Copper foil and composite film
The copper foil with a specific surface texture improves adhesion and moldability, addressing cracking issues in EMI countermeasure films, ensuring effective EMI shielding for dense electronic components.
Patent Information
- Application Number
- PCT/JP2024/012383
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Copper foil used in EMI countermeasure films for electronic devices faces challenges with cracking and thinning during three-dimensional processing due to its thinness and surface irregularities, which affects moldability and adhesion with resin layers, especially in densely packed components and high-frequency environments.
A copper foil with a gentle uneven surface having an arithmetic mean wavelength of 10 μm to 80 μm and an arithmetic mean inclination angle of 0.4° to 4° is developed, which enhances adhesion with resin and moldability, reducing the likelihood of cracking during three-dimensional processing.
The modified copper foil and composite film exhibit excellent moldability and adhesion, preventing cracking and ensuring effective electromagnetic interference (EMI) shielding, suitable for high-density electronic devices like smartphones and medical equipment.
Smart Images

Figure JP2024012383_03102024_PF_FP_ABST
Abstract
Description
Copper foil and composite film
[0001] The present invention relates to copper foils and composite films.
[0002] In recent years, electronic devices such as smartphones, medical devices, and automobiles have become increasingly highly integrated and performant. This has led to an increased importance of electromagnetic interference (EMI) countermeasures to suppress EMI in electronic devices. Therefore, components such as noise filters and electromagnetic wave absorbing sheets are used in electronic devices to prevent malfunctions of the electronic devices and degradation of communication data quality due to electromagnetic waves from inside and outside the electronic device's housing. Among these components, composite films known as EMI countermeasure films are used in many electronic devices. EMI countermeasure films are composite films having a laminated structure consisting of an electromagnetic wave shielding layer made of a metal or the like and a resin layer made of a conductive resin material. Copper foil is sometimes used as the electromagnetic wave shielding layer due to its high conductivity, shielding properties, and industrial productivity.
[0003] When attaching an EMI control film to an electronic device, an electromagnetic wave shielding layer is typically attached to a metal part within the electronic device via a resin layer. In recent years, as the density of component packaging in electronic devices such as smartphones has increased, EMI control films are increasingly being mounted in narrow spaces. Furthermore, as electronic devices operate at higher frequencies, EMI control films are required to adequately suppress electromagnetic noise leakage. Therefore, EMI control films are required to have excellent formability, so that they can easily deform to conform to the shape of the object they are attached to, such as an integrated circuit or a flexible substrate.
[0004] When attaching an EMI countermeasure film to an object, the EMI countermeasure film may be subjected to three-dimensional processing such as bulging or drawing. However, because copper foil is thin, this can cause thinning and lead to cracks. Furthermore, if the copper foil surface is uneven, the recesses are particularly thin and prone to stress concentration, making the film prone to thinning and cracking when three-dimensional processing is performed. Therefore, EMI countermeasure films are required to have excellent formability, such as being less likely to crack even when three-dimensional processing is performed, and being able to easily deform to follow the shape of the object to which they are attached. Furthermore, EMI countermeasure films are also required to have excellent adhesion between the copper foil and the resin layer.
[0005] Japanese Patent Publication No. 6805382 Japanese Patent Publication No. 6379071
[0006] Patent Documents 1 and 2 disclose composite films with excellent formability. However, in electronic devices such as smartphones, the density of component mounting is becoming increasingly high, and therefore, composite films such as EMI control films are required to have further improved formability. An object of the present invention is to provide a copper foil that has excellent adhesion to resins and excellent formability, and a composite film using the copper foil that has excellent formability.
[0007] In order to solve the above problems, the present inventors have conducted extensive research focusing on the surface shape of copper foil, and have found that if a gently uneven shape is uniformly formed on the surface of copper foil, when the copper foil is subjected to three-dimensional processing, the reduction in thickness occurs in a dispersed manner in each of the depressions uniformly present on the surface of the copper foil, thereby suppressing the phenomenon in which only specific depressions reduce thickness and cause cracks in the copper foil.
[0008] That is, in one aspect of the present invention, the copper foil has two surfaces, at least one of which is an uneven surface having an arithmetic mean wavelength Wλa of 10 μm or more and 80 μm or less, and an arithmetic mean tilt angle WΔa of 0.4° or more and 4° or less. In another aspect of the present invention, the composite film comprises the copper foil according to the above aspect of the present invention and a resin layer laminated on one or both of the two surfaces of the copper foil.
[0009] The copper foil according to the present invention has excellent adhesion to resin and excellent formability, and a composite film using the copper foil has excellent formability.
[0010] 1 is a cross-sectional view illustrating a composite film according to an embodiment of the present invention.
[0011] An embodiment of the present invention will be described below. Note that the embodiment described below is merely an example of the present invention. Furthermore, various modifications or improvements can be made to this embodiment, and such modifications or improvements are also included in the present invention. As shown in FIG. 1 , a composite film 1 according to this embodiment comprises a copper foil 10 forming an electromagnetic wave shielding layer, and a resin layer 20 made of a conductive resin material and laminated on one surface 10 a of the two surfaces of the copper foil 10.
[0012] Of the two surfaces of the copper foil 10, the surface 10a on which the resin layer 20 is laminated is an uneven surface having an arithmetic mean wavelength Wλa of 10 μm or more and 80 μm or less, and an arithmetic mean tilt angle WΔa of 0.4° or more and 4° or less. Of the two surfaces of the copper foil 10, the surface on which the resin layer 20 is not laminated is a surface that does not satisfy the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa.
[0013] That is, one surface 10a of the two surfaces of the copper foil 10 is an uneven surface that satisfies the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, and the other surface is a surface that does not satisfy the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, and a resin layer 20 is laminated on the uneven surface, thereby producing a composite film 1.
[0014] Due to this configuration, the copper foil 10 and the composite film 1 have excellent formability. That is, when the composite film 1 is subjected to three-dimensional processing, cracks are unlikely to occur in the copper foil 10. Furthermore, when the composite film 1 is attached to an attachment target such as an integrated circuit or a flexible substrate, the composite film 1 easily deforms to follow the shape of the attachment target.
[0015] Furthermore, if the uneven surface satisfies the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, the copper foil 10 will have high thickness uniformity and excellent adhesion to the resin layer 20. Furthermore, if the uneven surface satisfies the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, the uneven surface will have unevenness, but the unevenness will be gentle, resulting in a smooth and highly glossy surface.
[0016] Because of such excellent performance, the composite film 1 according to this embodiment can be suitably used as an EMI control film. Therefore, the composite film 1 according to this embodiment can be used as an EMI control film for various electronic devices and exhibits excellent EMI resistance. The composite film 1 according to this embodiment can be suitably used in electronic devices such as smartphones, medical devices, and automobiles, and can be particularly suitably used in mobile electronic devices such as smartphones.
[0017] The composite film 1 in FIG. 1 is an example in which only one surface 10a of the two surfaces of the copper foil 10 is an uneven surface that satisfies the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, and a resin layer 20 is laminated on the surface 10a, but the composite film according to the present invention is not limited to this example.
[0018] For example, only one surface 10a of the two surfaces of the copper foil 10 may be an uneven surface that satisfies the above conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, or both of the two surfaces of the copper foil 10 may be uneven surfaces that satisfy the above conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa.
[0019] When only one surface 10a of the two surfaces of the copper foil 10 has an uneven surface that satisfies the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, the resin layer 20 may be laminated on the uneven surface 10a that satisfies the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa, or the resin layer 20 may be laminated on the surface (the surface opposite to the surface 10a) that does not satisfy the conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa. Furthermore, the composite film 1 of FIG. 1 is an example in which the resin layer 20 is laminated on only one surface 10a of the two surfaces of the copper foil 10, but the resin layer 20 may be laminated on both of the two surfaces of the copper foil 10.
[0020] The composite film 1 according to this embodiment may further include at least one of a release film 30, an insulating layer 40, and a carrier film 50. That is, a modified example of the composite film 1 according to this embodiment may have a structure in which a release film 30 is further laminated on the resin layer 20, as shown in FIG. 2 . Also, a modified example of the composite film 1 according to this embodiment may have a structure in which an insulating layer 40 that electrically protects the copper foil 10 is further laminated on the surface 10b of the two surfaces of the copper foil 10 opposite the surface 10a on which the resin layer 20 is laminated, as shown in FIG. 2 . Furthermore, a modified example of the composite film 1 according to this embodiment may have a structure in which a carrier film 50 serving as a support is further laminated on the insulating layer 40, as shown in FIG. 2 .
[0021] 2 shows an example of a composite film 1 including the release film 30, the insulating layer 40, and the carrier film 50, but the modified example of the composite film 1 according to the present embodiment is not limited to this. However, when the resin layer 20 is laminated on both of the two surfaces 10a, 10b of the copper foil 10, the composite film 1 does not include the insulating layer 40 and the carrier film 50.
[0022] The composite film 1 according to this embodiment will be described in further detail below. (1) Copper Foil As the copper foil 10 of the composite film 1 according to this embodiment, either an electrolytic copper foil or a rolled copper foil can be used, and copper foil formed by a known method such as vapor deposition or sputtering can also be used. Copper foil whose surface shape and thickness have been adjusted by a known method such as etching or electropolishing may also be used as the copper foil 10 of the composite film 1 according to this embodiment.
[0023] The thickness of the copper foil 10 of the composite film 1 according to this embodiment is preferably 5 μm or more and 30 μm or less. If the thickness of the copper foil 10 is 30 μm or less, springback is less likely to occur during three-dimensional processing. Furthermore, if the thickness of the copper foil 10 is 30 μm or less, the composite film 1 tends to be thin and lightweight, making it suitable for mounting on mobile electronic devices such as smartphones. If the thickness of the copper foil 10 is 5 μm or more, pinholes are less likely to occur during manufacturing of the copper foil 10, making it less likely for cracks to occur in the copper foil 10 during three-dimensional processing. The thickness of the copper foil 10 is more preferably 5 μm or more and 20 μm or less.
[0024] (2) Regarding the uneven surface The arithmetic mean wavelength Wλa of the uneven surface of the copper foil 10 must be 10 μm or more and 80 μm or less, but preferably 20 μm or more and 70 μm or less. If the arithmetic mean wavelength Wλa is less than 10 μm, the frequency of unevenness on the copper foil surface is high, which deteriorates the adhesive filling ability and easily impairs adhesion with the resin. If the arithmetic mean wavelength Wλa exceeds 80 μm, the frequency of unevenness on the copper foil surface is low, making it difficult to obtain adhesion with the resin and to obtain crack prevention effect during three-dimensional processing.
[0025] The arithmetic mean tilt angle WΔa of the uneven surface of the copper foil 10 must be 0.4° or more and 4° or less, but is preferably 0.6° or more and 3° or less. If the arithmetic mean tilt angle WΔa is less than 0.4°, the unevenness of the copper foil surface is too gentle, making it difficult to prevent cracks during three-dimensional processing. If the arithmetic mean tilt angle WΔa is more than 4°, the unevenness of the copper foil surface is too steep, making it more likely to crack during three-dimensional processing.
[0026] Furthermore, the arithmetic mean waviness Wa of the uneven surface of the copper foil 10 is preferably 0.07 μm or more and 0.45 μm or less, and more preferably 0.10 μm or more and 0.40 μm or less. If the arithmetic mean waviness Wa is less than 0.07 μm, the copper foil surface is too smooth, making it difficult to prevent cracking during three-dimensional processing. If the arithmetic mean waviness Wa exceeds 0.45 μm, the copper foil surface is too rough, resulting in poor adhesive filling and a loss of adhesion to the resin. If the uneven surface of the copper foil 10 satisfies the above arithmetic mean waviness Wa condition, the copper foil 10 and the composite film 1 have excellent formability, and the copper foil 10 has excellent adhesion to the resin layer 20.
[0027] Furthermore, the developed area ratio Sdr of the uneven surface of the copper foil 10 is preferably 0.007 or more and 0.200 or less, and more preferably 0.007 or more and 0.100 or less. If the developed area ratio Sdr is less than 0.007, the copper foil surface is too smooth, making it difficult to prevent cracking during three-dimensional processing. If the developed area ratio Sdr exceeds 0.200, the copper foil surface is too rough, making it more likely to crack during three-dimensional processing. If the uneven surface of the copper foil 10 satisfies the above-mentioned developed area ratio Sdr condition, the copper foil 10 and the composite film 1 have excellent formability.
[0028] (3) Resin Layer The resin layer 20 of the composite film 1 according to this embodiment is made of a resin material having electrical conductivity. Examples of the resin material having electrical conductivity include a conductive pressure-sensitive adhesive containing a conductive filler and a conductive adhesive containing a conductive filler. The conductive pressure-sensitive adhesive and the conductive adhesive contain a conductive filler and a resin that imparts electrical conductivity to the resin layer 20.
[0029] The conductive adhesive may have adhesiveness at room temperature. The resin contained in the conductive adhesive may be a thermosetting resin or a thermoplastic resin. The conductive adhesive containing a thermosetting resin may be in an uncured, B-stage, or cured state in the composite film 1.
[0030] Examples of resins contained in conductive pressure-sensitive adhesives and conductive adhesives include epoxy-based, phenol-based, amino-based, alkyd-based, urethane-based, synthetic rubber-based, acrylate-based, acrylic-based, silicone-based, imide-based, isocyanate-based, vinyl chloride-based, vinyl acetate-based, styrene-based, and hydrocarbon-based resins and pressure-sensitive adhesives. Among these resins, epoxy resins are preferred because of their excellent heat resistance.
[0031] Examples of the conductive filler include metal particles and carbon particles. Examples of the metal include silver (Ag), platinum (Pt), gold (Au), copper (Cu), nickel (Ni), palladium (Pd), aluminum (Al), solder, and alloys thereof. Examples of the carbon particles include graphite particles, baked carbon particles, and plated baked carbon particles. Among these particles, copper particles and graphite particles are preferred from the viewpoints of moldability and industrial productivity when producing the resin layer 20.
[0032] The thickness of the resin layer 20 is preferably 5 μm or more and 50 μm or less. If the thickness of the resin layer 20 is 5 μm or more, the resin layer 20 can easily conform to the shape and steps of the ground (GND) opening of the printed wiring board or the metal housing of the electronic device, and the target location can be sufficiently filled with the resin layer 20. On the other hand, if the thickness of the resin layer 20 is 50 μm or less, the flexibility of the composite film 1 is excellent, and the composite film 1 can be mounted in a thinner space.
[0033] (4) Regarding the manufacturing method of copper foil Copper foil having an uneven surface that satisfies the above conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa can be manufactured by a known copper foil manufacturing method. Examples of copper foil manufacturing methods include sandblasting, embossing, etching, plating, etc. Among these methods, plating is suitable for achieving a surface shape with shallow and gentle unevenness. The plating method will be described in detail.
[0034] The copper foil 10 according to this embodiment can be obtained by plating a typical copper foil with smooth surfaces on both sides to convert the copper foil surface into a textured surface that satisfies the above-mentioned conditions of the arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa. Among various plating methods, a low current density electrolysis method using a mesh anode is preferred. Using a mesh anode as the anode results in a non-uniform current distribution on the copper foil surface, making it easier to form a surface shape with shallow, gentle texture. Examples of mesh anodes include mesh 100, a platinum mesh with a wire diameter of 0.07 mm.
[0035] The electrode distance during plating is preferably 20 mm or more and 80 mm or less. If the electrode distance is 20 mm or more, short circuits are unlikely to occur even if the copper foil moves due to the flow of the electrolyte. If the electrode distance is 80 mm or less, the current distribution on the surface of the copper foil is likely to be uneven, making it easier to form a surface shape with shallow, gentle irregularities.
[0036] The current density during plating is, for example, 1 A / dm 2 10A / dm or more 2 It is preferable that the current density is 10 A / dm or less. 2 If the current density is 1 A / dm or less, a surface shape with shallow and gentle unevenness is easily formed. 2 If the above conditions are met, a surface shape having shallow and gentle irregularities can be easily formed, and the copper foil 10 according to this embodiment can be produced with high productivity.
[0037] As described above, the current density during plating is preferably low. High current densities result in so-called roughening plating, which can lead to a uniform copper foil thickness, or the copper foil can break or the roughening particles can fall off during three-dimensional processing, potentially preventing the achievement of the object of the present invention. However, the appropriate current density is also significantly affected by the composition of the electrolytic solution (e.g., copper concentration, sulfuric acid concentration), temperature, flow rate, plating time, etc.
[0038] The flow rate of the electrolyte refers to the average flow rate of the electrolyte flowing between the electrodes. For example, in a system in which copper foil is transported through the electrolyte, the flow rate of the electrolyte is the relative speed with respect to a fixed anode, i.e., the transport speed of the copper foil. In a system in which the copper foil is fixed and the electrolyte is made to flow using a pump or the like, the flow rate of the electrolyte is the volume per unit time of the electrolyte transported between the electrodes by the pump divided by the cross-sectional area of the flow path of the electrolyte flowing between the electrodes (the cross-sectional area of the flow path of the electrolyte that appears when the flow path of the electrolyte is cut along a plane perpendicular to the direction of flow of the electrolyte).
[0039] The following methods can be mentioned as methods for producing the copper foil 10 other than the plating method. For example, a method can be used in which a textured pattern is formed in advance by machining or the like on the surface of a drum, for example made of titanium, used in the production of the electrolytic copper foil, and the electrolytic copper foil is produced using the drum. This method can provide an electrolytic copper foil having, on its surface, a replica shape of the textured pattern formed on the drum surface.
[0040] Another example is a method in which electrodeposition is performed on a copper foil having a smooth surface, and the copper foil surface is converted into an irregular surface that satisfies the above-mentioned conditions of arithmetic mean wavelength Wλa and arithmetic mean tilt angle WΔa. Methods for controlling the surface shape of the copper foil during electrodeposition include a method of controlling the electrodeposit shape using known organic additives such as glue or thiourea, and a method of controlling the electrodeposit shape using pulse electrolysis or PR electrolysis. These methods may be performed singly or in combination.
[0041] Furthermore, after the copper foil 10 according to this embodiment is produced by the above-described plating method, an anti-rust treatment may be applied to the irregular surface of the copper foil 10. An example of the anti-rust treatment is a plating treatment in which the copper foil 10 is coated with a film containing at least one metal selected from the group consisting of nickel, zinc (Zn), chromium (Cr), molybdenum (Mo), cobalt (Co), silicon (Si), and tungsten (W).
[0042] [Examples] The present invention will be explained in more detail below with reference to examples and comparative examples. (Example 1) The matte surface of a non-rust-proof electrolytic copper foil DR-WS manufactured by Furukawa Electric Co., Ltd. was plated to adjust the surface shape of the matte surface, and the arithmetic mean wavelength Wλa, arithmetic mean tilt angle WΔa, arithmetic mean waviness Wa, and developed area ratio Sdr of the matte surface were as shown in Table 1. The thickness of the copper foil was 10 μm.
[0043]
[0044] <Plating Treatment> The electrolytic solution used for the plating treatment contained copper and sulfuric acid, with a copper concentration of 40 g / L and a sulfuric acid concentration of 80 g / L. The temperature of the electrolytic solution was 25° C. The anode used was a platinum mesh with a mesh size of 100 and a wire diameter of 0.07 mm.
[0045] The electrode distance during plating was 50 mm, and the current density, plating time, and electrolyte flow rate were as shown in Table 1. In Example 1, the copper foil was transported in a stationary electrolyte, so the copper foil transport speed was used as the electrolyte flow rate. The plating time was adjusted by adjusting the length of the anode using a shielding plate.
[0046] <Measurement of Surface Profile> The arithmetic mean wavelength Wλa, arithmetic mean tilt angle WΔa, and arithmetic mean waviness Wa of the matte surface (plated surface) were measured as follows. In accordance with ISO 25178, the matte surface of the copper foil was analyzed using a laser microscope VK-X3000 manufactured by Keyence Corporation, and data analysis was performed using the software provided with the laser microscope. The objective lens magnification of the laser microscope was 50x, the scan mode was laser confocal, the measurement size was 2048 × 1536, the measurement quality was "High Precision," and the pitch was 0.1 μm.
[0047] In analyzing the matte surface (plated surface) of the copper foil, the line roughness was measured in a direction parallel to the width direction of the copper foil using a multiple line roughness measurement mode. At that time, the line roughness was measured at nine arbitrary points within the field of view. The obtained cross-sectional curve was then subjected to a filter treatment with λc: 0.008 mm to obtain a waviness curve, from which the arithmetic mean wavelength Wλa, arithmetic mean tilt angle WΔa, and arithmetic mean waviness Wa were obtained. This measurement was performed at three arbitrary fields of view, and the average values were used as the arithmetic mean wavelength Wλa, arithmetic mean tilt angle WΔa, and arithmetic mean waviness Wa of Example 1.
[0048] The arithmetic mean wavelength Wλa and the arithmetic mean tilt angle WΔa are parameters not described in ISO 25178, but are parameters described in the Multi-File Analysis Application Reference Manual for the VK-X3000 Series Laser Microscope manufactured by Keyence Corporation, and can be calculated using software provided with the laser microscope.
[0049] The developed area ratio Sdr of the matte surface (the surface that has been plated) is measured as follows. In accordance with the provisions of ISO 25178, the matte surface of the copper foil was analyzed using a laser microscope VK-X3000 manufactured by Keyence Corporation, and data analysis was performed using the software provided with the laser microscope. The objective lens magnification of the laser microscope was 100x, the scan mode was laser confocal, the measurement size was 2048 × 1536, the measurement quality was "High Precision," and the pitch was 0.06 μm.
[0050] The developed area ratio Sdr was calculated by performing the following reference surface correction, smoothed image processing, and filter processing on the measurement data using the attached analysis software, and then performing calculations on an arbitrary 100 μm × 100 μm field of view. Such measurements were performed on three arbitrary fields of view, and the average value was used as the developed area ratio Sdr of Example 1. Reference surface correction: entire surface; Smoothing: 3 × 3, Gaussian; Filter processing: L filter 0.025 mm
[0051] <Evaluation of Formability> The copper foil of Example 1 was subjected to an Erichsen test. The copper foil was cut to prepare square test pieces with sides of 100 mm. The prepared test pieces were then subjected to an Erichsen test in accordance with the standard test specified in JIS B7729 (2005). The test was performed so that the plated surface was the side that would be pressed convexly. The test (pressing) was temporarily interrupted when the pressing depth reached 1 mm and 2 mm, and the surface of the test piece was visually observed to confirm whether cracks had occurred in the copper foil. The results are shown in Table 1.
[0052] The results of the Erichsen test shown in Table 1 are evaluated based on the following evaluation criteria: A (pass): No cracks occurred when the indentation depth reached 2 mm B (pass): Cracks occurred when the indentation depth reached 2 mm C (fail): Cracks occurred when the indentation depth reached 1 mm
[0053] <Adhesion Test> An adhesion test was conducted on the copper foil of Example 1 to evaluate its adhesion to resin. A pressure-sensitive adhesive was applied in the form of a film to the matte surface (plated surface) of the copper foil, and then the film was heated at 80°C for 3 minutes to volatilize the solvent in the pressure-sensitive adhesive, forming a 30 μm thick pressure-sensitive adhesive layer. A polyimide film was attached to the pressure-sensitive adhesive layer on the copper foil in a 22°C environment, and pressure-bonded using a peel test pressure roller APR-97 manufactured by Imada Co., Ltd., and then allowed to stand for 30 minutes. This resulted in the copper foil and polyimide film being bonded via the pressure-sensitive adhesive layer.
[0054] The adhesive used was Finetack CT-5030, an acrylic adhesive manufactured by DIC Corporation. The polyimide film used was Upilex®-S, product number 25S, manufactured by UBE Corporation. The copper foil and polyimide film bonded together were cut to prepare square test pieces with sides of 20 mm. These test pieces were then placed in a thermo-hygrostat chamber at a temperature of 85°C and a relative humidity of 85% RH. The surfaces of the test pieces were visually observed after 48 hours and 96 hours to determine whether or not delamination had occurred between the copper foil and the polyimide film (i.e., whether or not there was any blistering). The results are shown in Table 1.
[0055] The results of the adhesion test shown in Table 1 are evaluated based on the following evaluation criteria: A (pass): No peeling occurred after 96 hours B (pass): Peeling occurred after 96 hours C (fail): Peeling occurred after 48 hours
[0056] (Examples 2 to 13) The copper foils were evaluated in the same manner as in Example 1, except that the plating conditions were changed as shown in Table 1 and the surface shape of the copper foil was adjusted as shown in Table 1. The results are shown in Table 1.
[0057] Comparative Example 1 Except for not being subjected to plating treatment, the copper foil was evaluated in the same manner as in Example 1. The results are shown in Table 1. In the adhesion test, a polyimide film was adhered to the matte surface of the copper foil.
[0058] (Comparative Example 2) Except for not being subjected to plating treatment, the copper foil was evaluated in the same manner as in Example 1. The results are shown in Table 1. In the adhesion test, a polyimide film was adhered to the shiny side of the copper foil.
[0059] Comparative Example 3 A commercially available non-roughened rolled copper foil (tough pitch copper) was used instead of the non-rust-proof electrolytic copper foil DR-WS foil, and the copper foil was evaluated in the same manner as in Example 1, except that no plating treatment was performed. The results are shown in Table 1. The thickness of the non-roughened rolled copper foil was 10 μm.
[0060] Comparative Example 4 A roughened copper foil FV-WS manufactured by Furukawa Electric Co., Ltd. was used instead of the non-rust-proof electrolytic copper foil DR-WS, and the copper foil was evaluated in the same manner as in Example 1, except that no plating treatment was performed. The results are shown in Table 1. The thickness of the roughened copper foil FV-WS was 10 μm.
[0061] Comparative Example 5 A copper foil having a thickness of 10 μm was produced according to the method described in Example 1 of Japanese Patent No. 6910381. The obtained copper foil was used instead of the non-anticorrosive electrolytic copper foil DR-WS foil, and the copper foil was evaluated in the same manner as in Example 1, except that no plating treatment was performed. The results are shown in Table 1.
[0062] (Comparative Examples 6 to 9) Evaluation of the copper foils was carried out in the same manner as in Example 1, except that the plating conditions were changed as shown in Table 1 and the surface shape of the copper foil was adjusted as shown in Table 1. The results are shown in Table 1.
[0063] As can be seen from Table 1, the copper foils of Examples 1 to 13 were less susceptible to cracking and had excellent formability, as well as excellent adhesion. In contrast, the copper foils of Comparative Examples 1 to 7 and 9 were prone to cracking and had insufficient formability because the surface shape of the copper foil (arithmetic mean wavelength Wλa and arithmetic mean tilt angle WΔa) did not satisfy the requirements of the present invention. Furthermore, Comparative Example 8 had good formability but insufficient adhesion.
[0064] DESCRIPTION OF SYMBOLS 1... Composite film 10... Copper foil 10a... Surface of copper foil 20... Resin layer
Claims
1. A copper foil, wherein at least one of the two surfaces of the copper foil is an uneven surface having projections and recesses, and the uneven surface has an arithmetic mean wavelength Wλa of 10 μm or more and 80 μm or less, and an arithmetic mean tilt angle WΔa of 0.4° or more and 4° or less.
2. The copper foil according to claim 1, wherein the arithmetic mean waviness Wa of the uneven surface is 0.07 μm or more and 0.45 μm or less.
3. The copper foil according to claim 1, wherein the developed area ratio Sdr of the uneven surface is 0.007 or more and 0.200 or less.
4. The copper foil according to claim 1, having a thickness of 5 μm or more and 30 μm or less.
5. A composite film comprising the copper foil according to any one of claims 1 to 4 and a resin layer laminated on one or both of the two surfaces of the copper foil.
6. The composite film according to claim 5, which is used as an EMI countermeasure film.
Citation Information
Patent Citations
Copper foil for resin bonding, and its manufacturing method
JP2003239082A
Treated copper foil for copper-clad laminated board and copper-clad laminated board obtained by adhering the treated copper foil onto insulating resin substrate, and printed circuit board using the copper-clad laminated board
JP2011219790A
Electromagnetic wave shield sheet and printed wiring board
JP2016143751A
Roughened copper foil, copper-clad laminate and print circuit board
JP2022085378A
Electrolytic copper foil, copper-clad laminate, printed wiring board, production method therefor, electronic device, and production method therefor
WO2018207786A1