Cement foaming agent suitable for carbon dioxide foaming, preparation method therefor and preparation device
By combining carbon dioxide foaming technology with magnesium oxide materials, the traditional air foaming technology solves the insufficient strength and environmental protection problems of magnesium oxide materials, realizes the preparation of efficient, low-carbon foam lightweight soil, and meets the sustainable development needs of modern engineering. .
Patent Information
- Application Number
- PCT/CN2023/125599
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-10-20
- Publication Date
- 2024-10-03
AI Technical Summary
Traditional air foaming technology cannot effectively improve the strength of foamed lightweight soil when using magnesium oxide materials, and the preparation process consumes a lot of energy, causes serious pollution, and has low carbon dioxide capture efficiency, making it difficult to meet the environmental protection and sustainable development needs of modern engineering construction. .
Carbon dioxide foaming technology is used to replace air with CO2 gas and combine with magnesium oxide materials to achieve carbonization reaction and generate stronger carbonization products. Carbon dioxide foam lightweight soil is prepared through specific devices and methods to achieve the storage and resource utilization of carbon dioxide. use.
It improves the thermal insulation and mechanical properties of foamed lightweight soil, achieves low-carbon and environmentally friendly construction efficiency, meets the sustainable development needs of modern engineering construction, and can be prepared in a short time, which is energy-saving and environmentally friendly.
Smart Images

Figure CN2023125599_03102024_PF_FP_ABST
Abstract
Description
A cement foaming agent suitable for carbon dioxide foaming and its preparation method and device Technical Field
[0001] The invention belongs to the technical field of civil engineering materials, and relates to a cement foaming agent suitable for carbon dioxide foaming, a foaming device and a preparation method thereof. Background Art
[0002] Traditional air foaming technology is to use a physical, chemical or biological foaming agent to absorb air using an air compressor, and pressurize the mixed air and foaming liquid for foaming to generate microbubble groups. Because it can form closed bubble pores to a certain extent and has a certain support, it is often used to be mixed into the soil, and some curing agents (cement-based binders, etc.), admixtures, etc. are added. It is fully stirred according to a specific proportion and condensed into an inorganic synthetic material - foam lightweight soil through a series of physical and chemical reactions. It has the advantages of strong adjustable bulk density, strong adjustable strength, high fluidity, good thermal insulation and sound insulation, and good anti-freeze and thaw properties. In recent years, it has been widely used in bridge abutment backfill, road widening, bridge span reduction, steep slope embankment, landslide roadbed, soft soil roadbed load reduction, underground structure load reduction and other projects. Among them, foaming technology is an important factor that determines the strength and stability of bubble-mixed lightweight soil. However, traditional foaming technology mostly uses air as the foam matrix and cement as the gelling material, which consumes a lot of energy and is prone to pollution. The preparation method is not environmentally friendly and economical. In addition, the strength of the foamed lightweight soil made by mixing it into cement soil increases slowly and the curing time is long. Therefore, it has certain limitations in actual engineering applications.
[0003] In addition, based on the characteristics of magnesium oxide cement, such as low calcination temperature, large amount of carbon dioxide absorption during carbonization, high strength and good durability, the applicant proposed to replace cement with magnesium oxide as a cementitious material in lightweight soil. Experiments have shown that its physical and mechanical properties can reach the same order of magnitude as traditional cement soil. However, since the strength cannot be significantly improved when traditional air foaming technology is applied to magnesium oxide-foam lightweight soil, adding carbon dioxide during the foaming process can greatly promote the carbonization reaction of magnesium oxide-foam lightweight soil and achieve a considerable amount of carbon sequestration. The present invention proposes a new type of cement foaming agent suitable for carbon dioxide foaming, its device and preparation method, and a method of using carbon dioxide gas instead of air as the foaming raw material. Carbon dioxide is injected into the lightweight soil through carbon dioxide foaming, which can capture carbon dioxide and achieve effective sequestration of carbon dioxide, and can also utilize the pore characteristics of the foam to reduce the consumption of raw materials and enhance the thermal insulation and mechanical properties of the foam lightweight soil. Summary of the Invention
[0004] Technical problem to be solved: The present invention discloses a cement foaming agent, a foaming device and a preparation method suitable for carbon dioxide foaming. The formula uses CO2 instead of air for physical foaming. Compared with traditional air foaming technology, it has the characteristics of high construction efficiency, reliable quality and low carbon and environmental protection, and meets the needs of carbon dioxide resource utilization, which is in line with the development trend of green construction in civil engineering.
[0005] Technical solution: A preparation device suitable for carbon dioxide foaming, including a CO2 cylinder, a foaming liquid storage tank, a foaming machine housing, a foam storage tank, a pressure regulating valve, a CO2 inlet pipe, a liquid inlet pipe, a bubble outlet pipe, a one-way valve, a pressurization chamber, an airway, a water pump speed regulating knob, and a digital display screen; the pressure regulating valve is arranged on the CO2 cylinder to control the introduction pressure of the CO2 gas, and the CO2 cylinder and the one-way valve are connected by the CO2 inlet pipe; the foaming liquid storage tank is connected to the foaming machine housing through the liquid inlet pipe; the one-way valve and the pressurization chamber are arranged in the foaming machine housing, and the water pump speed regulating knob is arranged on the foaming machine housing to adjust the suction rate of the foaming liquid; the inlet of the one-way valve is connected to the CO2 inlet pipe, and the outlet is connected to the airway; when the one-way valve is opened, CO2 enters from the CO2 inlet pipe, flows to the airway, and enters the pressurization chamber; the pressurization chamber and the foam storage tank are connected by the bubble outlet pipe.
[0006] The method for preparing carbon dioxide foam using the above-mentioned device includes the following steps: S1, preparing a foaming liquid: mixing a foaming agent and an aqueous solution in a volume ratio of 1:30 to 1:50, stirring evenly, and extending a liquid inlet pipe into a foaming liquid storage tank; S2, opening a valve: opening a one-way valve and introducing CO2; S3, starting a water pump: starting a foaming machine, turning on a water pump, and adjusting the water pump speed using a water pump speed control knob, and starting an air compressor after the foaming liquid completely enters the liquid inlet pipe; S4, preparing foam: opening a CO2 gas cylinder, allowing CO2 to continuously enter the pipeline, starting foaming, and allowing the prepared foam to enter the foam storage tank.
[0007] The ratio of the above-mentioned foaming agent to water is controlled at 1:40. When preparing the foaming liquid, water is added first and then the foaming agent.
[0008] The speed of the above-mentioned water pump is controlled at 80~100, and the corresponding flow rate on the digital display screen is 4L / min~5L / min.
[0009] In the above step S4, the CO2 cylinder is opened and the ventilation pressure of CO2 is controlled between 0.3 and 0.5 MPa by the pressure regulating valve.
[0010] The cement foaming agent prepared by the above method.
[0011] The cement foaming agent is classified into at least one of rosin resin, synthetic surfactant, protein and composite foaming agents according to the composition.
[0012] The foaming agent contains magnesium acetate.
[0013] Beneficial effects: (1) CO2 foaming replaces traditional air foaming, and a large amount of greenhouse gas carbon dioxide is used in the process, which provides a new idea for reducing carbon emissions. Compared with the foamed lightweight soil produced by traditional air foaming, it can be prepared in a short time, and has the characteristics of energy saving, environmental protection, low carbon and high efficiency. It can be directly used in soil reinforcement, roadbed load reduction, etc., and can achieve CO2 fixation and storage, meeting the requirements of sustainable development for modern engineering construction.
[0014] (2) The cementitious material added to the foamed lightweight soil prepared by traditional air foaming is generally cement. The CO2 foaming method adopted in the present invention can be combined with magnesium oxide materials. The CO2 in the foam can further react with MgO to generate a carbonized product with higher strength and good integrity. In addition, the magnesium oxide-carbonized foamed lightweight soil material prepared by carbon dioxide foaming has a uniform and fine skeleton structure, a high foaming ratio, and good physical and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] FIG1 is a preparation device suitable for carbon dioxide foaming according to the present invention.
[0016] FIG2 is a schematic diagram of the method for preparing carbon dioxide foam according to the present invention.
[0017] In the figure, 1-CO2 gas cylinder, 2-foaming liquid storage tank, 3-foaming machine chassis, 4-foam storage tank, 5-pressure regulating valve, 6-CO2 air inlet pipe, 7-foaming liquid injection pipe, 8-bubble outlet pipe, 9-check valve, 10-pressurization chamber, 11-air duct, 12-water pump speed control knob, 13-digital display screen.
[0018] FIG3 is a picture of the CO2 foam obtained in Example 1. FIG1 is a picture of the CO2 foam obtained in Example 1.
[0019] FIG4 is a picture of the cured magnesium oxide-foam lightweight soil test block in Example 6. DETAILED DESCRIPTION Example 1
[0020] 10. The preparation device for carbon dioxide foaming comprises a CO2 cylinder 1, a foaming liquid storage tank 2, a foaming machine housing 3, a foam storage tank 4, a pressure regulating valve 5, a CO2 air inlet pipe 6, a liquid inlet pipe 7, a foaming pipe 8, a one-way valve 9, a pressurizing chamber 10, an airway 11, a water pump speed regulating knob 12, and a digital display screen 13; the pressure regulating valve 5 is arranged on the CO2 cylinder 1 for controlling the pressure of the CO2 gas introduced, and the CO2 cylinder 1 and the one-way valve 9 are connected by the CO2 air inlet pipe 6; the foaming liquid storage tank 2 is connected to the foaming machine housing 3 through the liquid inlet pipe 7; the one-way valve 9 and the pressurizing chamber 10 are arranged in the foaming machine housing 3, and the water pump speed regulating knob 12 is arranged on the foaming machine housing 3 for adjusting the suction rate of the foaming liquid; the inlet of the one-way valve 9 is connected to the CO2 air inlet pipe 6, and the outlet is connected to the airway 11; when the one-way valve 9 is opened, CO2 enters through the CO2 inlet pipe 6, flows to the airway 11, and enters the pressurized chamber 10; the pressurized chamber 10 is connected to the foam storage tank 4 by the bubble outlet pipe 8.
[0021] The method for preparing carbon dioxide foam by the above-mentioned device includes the following steps: S1, preparing foaming liquid: mixing the foaming agent and the aqueous solution in a volume ratio of 1:30~1:50, stirring evenly, and extending the liquid inlet pipe 7 into the foaming liquid storage tank 2; S2, opening the valve: opening the one-way valve 9 and introducing CO2; S3, starting the water pump: starting the foaming machine, turning on the water pump, and adjusting the water pump speed through the water pump speed knob 12, the speed is controlled at 80~100, and the digital display screen 13 corresponds to a flow rate of 4L / min~5L / min. After the foaming liquid completely enters the liquid inlet pipe 7, the air compressor is started; S4, preparing foam: opening the CO2 gas cylinder, allowing CO2 to continuously enter the pipeline, controlling the CO2 ventilation pressure between 0.3~0.5Mpa through the pressure regulating valve 5 to start foaming, and the prepared foam enters the foam storage tank 4.
[0022] Specifically, the carbon dioxide foam of this embodiment is made by adjusting the following foaming device parameters and foaming agent dilution ratio: foaming agent dilution ratio 1:40, water pump speed 80, corresponding to a flow rate of 4 L / min, and CO2 ventilation pressure set to 0.3 MPa.
[0023] The carbon dioxide foam was prepared using the following steps:
[0024] S1. Preparation of foaming liquid: Mix the foaming agent and the aqueous solution in a ratio of 1:40. When preparing the foaming liquid, first add water and then add the foaming agent, stir evenly, place it in the foaming liquid storage tank 2, and extend the liquid inlet pipe 7 into the foaming liquid storage tank 2 to absorb the foaming liquid;
[0025] S2. Start the water pump: Start the foaming machine, turn on the water pump, and control the water pump speed to 80 through the water pump speed knob 12, corresponding to a flow rate of 4L / min. After the foaming liquid completely enters the liquid inlet pipe 7, start the air compressor;
[0026] S3. Prepare foam: Open the CO2 cylinder, adjust the pressure regulating valve 5 so that the ventilation pressure of CO2 is 0.3 MPa, and continue to introduce CO2 into the pipeline to start foaming. The prepared foam is collected in the foam storage tank 4. Example 2
[0027] The carbon dioxide foam of this example was produced by adjusting the following foaming apparatus parameters and foaming agent dilution ratio: a foaming agent dilution ratio of 1:40, a water pump speed of 90°, corresponding to a flow rate of 4.5 L / min, and a CO2 aeration pressure of 0.3 MPa. The same apparatus and foaming agent as in Example 1 were used, and the carbon dioxide foam in Example 2 was produced using the same method as in Example 1. Example 3
[0028] The carbon dioxide foam of this example was produced by adjusting the following foaming apparatus parameters and foaming agent dilution ratio: a foaming agent dilution ratio of 1:40, a water pump speed of 100, corresponding to a flow rate of 5 L / min, and a CO2 ventilation pressure of 0.3 MPa. The same apparatus and foaming agent as in Example 1 were used, and the carbon dioxide foam in Example 2 was produced using the same method as in Example 1. Example 4
[0029] The carbon dioxide foam of this example was produced by adjusting the following foaming apparatus parameters and foaming agent dilution ratio: a foaming agent dilution ratio of 1:40, a water pump speed of 80, corresponding to a flow rate of 4 L / min, and a CO2 aeration pressure of 0.4 MPa. The same apparatus and foaming agent as in Example 1 were used, and the carbon dioxide foam in Example 2 was produced using the same method as in Example 1. Example 5
[0030] The carbon dioxide foam of this example was produced by adjusting the following foaming apparatus parameters and foaming agent dilution ratio: a foaming agent dilution ratio of 1:40, a water pump speed of 80, corresponding to a flow rate of 4 L / min, and a CO2 aeration pressure of 0.5 MPa. The same apparatus and foaming agent as in Example 1 were used, and the carbon dioxide foam in Example 2 was produced using the same method as in Example 1. Example 6
[0031] A carbonized foamed lightweight soil. Each cubic meter of the carbonized foamed lightweight soil contains: 100 parts activated magnesium oxide powder, 100 parts silty clay, 60 parts CO2 foam, and 160 parts water. The silty clay needs to be air-dried, then crushed and passed through a 2mm sieve. The water used is distilled water.
[0032] The carbonized foamed lightweight soil was prepared by the following steps:
[0033] S1. Raw material preparation: weigh 100 parts of activated magnesium oxide powder and 100 parts of silty clay and set aside;
[0034] S2. Slurry preparation: Magnesium oxide and silty clay are added into a stirring device according to a certain proportion, and stirred at a speed of about 100 r / min for 2 minutes to mix the magnesium oxide and silty clay evenly;
[0035] S3, CO2 foam preparation: Mix the foaming agent with water at a dilution ratio of 40 times to obtain a foaming liquid, then turn on the water pump and adjust the pump speed to 80 to absorb the foaming liquid for 10-15 seconds, open the CO2 vent valve and adjust the pressure to 0.4 MPa to release fine and stable CO2 foam, and collect the prepared foam in the foam storage tank 4;
[0036] S4. Mixing and stirring: Immediately after obtaining the foam (within 10 minutes), add 60 parts of CO2 foam to the above mixture and continue stirring at a constant speed of 30 r / min for 10 minutes to ensure that the CO2 foam is evenly distributed, the foam is not broken, and there is no sedimentation in the slurry, thus obtaining a mixed mixture;
[0037] S5. Sample Preparation and Curing: Immediately cast the mixed material into a mold and cure it in a carbonization chamber for 48 hours. The carbonization process further strengthens the lightweight soil, resulting in a magnesium oxide-carbonized foam lightweight soil specimen. Sample preparation from steps S4 to S5 must be completed within the half-life of the foaming agent to prevent foam rupture and CO2 leakage. Example 7
[0038] A carbonized foamed lightweight soil, wherein each cubic meter of the carbonized foamed lightweight soil contains: 100 parts of activated magnesium oxide powder, 100 parts of silty clay, 70 parts of CO2 foam, and 160 parts of water. The silty clay, magnesium oxide, water, and foaming agent are the same as those in Example 6, and the processing methods for each material are also consistent. Example 8
[0039] A carbonized foamed lightweight soil, wherein each cubic meter of the carbonized foamed lightweight soil contains: 100 parts of activated magnesium oxide powder, 100 parts of silty clay, 80 parts of CO2 foam, and 160 parts of water. The silty clay, magnesium oxide, water, and foaming agent are the same as those in Example 6, and the processing methods for each material are also consistent. Example 9
[0040] A carbonized foamed lightweight soil, wherein each cubic meter of the carbonized foamed lightweight soil contains: 80 parts of activated magnesium oxide powder, 100 parts of silty clay, 90 parts of CO2 foam, and 160 parts of water. The silty clay, magnesium oxide, water, and foaming agent are the same as those in Example 6, and the processing methods for each material are also consistent. Example 10
[0041] A carbonized foamed lightweight soil, wherein each cubic meter of the carbonized foamed lightweight soil contains: 100 parts cement, 100 parts silty clay, 80 parts CO2 foam, and 160 parts water. The same silty clay, magnesium oxide, water, and foaming agent as in Example 6 are used, and the processing methods for each material are also consistent.
[0042] Test and Inspection
[0043] The carbon dioxide foams prepared in Examples 1 to 5 were tested for foam density, 1-hour settlement distance / mm, and total water seepage. The tests were conducted in accordance with the specification "CECS 249-2008 Technical Specification for Cast-in-Place Foam Lightweight Soil".
[0044] The carbonized foam lightweight soil samples prepared in Examples 6 and 7 were tested for 7-day unconfined compressive strength and wet bulk density. The unconfined compressive strength test was conducted in accordance with the "Highway Geotechnical Test Code JTG E40-2007" using a CBR-2 bearing ratio tester. The wet bulk density test was conducted in accordance with the "CECS 249-2008 Technical Code for Cast-in-situ Foam Lightweight Soil"
[0045] Test results
[0046] Table 1 Foam density, 1h settling distance and total water exudation of carbon dioxide foam
[0047]
[0048] Table 2 Properties of magnesium oxide-carbonized foam lightweight soil
[0049]
[0050] As can be seen from Tables 1 and 2, the carbon dioxide foam provided by the present invention has good foaming properties and can be combined with magnesium oxide and soil to form magnesium oxide-carbonized foamed lightweight soil. Compared with the foamed lightweight soil formed by combining carbon dioxide foam with traditional cement, the strength is greatly improved.
[0051] The present invention will be further described below with reference to the accompanying drawings.
[0052] As shown in Figure 1, a preparation device suitable for carbon dioxide foaming of the present invention includes a CO2 gas cylinder 1, a foaming liquid storage tank 2, a foaming machine box 3, a foam storage tank 4, a pressure regulating valve 5, a CO2 air inlet pipe 6, a liquid inlet pipe 7, a foaming pipe 8, a one-way valve 9, a pressurizing chamber 10, an air duct 11, and a water pump speed control knob 12;
[0053] The CO2 cylinder 1 is provided with a pressure regulating valve 5 for controlling the inlet pressure of the CO2 gas. The CO2 cylinder 1 and the one-way valve 9 are connected by a CO2 inlet pipe 6.
[0054] The foaming liquid storage tank 2 is connected to the box body through the liquid inlet pipe 7; the pressurizing chamber 10 is connected to the foam storage tank 4 by the bubble outlet pipe 8, and the foam storage tank 4 is used to receive the prepared CO2 bubbles;
[0055] The foaming machine housing 3 includes a one-way valve 9 and a foam storage tank 4. The foaming machine housing 3 is provided with a water pump speed control knob 12 for adjusting the suction rate of the foaming liquid;
[0056] The first inlet of the one-way valve 9 is connected to the CO2 inlet pipe 6, and the second inlet is connected to the airway 11; when the one-way valve 9 is opened, CO2 enters from the CO2 inlet pipe 6, flows to the airway 11, and enters the pressurized chamber;
[0057] The pressurizing chamber 10 is connected to the foam storage tank 4 via a foam outlet pipe 8 .
[0058] As shown in FIG2 , a method for preparing carbon dioxide foam using the above-mentioned device suitable for carbon dioxide foaming comprises the following steps:
[0059] S1. Weighing the solvent: Use an electronic scale to weigh a certain amount of foaming agent and water, with a volume ratio of 1:40;
[0060] S2. Prepare the foaming liquid: first add the weighed water to the foaming liquid storage tank 2, then add the weighed foaming agent, mix them thoroughly, let them stand for use, and extend the liquid inlet pipe 7 into the foaming storage tank 2 to absorb the foaming liquid;
[0061] S3. Start the water pump: Start the foaming machine, turn on the water pump, and adjust the water pump speed to 80~100 (flow rate is 4L / min~5L / min). Wait for about 10~15 seconds. When the foaming liquid completely enters the liquid inlet pipe 7, turn on the air compressor and the machine starts to operate to absorb gas;
[0062] S4. Prepare foam: Open the CO2 gas cylinder 2, adjust the pressure regulating valve 5 to control the CO2 ventilation pressure to 0.3MPa~0.5MPa, at this time, the output end of the bubble tube 8 begins to release fine CO2 foam, and when the bubbles are observed to be uniform and dense and no "big bubbles" appear, the foam can be collected by the foam storage tank 4. After the foam fills the foam storage tank 4, stop the preparation and obtain the CO2 bubbles for subsequent use.
[0063] Finally, the method of this application is only a preferred embodiment and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A preparation device suitable for carbon dioxide foaming, characterized in that: The invention comprises a CO2 gas cylinder (1), a foaming liquid storage tank (2), a foaming machine housing (3), a foam storage tank (4), a pressure regulating valve (5), a CO2 air inlet pipe (6), a liquid inlet pipe (7), a foam outlet pipe (8), a one-way valve (9), a pressurizing chamber (10), an airway (11), a water pump speed regulating knob (12), and a digital display screen (13); the pressure regulating valve (5) is arranged on the CO2 gas cylinder (1) and is used to control the inlet pressure of the CO2 gas; the CO2 gas cylinder (1) and the one-way valve (9) are connected to each other. ) are connected by a CO2 inlet pipe (6); the foaming liquid storage tank (2) is connected to the foaming machine housing (3) through a liquid inlet pipe (7); the one-way valve (9) and the pressurizing chamber (10) are arranged in the foaming machine housing (3), and a water pump speed regulating knob (12) is arranged on the foaming machine housing (3) for adjusting the suction rate of the foaming liquid; the inlet of the one-way valve (9) is connected to the CO2 inlet pipe (6), and the outlet is connected to the airway (11); when the one-way valve (9) is opened, CO2 enters through the CO2 inlet pipe (6), flows to the airway (11), and enters the pressurizing chamber (10); the pressurizing chamber (10) and the foam storage tank (4) are connected by a bubble outlet pipe (8).
2. The method for preparing carbon dioxide foam using the device according to claim 1, characterized in that: The following steps are involved: S1. Preparation of foaming liquid: Mix the foaming agent and the aqueous solution in a volume ratio of 1:30 to 1:50, stir evenly, and extend the liquid inlet pipe (7) into the foaming liquid storage tank (2); S2. Open the valve: Open the one-way valve (9) and introduce CO2; S3. Start the water pump: Start the foaming machine, turn on the water pump, and adjust the water pump speed through the water pump speed knob (12). After the foaming liquid completely enters the liquid inlet pipe (7), start the air compressor; S4, preparing foam: opening the CO2 gas cylinder, allowing CO2 to continuously flow into the pipeline, starting to make foam, and the prepared foam enters the foam storage tank (4).
3. The method according to claim 2, characterized in that The ratio of the foaming agent to water is controlled at 1:
40. When preparing the foaming liquid, water is added first and then the foaming agent.
4. The method according to claim 2, characterized in that: The water pump speed is controlled at 80-100, and the corresponding flow rate on the digital display screen (13) is 4L / min-5L / min.
5. The method according to claim 2, characterized in that: In step S4, the CO2 gas cylinder is opened, and the ventilation pressure of CO2 is controlled to be between 0.3 and 0.5 MPa by the pressure regulating valve (5).
6. A cement foaming agent obtained by the method according to any one of claims 2 to 5.
7. The cement foaming agent according to claim 6, characterized in that The foaming agent is classified into at least one of rosin resin, synthetic surfactant, protein and composite foaming agents according to its components.
8. The cement foaming agent according to claim 6, characterized in that The foaming agent contains magnesium acetate.
Citation Information
Patent Citations
Foam concrete foaming machine with automatic control system
CN103128852A
Foam concrete foaming machine and foaming method thereof
CN103302725A
Light CO2 foamed cement-based material based on carbonization and optimized preparation method and application thereof
CN113277787A
Carbonized foam light soil and preparation method thereof
CN113968711A
Cement foaming agent suitable for carbon dioxide foaming and preparation method and device thereof
CN116354742A
Cited By
CO2 foam cement mortar material and soft rock reinforcing method and system
CN119528540A