Preparation method for cast-rolled aluminum plate, and cast-rolled aluminum plate and vehicle
By properly proportioning Mg, Mn, Si and other elements and performing heat treatment, the Mg2Si strengthening phase is formed, which solves the problems of insufficient yield strength and stamping cracking of cast-rolled aluminum alloys, improves the performance of cast-rolled aluminum plates, and is suitable for high-end passenger vehicles automotive field.
Patent Information
- Application Number
- PCT/CN2024/084783
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing cast-rolled aluminum alloys are difficult to meet the working conditions in the field of high-end passenger cars in terms of yield strength and stamping forming, resulting in insufficient yield strength and cracking during stamping.
By rationally proportioning Mg, Mn, Si and other alloying elements in the cast-rolled aluminum plate, the Mg2Si strengthening phase is formed, and combined with the heat treatment process, the recrystallization temperature and grain uniformity of the aluminum alloy are increased, and the yield strength and formability of the cast-rolled aluminum plate are improved. performance.
It significantly improves the tensile strength, yield strength and elongation of cast-rolled aluminum plates, meets the mechanical performance requirements in the field of high-end passenger cars, and improves the situation of insufficient yield strength and stamping forming cracking.
Smart Images

Figure PCTCN2024084783-FTAPPB-I100001
Abstract
Description
Method for preparing cast-rolled aluminum plate, cast-rolled aluminum plate and vehicle
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure is based on and claims the priority of Chinese patent application with application number 202310323672.5 and application date March 29, 2023. The entire content of the Chinese patent application is hereby incorporated into this disclosure by reference. Technical Field
[0003] The present disclosure relates to the technical field of aluminum alloy preparation, and in particular to a method for preparing a cast-rolled aluminum plate, a cast-rolled aluminum plate, and a vehicle. Background Art
[0004] Energy conservation and emission reduction have become global priorities, and lightweighting is a key approach. For example, for every 100kg reduction in vehicle mass, fuel consumption per 100km decreases by 0.3-0.6L. Therefore, lightweighting has become a growing trend. Aluminum alloys, due to their lightweight advantages, have attracted widespread attention.
[0005] As demand for aluminum alloys in automotive applications increases, higher requirements are being placed on their performance and operating environment. Currently, cast-rolled aluminum sheet is primarily used in building curtain walls, truck flooring, and various foils, where mechanical and stamping properties are not critical. It has yet to find practical use in the high-end passenger vehicle market. Existing cast-rolled aluminum alloy grades, in terms of yield strength and stamping formability, struggle to meet these requirements, necessitating improvements to the aluminum alloys used in related technologies.
[0006] Summary of the Invention
[0007] The embodiments of the present disclosure provide a method for preparing a cast-rolled aluminum plate, a cast-rolled aluminum plate, and a vehicle, which can improve the situation of insufficient yield strength and cracking due to stamping.
[0008] In a first aspect, an embodiment of the present disclosure provides a method for manufacturing a cast-rolled aluminum plate, comprising the following steps:
[0009] A cast ingot is provided, which includes the following components in percentage by mass: Si: 0.1%-0.5%; Mn: 0.5%-1.5%; Mg: 0.06%-0.7%; wherein Si+Mn<1.6%, 0.2%≤Si+Mg≤0.5%, and the ratio of Mg to Si is: 0.55-2; the cast ingot is annealed and cold rolled to obtain a cast-rolled aluminum plate, which includes Mg2Si.
[0010] According to an embodiment of the first aspect of the present disclosure, the ingot also includes the following components in percentage by mass: Fe: 0.1%-0.7%, Cu: 0-0.15%, Ti<0.1%, and other unavoidable impurities, with a single impurity ≤0.03%, a total impurity amount ≤0.15%, and the balance being Al.
[0011] According to an embodiment of the first aspect of the present disclosure, the steps of annealing and cold rolling the ingot include: subjecting the ingot to a first annealing treatment and a second annealing treatment, with at least one cold rolling treatment between the first annealing treatment and the second annealing treatment; the process parameters of the first annealing treatment are: annealing at 500°C-600°C for 10h-20h; the process parameters of the second annealing treatment are: annealing at 240°C-450°C for 2h-8h.
[0012] According to an embodiment of the first aspect of the present disclosure, the step of annealing and cold rolling the cast billet includes: before the cast billet is subjected to the first annealing treatment, the step also includes performing at least one pass of cold rolling on the cast billet.
[0013] According to an embodiment of the first aspect of the present disclosure, after the cast billet is subjected to the second annealing treatment, the cast billet is further subjected to at least one cold rolling treatment.
[0014] According to an embodiment of the first aspect of the present disclosure, the cold rolling process has a cold rolling speed of 30 m / min-80 m / min.
[0015] According to an embodiment of the first aspect of the present disclosure, the reduction ratio of the cold rolling process is 55%-90%.
[0016] According to an embodiment of the first aspect of the present disclosure, the cold rolling process includes 2 to 5 passes, with a reduction rate of 18%-50% for each pass.
[0017] According to an embodiment of the first aspect of the present disclosure, the thickness of the ingot is 6 mm to 10 mm, and the thickness of the cast-rolled aluminum plate is 1.0 mm to 2.5 mm.
[0018] In a second aspect, an embodiment of the present disclosure provides a cast-rolled aluminum plate, comprising the following components in percentage by weight:
[0019] Si: 0.1%-0.5%; Fe: 0.1%-0.7%; Cu<0.15%; Mn: 0.5%-1.5%; Mg: 0.06%-0.7%; Ti<0.1%; wherein Si+Mn<1.6%, 0.2%≤Si+Mg≤0.5%, and the ratio of Mg to Si is: 0.55-2.
[0020] According to an embodiment of the second aspect of the present disclosure, the tensile strength of the cast-rolled aluminum plate is 120 MPa to 200 MPa, and the yield strength of the cast-rolled aluminum plate is 120 MPa to 200 MPa.
[0021] According to an embodiment of the second aspect of the present disclosure, the elongation of the cast-rolled aluminum plate is greater than or equal to 5%.
[0022] In a third aspect, an embodiment of the present disclosure provides a vehicle comprising the aforementioned cast-rolled aluminum plate.
[0023] The present invention discloses a method for reasonably proportioning alloying elements such as Mg, Mn, and Si in cast-rolled aluminum plates, wherein Mg and Si can form an effective Mg2Si strengthening phase, Mn can promote the recrystallization process of the aluminum alloy, increase the recrystallization temperature, and significantly refine the recrystallized grains. At the same time, combined with heat treatment process, the uniformity of subsequent recrystallization is improved, so that the cast-rolled aluminum plates can not only improve the strength but also have a good level of forming performance, and can improve the problems of insufficient yield strength and cracking during stamping. DETAILED DESCRIPTION
[0024] The features and exemplary embodiments of various aspects of the present disclosure are described in detail below. In the detailed description that follows, many specific details are set forth in order to provide a comprehensive understanding of the present disclosure. However, it will be apparent to those skilled in the art that the present disclosure can be implemented without some of these specific details. The following description of the embodiments is merely intended to provide a better understanding of the present disclosure by illustrating examples of the present disclosure. In the following description, at least some of the well-known structures and technologies are not shown in order to avoid unnecessary ambiguity in the present disclosure; and, for clarity, the sizes of some structures may be exaggerated. In addition, the features, structures, or characteristics described below may be combined in any suitable manner in one or more embodiments.
[0025] It should also be noted that, in the description of this disclosure, unless otherwise expressly specified or limited, the terms "mounted" and "connected" should be understood broadly. For example, they may refer to fixed connections, detachable connections, or integral connections; and they may refer to direct connections or indirect connections. Those skilled in the art will understand the specific meanings of these terms in this disclosure depending on the specific circumstances.
[0026] Currently, cast-rolled aluminum sheet is primarily used in building curtain walls, truck flooring, and various foils, where mechanical and stamping properties are not critical. It has yet to find practical use in high-end passenger vehicles. Existing cast-rolled aluminum alloy grades, in terms of yield strength and stamping formability, struggle to meet these requirements, necessitating improvements to the aluminum alloys used in these technologies.
[0027] In view of this, the inventors of the present disclosure have conducted research and provided a method for preparing a cast-rolled aluminum plate, a cast-rolled aluminum plate and a vehicle, which can improve the situation of insufficient yield strength and cracking due to stamping.
[0028] In a first aspect, an embodiment of the present disclosure provides a method for manufacturing a cast-rolled aluminum plate, comprising the following steps:
[0029] A cast ingot is provided, which includes the following components in percentage by mass: Si: 0.1%-0.5%; Mn: 0.5%-1.5%; Mg: 0.06%-0.7%; wherein Si+Mn<1.6%, 0.2%≤Si+Mg≤0.5%, and the ratio of Mg to Si is: 0.55-2; the cast ingot is annealed and cold rolled to obtain a cast-rolled aluminum plate, which includes Mg2Si.
[0030] In the step of providing the ingot, the processing technology for obtaining the ingot adopts conventional means in the field. For example, the raw materials of the cast-rolled aluminum plate are smelted and cast in sequence to obtain the ingot disclosed in the present invention. As for the specific process conditions in the above steps, they are all process conditions well known in the field and will not be repeated here.
[0031] The present disclosure improves the insufficient yield strength of cast-rolled aluminum sheets and cracking caused by stamping by rationally formulating chemical components and contents and supplementing with thermal processing. In the composition design of the present disclosure:
[0032] Si can improve the tensile strength, hardness and corrosion resistance of cast aluminum plates; Mg can improve the strength, hardness, heat resistance, corrosion resistance and cutting performance of aluminum alloys. Si and Mg can form an effective Mg2Si strengthening phase, but excessive Mg is prone to hot brittleness and cause cracks in the alloy.
[0033] Mn can promote the recrystallization process of aluminum alloys, increase the recrystallization temperature, and significantly refine the recrystallized grains; however, excessive Mn can cause segregation and reduce plasticity. Therefore, based on comprehensive considerations, the present disclosure controls the Si content to 0.1%-0.5%, the Mn content to 0.5%-1.5%, and the Mg content to 0.06%-0.7%, while also satisfying the following conditions: Si + Mn < 1.6%, 0.2% ≤ Si + Mg ≤ 0.5%, and a Mg to Si content ratio of 0.55-2.
[0034] The present invention discloses a method for reasonably proportioning alloy elements such as Mg, Mn, and Si in cast-rolled aluminum plates, wherein Mg and Si can form an effective Mg2Si strengthening phase, Mn can promote the recrystallization process of the aluminum alloy, increase the recrystallization temperature, and significantly refine the recrystallized grains. At the same time, combined with heat treatment process, the uniformity of subsequent recrystallization is improved, so that the cast-rolled aluminum plates can have improved strength and better formability, and can improve the problems of insufficient yield strength and cracking during stamping.
[0035] For example, the mass percentage of Si may be 0.1%, 0.2%, 0.3%, 0.4% or 0.5%.
[0036] For example, the mass percentage of Mn may be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.31%, 1.35% or 1.5%.
[0037] For example, the mass percentage of Mg may be 0.06%, 0.08%, 0.1%, 0.15%, 0.18%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6% or 0.7%.
[0038] The mass percentage of Si+Mg may be 0.2%, 0.3%, 0.4% or 0.5%.
[0039] In some embodiments, the ingot further includes the following components in percentage by mass: Fe: 0.1%-0.7%, Cu: 0-0.15%, Ti<0.1%, and other unavoidable impurities, with a single impurity ≤0.03%, a total impurity amount ≤0.15%, and the balance being Al. Fe can improve the hardness of the cast aluminum plate, but excessive iron will form flaky or needle-like structures of FeAl3, Fe2Al, or Al-Si-Fe, reducing the mechanical properties. Therefore, the range of controlling the Fe content in the present disclosure is 0.1-0.7%. For example, the Fe content by mass can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, or 0.7%.
[0040] Cu can improve strength, hardness, heat resistance, and machinability, as well as improve casting fluidity. However, excessive Cu content can affect the corrosion resistance and plasticity of the cast aluminum sheet and increase the tendency to hot cracking. Therefore, the Cu content in the present disclosure is controlled within a range of 0-0.15%. For example, the Cu content by mass can be 0, 0.02%, 0.04%, 0.05%, 0.06%, 0.08%, 0.10%, 0.12%, 0.14%, or 0.15%.
[0041] Ti can significantly refine the grain structure, effectively improving the alloy's mechanical properties and reducing its tendency to hot cracking. However, adding too much Ti increases the alloy's cost. Therefore, in the present disclosure, the Ti content is controlled within a range of 0-0.1%. For example, the Ti content by mass can be 0, 0.01%, 0.015%, 0.02%, 0.04%, 0.06%, 0.08%, or 0.10%.
[0042] In summary, the present invention improves the uniformity of subsequent recrystallization by reasonably proportioning alloy elements such as Mn, Mg, Si, Fe, Cu, Ti in the cast-rolled aluminum plate and processing it through a heat treatment process, so that the cast-rolled aluminum plate can not only improve the strength but also have a better level of forming performance, and can improve the situation of insufficient yield strength and cracking during stamping.
[0043] In some embodiments, the steps of annealing and cold rolling the ingot include: subjecting the ingot to a first annealing treatment and a second annealing treatment, with at least one cold rolling treatment between the first annealing treatment and the second annealing treatment; the process parameters of the first annealing treatment are: annealing at 500°C-600°C for 10h-20h; the process parameters of the second annealing treatment are: annealing at 240°C-450°C for 2h-8h.
[0044] In the disclosed embodiments, the annealing process includes at least two passes, and at least one cold rolling process is included between the two annealing processes. For example, the cold rolling process may include 2-5 passes, and the 2-5 cold rolling passes may all be performed between the two annealing processes, or only one cold rolling pass may be included between the two annealing processes.
[0045] The first annealing treatment is to anneal the cast aluminum plate at 500°C-600°C for 10h-20h. Annealing under this condition can promote the precipitation of manganese-containing phase and is beneficial to grain homogenization.
[0046] The second annealing treatment is to anneal the cast aluminum plate at 240℃-450℃ for 2h-8h. After at least one cold rolling process, annealing is performed again, which is beneficial to further homogenize the grains during recrystallization and improve the yield strength and tensile strength of the cast aluminum plate.
[0047] Compared with the related art, the present disclosure adopts at least two annealing treatments to keep the yield strength and elongation of the material in a state of good mutual matching, so that both the strength and the stamping forming requirements can be met.
[0048] In some embodiments, the step of annealing and cold rolling the ingot includes: before the ingot is subjected to the first annealing treatment, the ingot is further subjected to at least one pass of cold rolling treatment.
[0049] In the present disclosure, before the first annealing treatment, the casting may further include performing at least one pass of cold rolling on the casting, where one pass means that the casting passes through a roll gap once.
[0050] For example, before the first annealing treatment, one or two passes of cold rolling treatment can be performed. The cold rolling treatment can improve the strength of the cast aluminum plate. Annealing treatment after the cold rolling treatment helps to improve the yield strength and tensile strength of the cast aluminum plate.
[0051] In some embodiments, the step of annealing and cold rolling the ingot includes: after the ingot is subjected to the second annealing treatment, further comprising performing at least one pass of cold rolling on the ingot.
[0052] Performing at least one cold rolling process after the second annealing process helps to further improve the yield strength and tensile strength of the cast aluminum plate.
[0053] In some embodiments, the cold rolling process has a cold rolling speed of 30 m / min to 80 m / min.
[0054] According to the embodiments of the present disclosure, the cold rolling speed is within the range of 30 m / min-80 m / min, which can make the material structure of the cast aluminum plate more uniform.
[0055] In some embodiments, the reduction ratio of the cold rolling process is 55%-90%. According to the embodiments of the present disclosure, the reduction ratio is 55%-90%, which can effectively improve the strength of the cast aluminum plate.
[0056] In some embodiments, the cold rolling process includes 2 to 5 passes, with each pass having a reduction ratio of 18% to 50%.
[0057] According to embodiments of the present disclosure, the cold rolling process may include 2, 3, 4, or 5 passes. Multiple cold rolling passes combined with two annealing treatments can increase the strength and hardness of the ingot. The reduction ratio of each pass may be 18%, 20%, 25%, 28%, 30%, 33%, 35%, 38%, 40%, 45%, or 50%.
[0058] In some embodiments, the thickness of the ingot is 6 mm to 10 mm, and the thickness of the cast aluminum plate is 1.0 mm to 2.5 mm.
[0059] In a second aspect, an embodiment of the present disclosure provides a cast-rolled aluminum plate, comprising the following components in percentage by weight:
[0060] Si: 0.1%-0.5%; Fe: 0.1%-0.7%; Cu<0.15%; Mn: 0.5%-1.5%; Mg: 0.06%-0.7%, Ti<0.1%; wherein Si+Mn<1.6%, 0.2%≤Si+Mg≤0.5%, and the ratio of Mg to Si is: 0.55-2.
[0061] The present invention discloses a method for reasonably proportioning alloying elements such as Mn, Mg, Si, Fe, Cu, and Ti in cast-rolled aluminum plates. Mg and Si can form an effective Mg2Si strengthening phase, and Mn can promote the recrystallization process of the aluminum alloy, increase the recrystallization temperature, and significantly refine the recrystallized grains. At the same time, through heat treatment, the uniformity of subsequent recrystallization is improved, so that the cast-rolled aluminum plates can have improved strength and better formability, and can improve the problems of insufficient yield strength and cracking during stamping.
[0062] Iron can improve the hardness of cast aluminum sheets, but excessive iron can form flaky or acicular structures called FeAl₃, Fe₂Al, or Al-Si-Fe structures, reducing mechanical properties. Therefore, the Fe content in this disclosure is controlled within a range of 0.1-0.7%. For example, the Fe content by mass can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, or 0.7%.
[0063] Cu can improve strength, hardness, heat resistance, and machinability, as well as improve casting fluidity. However, excessive Cu content can affect the corrosion resistance and plasticity of the cast aluminum sheet and increase the tendency to hot cracking. Therefore, the Cu content in the present disclosure is controlled within a range of 0-0.15%. For example, the Cu content by mass can be 0, 0.02%, 0.04%, 0.05%, 0.06%, 0.08%, 0.10%, 0.12%, 0.14%, or 0.15%.
[0064] Ti can significantly refine the grain structure, effectively improving the alloy's mechanical properties and reducing its tendency to hot cracking. However, adding too much Ti increases the alloy's cost. Therefore, in the present disclosure, the Ti content is controlled within a range of 0-0.1%. For example, the Ti content by mass can be 0, 0.01%, 0.015%, 0.02%, 0.04%, 0.06%, 0.08%, or 0.10%.
[0065] In some embodiments, the cast-rolled aluminum plate includes, in addition to the aforementioned components, unavoidable impurities, with a single impurity being ≤0.03%, a total impurity amount being ≤0.15%, and the balance being Al.
[0066] In some embodiments, the tensile strength of the cast aluminum plate is 120 MPa to 200 MPa.
[0067] In some embodiments, the cast aluminum sheet has a yield strength of 120 MPa to 200 MPa.
[0068] In some embodiments, the cast aluminum sheet has an elongation greater than or equal to 5%.
[0069] In a third aspect, an embodiment of the present disclosure provides a vehicle comprising the aforementioned cast-rolled aluminum plate.
[0070] The tensile strength and yield strength of the cast-rolled aluminum plate provided by the present disclosure are effectively improved, and can be applied to vehicles, especially in scenarios where the stamping requirements in vehicles are not complicated.
[0071] Hereinafter, the method for producing the cast-rolled aluminum plate material of the present disclosure will be described in more detail through examples, but the present disclosure is not limited to these examples at all.
[0072] Example 1
[0073] This embodiment provides a method for manufacturing a cast-rolled aluminum plate, which comprises the following steps:
[0074] The ingot is provided. The measured composition of the ingot is as follows: Si: 0.221%, Fe: 0.501%, Cu: 0.066%, Mn: 1.069%, Mg: 0.212%, Ti: 0.009%, individual impurities ≤ 0.03%; total impurities ≤ 0.15%, the balance being aluminum. The ingot thickness is 6.8 mm.
[0075] After the first cold rolling to 5.5mm, the first annealing treatment is carried out with the process parameters of 585℃X15h; then two cold rolling passes (3.1mm, 1.9mm) are carried out, and the second annealing treatment is carried out after completion with the process parameters of 380℃X2h. Finally, the cast aluminum plate is cold rolled once to a thickness of 1.5mm.
[0076] Example 2
[0077] This embodiment provides a method for manufacturing a cast-rolled aluminum plate, which is similar to Example 1, except that the actual measured composition of the ingot is as follows: Si: 0.305%, Fe: 0.522%, Cu: 0.061%, Mn: 1.150%, Mg: 0.177%, Ti: 0.011%, and a single impurity is ≤0.03%; the total amount of impurities is ≤0.15%, and the balance is aluminum.
[0078] Example 3
[0079] This embodiment provides a method for manufacturing a cast-rolled aluminum plate, which is similar to Example 1, except that the actual measured composition of the ingot is as follows: Si: 0.162%, Fe: 0.501%, Cu: 0.066%, Mn: 1.069%, Mg: 0.233%, Ti: 0.009%, and a single impurity is ≤0.03%; the total amount of impurities is ≤0.15%, and the balance is aluminum.
[0080] Example 4
[0081] This embodiment provides a method for manufacturing a cast-rolled aluminum plate. The manufacturing method is similar to that of Example 1, except that:
[0082] After the first cold rolling to 5.5mm, the first annealing treatment is carried out with the process parameters of 585℃X15h; then two cold rolling passes (3.1mm, 1.75mm) are carried out, and the second annealing treatment is carried out after completion with the process parameters of 380℃X2h. Finally, the cast aluminum plate is cold rolled to a thickness of 1.5mm.
[0083] Example 5
[0084] This embodiment provides a method for manufacturing a cast-rolled aluminum plate. The manufacturing method is similar to that of Example 1, except that:
[0085] After the first cold rolling to 5.5mm, the first annealing treatment is carried out with the process parameters of 585℃X15h; then two more cold rolling passes (3.1mm, 2.2mm) are carried out, and the second annealing treatment is carried out after completion with the process parameters of 380℃X2h. In the final pass, the plate thickness is rolled to 1.5mm.
[0086] Example 6
[0087] This embodiment provides a method for manufacturing a cast-rolled aluminum plate. The manufacturing method is similar to that of Example 1, except that:
[0088] After the first cold rolling to 5.5mm, the first annealing treatment is carried out with the process parameters of 585℃X15h; then three cold rolling passes (3.1mm, 1.9mm, 1.5mm) are carried out, and the second annealing treatment is carried out after completion with the process parameters of 260℃X2h. The final plate thickness is 1.5mm.
[0089] Comparative Example 1
[0090] This embodiment provides a method for manufacturing a cast-rolled aluminum plate, which is similar to Example 1, except that the actual measured composition of the ingot is as follows: Si: 0.12%, Fe: 0.53%, Cu: 0.08%, Mn: 1.09%, Mg: 0.004%, Ti: 0.027%, and a single impurity is ≤0.03%; the total amount of impurities is ≤0.15%, and the balance is aluminum.
[0091] Comparative Example 2
[0092] This embodiment provides a method for manufacturing a cast-rolled aluminum plate. The manufacturing method is similar to that of Example 1, except that:
[0093] The ingot was cold rolled in four passes to 5.5 mm, 3.1 mm, 2.2 mm and 1.5 mm respectively, and then annealed once. The process parameters were: 380 ° C X 2 h.
[0094] Comparative Example 3
[0095] This embodiment provides a method for manufacturing a cast-rolled aluminum plate. The manufacturing method is similar to that of Example 1, except that:
[0096] The ingot was cold rolled in four passes to 5.5 mm, 3.1 mm, 1.9 mm and 1.5 mm respectively, and then annealed once. The process parameters were: 380 ° C X 2 h.
[0097] Comparative Example 4
[0098] This embodiment provides a method for manufacturing a cast-rolled aluminum plate. The manufacturing method is similar to that of Example 1, except that: after the first cold rolling to 5.5 mm, a first annealing treatment is performed with process parameters of 300°C x 15 h; then two cold rolling passes (3.1 mm, 1.9 mm) are performed, and after completion, a second annealing treatment is performed with process parameters of 380°C x 2 h. Finally, a final cold rolling pass is performed to roll the cast-rolled aluminum plate to a thickness of 1.5 mm.
[0099] Performance testing:
[0100] Test method: Tested according to GB / T 228.1-2021
[0101] Table 1 Performance comparison between comparative examples and examples
[0102] The present invention discloses a method for reasonably designing material composition, reasonably proportioning alloy elements such as Mn, Mg, Si, Fe, Cu, and Ti in cast-rolled aluminum plates, and adopting a reasonable heat treatment process during the casting and rolling process, so that the yield strength and elongation of the material are kept in a state of good mutual matching, and the strength can meet the requirements, and the stamping forming requirements can also be met. The tensile strength is 120Mpa to 200Mpa, the yield strength is 120Mpa to 200Mpa, and the elongation is greater than 5%, thereby achieving a good balance between mechanical strength and machinability.
[0103] It's important to note that the various elements in cast aluminum sheet interact with each other, collectively influencing the final sheet's properties. For example, Si improves the tensile strength, hardness, and corrosion resistance of cast aluminum sheet. Mg, on the other hand, enhances the strength, hardness, heat resistance, corrosion resistance, and machinability of aluminum alloys. Si and Mg form a Mg2Si strengthening phase, improving the sheet's properties.
[0104] Compared to the examples disclosed herein, Comparative Example 1 has a lower Mg content, with Si+Mg less than 0.2% and a Mg to Si ratio of less than 0.55, resulting in poor tensile strength and yield strength. This may be because Si and Mg cannot form an effective Mg2Si strengthening phase or the amount of strengthening phase formed is too low. Furthermore, Example 2, while having a lower Mg content than Examples 1 and 3, also achieves relatively good performance. This may be because Mg and Mn can jointly strengthen the steel, creating a synergistic effect.
[0105] Compared to Example 1, which underwent two annealing treatments, Comparative Examples 2 and 3 only underwent a single annealing treatment, resulting in lower tensile strength and yield strength. This is because in Example 1, the cast aluminum sheet was first annealed at 585°C, which promoted the precipitation of manganese-containing phases and facilitated grain homogenization. The second annealing treatment, performed at 380°C, further facilitated grain homogenization during recrystallization, increased the yield strength and tensile strength of the cast aluminum sheet, and maintained a good match between the material's yield strength and elongation, meeting both strength and stamping requirements. However, Comparative Examples 2 and 3 only underwent a single annealing treatment, which was not conducive to promoting the precipitation of manganese-containing phases and grain homogenization, resulting in unsatisfactory strength.
[0106] In Comparative Example 4, the first annealing treatment was performed at 300° C., which was not conducive to promoting the precipitation of the manganese-containing phase and grain homogenization. Compared with Example 1, the elongation was significantly reduced to less than 5%, and the tensile strength and yield strength were also reduced.
[0107] While the present disclosure has been described with reference to preferred embodiments, various modifications may be made thereto and equivalent components may be substituted without departing from the scope of the present disclosure. In particular, the various technical features described in the various embodiments may be combined in any manner, provided no structural conflicts exist. The present disclosure is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.
Claims
1. A method for manufacturing a cast-rolled aluminum plate, comprising the following steps: Obtaining a casting billet, the casting billet comprises the following components in percentage by mass: Si: 0.1%-0.5%; Mn: 0.5%-1.5%; Mg: 0.06%-0.7%; wherein Si+Mn<1.6%, 0.2%≤Si+Mg≤0.5%, and the content ratio of Mg to Si is: 0.55-2; The ingot is subjected to annealing and cold rolling to obtain a cast aluminum plate, which includes Mg2Si.
2. The method for manufacturing a cast-rolled aluminum plate according to claim 1, wherein the cast billet further comprises the following components in percentage by mass: Fe: 0.1%-0.7%, Cu: 0-0.15%, Ti<0.1%, and other unavoidable impurities, and a single impurity ≤0.03%, the total amount of impurities ≤0.15%, the balance is Al.
3. The method for manufacturing a cast-rolled aluminum plate according to claim 1 or 2, wherein the step of annealing and cold rolling the cast billet comprises: The ingot is subjected to a first annealing treatment and a second annealing treatment, wherein at least one cold rolling process is included between the first annealing treatment and the second annealing treatment; The process parameters of the first annealing treatment are: annealing at 500°C-600°C for 10h-20h; The process parameters of the second annealing treatment are: annealing at 240° C.-450° C. for 2 h-8 h.
4. The method for manufacturing a cast-rolled aluminum plate according to claim 3, wherein the step of annealing and cold rolling the cast billet comprises: Before the cast billet is subjected to the first annealing treatment, the cast billet is subjected to at least one cold rolling treatment.
5. The method for manufacturing a cast-rolled aluminum plate according to claim 3, wherein the step of annealing and cold rolling the cast billet comprises: After the cast billet is subjected to the second annealing treatment, the cast billet is further subjected to at least one cold rolling treatment.
6. The method for manufacturing a cast-rolled aluminum plate according to claim 3, wherein the cold rolling speed of the cold rolling treatment is 30m / min-80m / min.
7. The method for manufacturing a cast-rolled aluminum plate according to any one of claims 1 to 6, wherein the reduction ratio of the cold rolling treatment is 55% to 90%.
8. The method for manufacturing a cast-rolled aluminum plate according to claim 7, wherein the cold rolling process comprises 2 to 5 passes, and the reduction rate of each pass is 18%-50%.
9. The method for manufacturing the cast-rolled aluminum plate according to any one of claims 1 to 8, wherein the thickness of the ingot is 6 mm to 10 mm, and the thickness of the cast-rolled aluminum plate is 1.0 mm to 2.5 mm.
10. A cast-rolled aluminum plate comprising the following components in percentage by mass: Si: 0.1%-0.5%; Fe: 0.1%-0.7%; Cu<0.15%; Mn: 0.5%-1.5%; Mg: 0.06%-0.7%; Ti<0.1%; Among them, Si+Mn<1.6%, 0.2%≤Si+Mg≤0.5%, and the content ratio of Mg to Si is: 0.55-2. 11 . The cast-rolled aluminum plate according to claim 10 , wherein the tensile strength of the cast-rolled aluminum plate is 120 MPa to 200 MPa, and the yield strength of the cast-rolled aluminum plate is 120 MPa to 200 MPa.
12. The cast-rolled aluminum plate according to claim 10 or 11, wherein the elongation of the cast-rolled aluminum plate is greater than or equal to 5%.
13. A vehicle, wherein the vehicle comprises the cast-rolled aluminum plate according to any one of claims 10 to 12.
Citation Information
Patent Citations
Aluminium tape for hollow super insulated aluminum strip and preparation method thereof
CN104313398A
5G novel capacitor outer shell aluminum strip and preparation method thereof
CN111850353A
New energy battery aluminum shell material for continuous die stamping and manufacturing method thereof
CN115216669A
Method of making aluminum rivets with high ductility retention
US4620886A
Aluminium alloy sheet for metallic bottle or aerosol container
WO2014184450A1