base metal oxides (21) are added to molten slag (7), which is then melted and reduced, and the PGM alloy remaining in the molten slag (7) is recovered. Below, the process will be described in the order of <1> base metal oxides and <2> a method for adding the base metal oxides, with reference to Figures 1 and 2. However, explanations of parts that overlap with the prior art already described with reference to Figure 3 may be omitted.

[0026] <1> Base metal oxide As the base metal oxide (21) to be added to the molten slag (7), it is preferable to use one or more of the base metal oxides selected from copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide, as described in “[1] Reduction smelting step”. In this case, although it is possible to use a base metal oxide different from that used in the "reduction smelting step (1)", it is advantageous from the viewpoint of PGM recovery described below to use the same base metal oxide as that used in the "reduction smelting step (1)". Since it is preferable to use copper and / or copper oxide in the reduction smelting step, it is preferable to use copper oxide as the base metal oxide added to the molten slag.

[0027] The base metal oxide (21) is preferably in a granular form that is easily dissolved after being added to the molten slag, and the particle size is preferably 1 mm or less, and more preferably 100 μm or less.

[0028] The amount of base metal oxide (21) added is preferably 5% by mass or more and less than 35% by mass based on the mass of the molten slag (7), because adding it in this range can obtain the effect of recovering the PGM alloy, and adding it less than 25% by mass can ensure productivity by preventing the retention time until the precipitation of the base metal oxide (21), which will be described later, from becoming too long.

[0029] Furthermore, the amount of base metal oxide (21) added is preferably 10 times or more and 500 times or less the mass of PGM contained in the molten slag (7). This is because adding 10 times or more the mass of base metal oxide (21) of the PGM can ensure the recovery rate of the PGM alloy suspended in the molten slag (7). On the other hand, if the amount is 500 times or less, it is possible to avoid an excessively long recovery time of the PGM alloy and to avoid an excessively high metal concentration in the slag, which would result in an increase in the loss of the PGM alloy due to the molten slag (25) after the recovery of the recovered metal and the molten slag (26) after the recovery of the PGM alloy. From this viewpoint, it is more preferable that the amount of base metal oxide (21) added is 100 times or more and 300 times or less the mass of PGM contained in the molten slag (7). The amount of PGM alloy contained in the molten slag (7) can be quantitatively analyzed by, for example, ICP analysis.

[0030] <2> Method of adding base metal oxide It is believed that the base metal oxide (21) sediments in the molten slag (7) after it is added, and picks up the remaining PGM alloy. For this reason, it is preferable to hold the base metal oxide (21) for at least two hours after it is added. If the holding time is two hours or more, the sedimentation of the base metal oxide (21) progresses sufficiently, and the state in which the base metal oxide (21) is suspended in the molten slag (7) is completed.

[0031] In order to increase the efficiency of the base metal oxide (21) in capturing the residual PGM alloy in the molten slag (7), it is preferable that the base metal oxide (21) dissolves once in the molten slag (7). Therefore, the temperature of the molten slag (7) after the addition of the base metal oxide (21) is preferably higher than the melting point of the base metal oxide (21) or the eutectic temperature of the slag formed by the furnace slag (7) and the base metal oxide (21). If the base metal oxide (21) does not dissolve in the molten slag (7), it may precipitate or settle without participating in the alloying reaction with the suspended PGM alloy.

[0032] The base metal oxide (21) can be added before and / or after the extraction of the molten slag (7) from the reduction furnace (5) used for reduction smelting. Below, the case of adding the base metal oxide before the extraction of the molten slag will be described in the order of {a} with reference to FIG. 1, and {b} with reference to FIG. 2.

[0033] When base metal oxide is added before extraction of molten slag Before the molten slag (7) in the reduction furnace (5) used for reduction smelting is extracted, base metal oxides (21) can be added to the molten slag (7) from the top of the reduction furnace (5) used for reduction smelting and can be retained in the molten slag (7). The base metal oxides (21) are preferably added over a wide area of ​​the surface of the molten slag (7) in order to increase the efficiency of contact with the PGM alloy remaining in the molten slag (7).

[0034] The base metal oxides (21) are preferably held in the molten slag (7) for at least 2 hours. It is believed that this holding reduces the base metal oxides (21) to form alloys with the PGM alloy, and the resulting grains grow sufficiently to facilitate settling. The alloy of the metals from the settled base metal oxides (21) and the recovered PGM alloy combines with the reduction furnace metal (6). On the other hand, the molten slag (26) after the PGM alloy is recovered becomes waste.

[0035] When base metal oxide is added after extraction of the molten slag When base metal oxides (21) are added after the molten slag (7) is extracted from the reduction furnace (5) used for reduction smelting, a reduction furnace (22) other than the reduction furnace (5) used for reduction smelting is used again to keep the molten slag (7) molten, and the base metal oxides (21) are added thereto and left to stand until they settle. In this way, an alloy layer with the PGM alloy remaining in the molten slag (7) is separated from the molten slag (23) in the reduction furnace and formed as recovered metal (24) at the bottom of the reduction furnace (22), whereby the remaining PGM alloy can be recovered. On the other hand, the molten slag (25) remaining after the recovery of the recovered metal becomes waste.

[0036] The recovered metal (24) may be added to an oxidation furnace (9) used for oxidation smelting to obtain a PGM alloy (10) and further to obtain PGM, or a separate appropriate process may be provided to obtain PGM.

[0037] [5] Oxidation smelting process according to the present invention The distribution ratio of platinum, rhodium, and palladium between the base metal oxide slag (11) and the PGM alloy (10) in the oxidation smelting process according to the present invention is about 100 times larger than the distribution ratio between the molten slag (7) and the reduction furnace metal (6) in the reduction smelting process. Therefore, in the process of concentrating the PGM in the PGM alloy recovered by the base metal oxide and the reduction furnace metal (6), a considerable amount of PGM is distributed into the generated base metal oxide slag (11). In other words, the recovery rate of PGM as the PGM alloy (10) is suppressed.

[0038] Therefore, it is preferable to repeatedly feed the base metal oxide slag (11) to which the considerable amount of PGM has been distributed as the extractant (3) to the subsequent reduction smelting step. With this configuration, the considerable amount of PGM distributed in the base metal oxide slag (11) is circulated within the system between the reduction smelting step and the oxidation smelting step, and as a result, the PGM can be recovered with high efficiency.

[0039] It is also preferable to add oxides (8) during the oxidation smelting process, and to stir the molten reduction furnace metal (6) and then leave it to stand, thereby reducing the distribution of PGM to the base metal oxide slag (11).

[0040] [6] Example of PGM recovery method according to the present invention The PGM recovery process according to the present invention will now be described with reference to an example. The material to be treated (2), which contains PGM such as a ceramic automobile catalyst, the extractant (3) which is a base metal and / or base metal oxide, the flux (1) which is CaO and / or SiO2, and the reducing agent (4) which is a C-containing material such as SiC are loaded into a reduction furnace (5) for reduction smelting and heated. Thereafter, the molten metal, which is an alloy of base metals containing PGM, is allowed to settle below the molten slag (7) which is mainly composed of oxides (CaO-SiO2-Al2O3), to obtain the reduction furnace metal (6) in which the PGM is concentrated in the base metal alloy.

[0041] On the other hand, fine copper oxide powder is dispersed and added as base metal oxide (21) to the entire surface of the molten slag (7) whose base metal content has been reduced to 3.0 mass % or less, and the molten slag (7) is left to stand for about 4 to 10 hours, after which the molten slag (7) is extracted and discharged from the reduction furnace (5) used for the reduction smelting.

[0042] The reduction furnace metal (6) in which PGM is concentrated is extracted and transferred in a molten state to an oxidation furnace (9) for oxidation smelting. When the molten reduction furnace metal (6) is oxidized and smelted, one or more oxides (8) selected from SiO2, CaO, and Na2O can be added. When adding oxides (8) such as SiO2 to the reduction furnace metal (6), it is preferable to add them little by little rather than adding the entire amount at once. This is because if the entire amount of the oxides (8) to be added is added to the reduction furnace metal (6) at once, the solution temperature of the molten reduction furnace metal (6) will drop and the added oxides (8) will not be able to dissolve. Therefore, the time for adding the oxides (8) depends on the amount of the molten reduction furnace metal (6), but it is preferable to add them over a period of 20 minutes or more.

[0043] After the oxide (8) is added, the reduction furnace metal (6) is stirred to dissolve the oxide (8). The preferred method for stirring the solution is aeration with air and / or oxygen.

[0044] After the oxides (8) have melted, the solution is left to stand. At this time, it is estimated that the temperature near the center of the molten material in the oxidation furnace (9) used for oxidation smelting is 1200 to 1500°C. The material is then separated into a base metal oxide slag (11) mainly made of oxides and a PGM alloy (10) in which the PGM is further concentrated, to obtain the PGM alloy (10). The PGM is obtained from the obtained PGM alloy (10) by an appropriate recovery method (mainly a wet method). EXAMPLES

[0045] Example 1 The reagents Al2O3 and SiO2, and CaO obtained by calcining CaCO3 reagent were prepared. These were then weighed and mixed to give 35% Al2O3, 30% CaO, and 35% SiO2 by mass. 200g of slag prepared by the dry method was inserted into an MgO crucible together with 125g of rod-shaped graphite (62.8g after 12 hours). The sample was kept molten at 1450°C. Then, 100g of 35% Al2O3-30% CaO-35% SiO2 by mass and 0.3g of Pt powder with a particle size of 0.4-0.8μm were added to the slag kept at 1450°C and kept for another 3 hours, to obtain a slag that imitates the molten slag obtained in the above-mentioned PGM recovery method example.

[0046] Next, 33.78 g of Cu2O (containing 30 g of Cu in terms of metallic Cu) was added as a base metal oxide to the slag while continuing to heat at 1450°C. The particle size of the added Cu2O was 53 μm or less. After the addition of the base metal oxide, heating was continued at 1450°C, and about 1 g of molten slag samples were sampled by suction and water-cooled every 0.5, 1, 2, 3, 4, 6, 8, and 12 hours. However, after 12 hours, the molten slag sample was water-cooled together with the MgO crucible, and a sample was taken. The molten slag sample was sampled by suction using a mullite tube and a syringe from near the center of the thickness direction of the molten slag layer.

[0047] The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pt concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted in the graph of Figure 4 with -▲-. The graph in Figure 4 is a semi-logarithmic graph with the vertical axis representing the logarithm of the Pt concentration (ppm) in the molten slag sample after separation of the recovered metal (metallic copper) and the horizontal axis representing the sampling time after the addition of base metal oxide. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. The recovery rate of PGM after water cooling in this example is shown in Table 2. The recovery rate was calculated using the following formula. JPEG0007595305000001.jpg13170 where R is the recovery rate (%), m m is the mass of the alloy phase (g), m s is the mass of the slag phase (g), x m is the PGM concentration in the alloy phase (mass%), x s represents the PGM concentration (mass%) in the slag phase. Slag is composed of the components AlO 3、 In addition to CaO and SiO2, it contains MgO, which is a crucible component, Cu2O derived from the extractant, and suspended metal particles. In addition, the slag mass is reduced by about 8 g in total due to the sampling at each retention time, but it is assumed that the effect of these on the slag mass is small, and the mass of the slag phase m s is molten AlO 3、 The calculation was based on the mass of CaO and SiO2 of 300g.

[0048] Example 2 The same operation as in Example 1 was carried out, except that 67.56 g of Cu2O powder (containing 60 g of Cu in terms of metallic Cu) was added to the molten slag sample as a base metal oxide. The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pt concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted as . . . ▼ . . . in the graph in Figure 4. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. Table 2 shows the recovery rate of PGM after water cooling in this example.

[0049] Comparative Example 1 The same operation as in Example 1 was carried out, except that 30 g of Cu powder (particle size 53 μm or less) was added to the molten slag sample instead of the base metal oxide. The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pt concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted in the graph of Figure 4 with -●-. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. Table 2 also shows the recovery rate of PGM after water cooling in this comparative example.

[0050] Comparative Example 2 The same procedure as in Example 1 was carried out, except that no Cu2O powder was added to the molten slag sample. The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pt concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted in the graph of Figure 4 with -◆-. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. Table 2 also shows the recovery rate of PGM after water cooling in this comparative example.

[0051] Example 3 The same procedure as in Example 1 was carried out, except that Pd powder was used instead of Pt powder when preparing molten slag simulating the molten slag obtained in the above-mentioned PGM recovery method example. The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pd concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted as ...△... in the graph in Figure 4. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. Table 2 shows the recovery rate of PGM after water cooling in this example.

[0052] Comparative Example 3 The same procedure as in Comparative Example 1 was carried out, except that Pd powder was used instead of Pt powder when preparing molten slag simulating the molten slag obtained in the above-mentioned PGM recovery method example. The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pd concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted as ··· ◯··· in the graph in Figure 4. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. Table 2 also shows the recovery rate of PGM after water cooling in this comparative example.

[0053] Comparative Example 4 The same procedure as in Comparative Example 2 was carried out, except that Pd powder was used instead of Pt powder when preparing molten slag simulating the molten slag obtained in the above-mentioned PGM recovery method example. The recovered metal (metallic copper) was separated from each of the recovered molten slag samples. The Pd concentration in the molten slag samples after separation of the recovered metal (metallic copper) was then measured. The results are plotted as ···◇··· in the graph in Figure 4. Table 1 also shows the results of the compositional analysis of the recovered metal (metallic copper) measured by ICP. Table 2 also shows the recovery rate of PGM after water cooling in this comparative example.

[0054] (summary) In Examples 1 to 3, in which Cu2O was added as a base metal oxide to the molten slag sample, the Pt or Pd concentration in the molten slag sample significantly decreased over time, confirming that Pt or Pd was recovered. The recovery of Pt or Pd was also confirmed by the fact that the Pt or Pd concentration was high in the analysis results of the recovered metal. In contrast, in Comparative Example 1, in which Cu was added as a base metal to the molten slag sample, the Pt or Pd concentration was slightly reduced, and in Comparative Example 2, in which nothing was added, the Pt or Pd concentration was hardly reduced, and it was confirmed that the recovery of Pt hardly progressed. The slow progress of the recovery of Pt was also confirmed by the low Pt or Pd concentration in the analysis results of the recovered metal.

[0055] [Table 1] [Table 2] [Explanation of symbols]

[0056] (1) Flux (2) Material to be treated (3) Extractant (4) Reducing agent (5) Reduction furnace used for reduction smelting (6) Reduction furnace metal (7) Molten slag (8) Oxide (9) Oxidation furnace for oxidizing smelting (10)PGM alloy (11) Base metal oxide slag (21) Base metal oxides (22) Reduction furnace (23) Molten slag in the reduction furnace (24) Recovered metal (25) Molten slag after recovery of recovered metals (26) Molten slag after PGM alloy recovery

Claims

1. a reduction smelting process in which a PGM-containing workpiece, a base metal and / or a base metal oxide, a flux, and a reducing agent are placed in a reduction furnace used for reduction smelting, heated, and melted to form molten slag and reduction furnace metal; extracting the molten slag from the reduction furnace to obtain reduction furnace metal containing PGM; a step of transferring the reduction furnace metal to an oxidation furnace used for oxidation smelting, oxidizing and melting the metal to form a slag of base metal oxides and a PGM alloy, and then extracting the base metal oxide slag to obtain a PGM alloy enriched in PGM; A method for recovering PGM, characterized in that at least one base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide is added to the molten slag from the top of the reduction furnace, or to the molten slag maintained in a molten state using a reduction furnace separate from the reduction furnace, before the molten slag is extracted from the reduction furnace, and the PGM alloy contained in the molten slag is recovered by allowing it to settle in the molten slag.

2. 2. The method for recovering PGM according to claim 1, characterized in that less than 35% by mass of the base metal oxide is added relative to the mass of the molten slag.

3. A method for recovering PGM as described in claim 1 or 2, characterized in that at least one base metal oxide selected from the group consisting of copper oxide, iron oxide, tin oxide, nickel oxide and lead oxide is added to the molten slag, and a holding time of at least two hours is set when recovering the PGM alloy contained in the molten slag.

4. 4. A method for recovering PGM according to claim 1, wherein the base metal oxide is added in an amount between 10 and 500 times the mass of the PGM contained in the molten slag.

Citation Information

Patent Citations

  • Device for recovering platinum group element

    JP2009024263A

  • Method for treating material to be treated, containing platinum group element, rhenium and / or arsenic

    JP2010077470A

  • Method for recovering platinum group element

    WO2004081243A1

  • Method for recovering pgm

    WO2012099009A1

  • Method for recovering PGM from member to be processed that contains pgm