Method for hardening a friction ring
Patent Information
- Application Number
- PCT/AT2023/060409
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-11-23
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional methods for hardening friction rings in brake discs are unable to achieve uniform high hardness while maintaining corrosion protection and avoiding deformation, leading to uneven wear and increased fine dust emissions.
A laser hardening process is used to treat the friction layer of friction rings made of cast iron, incorporating elements like phosphorus, chromium, copper, manganese, and silicon, which are altered by temperature to enhance hardness and corrosion resistance, ensuring homogeneous hardening and maintaining the material's microstructure.
The method achieves a higher hardness of up to 600 HV, ensuring even wear and reduced fine dust emissions, while being cost-effective and simple to implement, without compromising the structural integrity of the brake disc.
Smart Images

Figure AT2023060409_24102024_PF_FP_ABST
Abstract
Description
[0001] Process for hardening a friction ring
[0002] The invention relates to a method for hardening a friction ring, in which in a first step a friction ring is provided which has a friction layer and in a second step a laser beam is guided over the entire surface of the friction layer with the aid of a laser.
[0003] The invention further relates to a friction ring produced by a method according to the invention.
[0004] Brake discs are known from the prior art and are used primarily in disc brakes. Here, a moving, e.g. rotating element such as a vehicle wheel is firmly connected to the brake disc. In order to brake the brake disc or the moving element, at least one surface of the brake disc is contacted by brake pads, so that friction is created between the brake disc and the brake pad. This friction causes the kinetic energy to be converted into thermal energy and thus a deceleration of the brake disc and thus of the moving element. The brake pads are usually arranged on brake blocks that can be pressed optionally onto the brake disc.
[0005] Brake discs typically have a friction ring comprising at least one friction layer that comes into contact with the brake pads during braking. The friction ring is generally held in place by a retaining element surrounded by the friction ring. Known friction rings are made of cast iron, particularly gray cast iron. Such friction rings have a hardness in the range of approximately 190-230 HV (Vickers hardness).
[0006] A higher hardness of the friction rings, particularly of the friction layer, is desirable as this leads to less wear and therefore less emission of fine dust. However, hardening a friction ring using conventional hardening processes is not or hardly possible as there is a risk that the friction ring will be deformed by the hardening process and the structure of the friction ring will be adversely changed. Furthermore, it is hardly possible to harden the friction layer of a friction ring homogeneously using conventional processes, so that the friction layer has essentially the same hardness over its entire surface and depth. However, this is important in order to enable even wear of the friction layer.Uneven wear due to an uneven hardness distribution in the friction layer leads to excessively rapid wear of the friction layer and undesirable noises during braking, which significantly limits the comfort of a vehicle equipped with the friction ring, for example.
[0007] In order to reduce wear and the fine dust generated by friction rings, additional layers of harder material can be applied to the friction ring, thereby increasing the hardness of the friction layer exposed to friction. However, applying additional materials to a friction ring is complex and expensive, so this process is only used for friction rings in higher vehicle classes. GB 2373792 A discloses a process in which the surface of the friction layer of a brake disc is hardened using a laser and a process gas. The disadvantage of this process, however, is that only relatively low degrees of hardness and insufficient corrosion protection can be achieved. Furthermore, the use of a process gas is necessary.
[0008] It is therefore an object of the invention to provide a method for hardening a friction ring that enables uniform, high hardening of the friction layer of the friction ring while simultaneously providing good corrosion protection. In particular, the method should be simple and cost-effective.
[0009] According to the invention, in a method of the type mentioned at the outset, the friction layer comprises phosphorus, chromium, copper, manganese, silicon and / or zinc after the second step, so that the surface of the friction layer is hardened by the laser beam. The friction ring or the friction layer is hardened using a laser hardening process, wherein the elements phosphorus, chromium, copper, manganese, silicon and / or zinc are changed in the second step by the effect of temperature in such a way that both greater hardness and improved corrosion protection are achieved after the second step. This enables homogeneous hardening of the friction layer to the desired depth and is comparatively cost-effective. In addition, it has been found that the microstructure of the material of the friction ring, e.g. cast iron, is not adversely affected by the hardening process according to the invention.It is preferably provided that the friction layer comprises phosphorus, chromium, copper, manganese, silicon and / or zinc before the second step. Due to the temperature and speed of the laser hardening, the properties of the chemical elements phosphorus, chromium, copper, manganese, silicon and / or zinc are changed in the edge zone of the substrate in such a way that their valence is altered by up to 10 points. This results in an improvement in corrosion protection within the hardened zone. In this case, the friction layer therefore already comprises the elements phosphorus, chromium, copper, manganese, silicon and / or zinc before hardening with the aid of the laser.
[0010] Alternatively or additionally, it is preferably provided that phosphorus, chromium, copper, manganese, silicon and / or zinc are added to the friction layer during the second step. The elements phosphorus, chromium, copper, manganese, silicon and / or zinc are preferably added to the friction layer via the laser. Due to the high temperature introduced by the laser, for example, over 600 °C, the chemical elements are embedded in the melt and remain in the molten substrate. After the second step or after cooling, this provides improved corrosion protection.
[0011] The friction ring provided in the first step is preferably made substantially from cast iron, particularly preferably grey cast iron, for example EN GJL 150. The friction layer is preferably an upper layer of the friction ring and likewise preferably consists of the same material as the rest of the friction ring, for example cast iron. Cast iron and in particular grey cast iron are known and comparatively inexpensive materials that are well suited as the base material of a friction ring and for the hardening according to the invention. The friction ring can be produced in the first step using a known method. The friction ring can, for example, be cast.
[0012] The laser device used according to the invention preferably has hardening optics. Furthermore, preferably during the second method step, i.e. during hardening, the temperature at the laser's point of action, i.e. the surface of the friction layer, is recorded coaxially to the laser beam using a sensor. The temperature determined in this way can preferably be used as a basis for controlling the laser device, e.g. for adjusting the laser power and / or the laser speed (scanning speed). This is particularly advantageous when brake discs of different sizes or properties are to be hardened, for which suitable processing parameters for the laser device are not yet available.
[0013] It is preferably provided that the laser beam is guided over the surface of the friction layer at a speed of 1 to 100 m / min or 0.2 to 100 m / min, preferably 0.5 to 50 m / min, particularly preferably 1 to 30 m / min, particularly preferably 1 to 2 m / min, in particular approximately 1.5 m / min. The laser speed or scanning speed is determined on the surface of the friction layer. At these speeds, there is a particularly good relationship between the production speed and the quality of the hardening, in particular when the material of the friction ring is made of cast iron, e.g. gray cast iron. In particular, this makes it possible to ensure essentially homogeneous hardening down to a sufficient depth of approximately 0.5 to 1 mm. In principle, the hardness achieved is reduced at higher speeds, but the production speed is increased.
[0014] Likewise, the method according to the invention produces a structural change in the friction layer. The chemical elements present in the substrate, preferably silicon and / or manganese, shift the phase of martensite formation, transforming the normally present hard phases into a tough structure. This transformation is a factor in ensuring that, in addition to the desired effects of wear resistance, no unwanted hardness deviations occur in the friction layer. The shift is achieved via the hardening rate as described. This, in turn, means that the desired effects of improved comfort and reduced particulate matter do not have a negative impact on the strength of the brake disc, which would occur with pure hardening, e.g., using a laser.
[0015] It is preferably provided that the friction layer after the second step comprises silicon and / or manganese.
[0016] For example, it is provided that the friction layer before the second step comprises phosphorus, chromium, manganese, silicon, copper and / or zinc. Preferably, the friction layer before the second step comprises 0.05 to 1.12 wt.% phosphorus, 0.1 to 0.4 wt.% chromium, 0.2 to 0.8 wt.% copper and / or 0.2 to 0.8 wt.% zinc. Particularly preferably, the friction layer before the second step comprises 0.5 to 1.00 wt.% phosphorus, 0.2 to 0.3 wt.% chromium, 0.4 to 0.6 wt.% copper and / or 0.4 to 0.6 wt.% zinc.
[0017] Alternatively or additionally, it is preferably provided that silicon, chromium, and / or manganese are added to the friction layer during the second step. For example, a material comprising 10 to 20 wt.% manganese, 8 to 16 wt.% silicon, and / or 6 to 12 wt.% chromium can be added. Particularly preferably, the material comprises 12 to 18 wt.% manganese, 10 to 14 wt.% silicon, and / or 8 to 10 wt.% chromium.
[0018] Furthermore, the material preferably consists of 10 to 20 wt.% manganese, 8 to 16 wt.% silicon, 6 to 12 wt.% chromium, and the remainder iron. Particularly preferably, the material consists of 12 to 18 wt.% manganese, 10 to 14 wt.% silicon, 8 to 10 wt.% chromium, and the remainder iron. Apart from any minor impurities, no further components are provided. This composition results in a particularly hard friction surface with good corrosion protection.
[0019] The following table shows the preferred pairs of laser speed and temperature that enable particularly good hardening of the friction layer. Here, the laser speed is the speed of the laser dot on the surface of the friction layer, and the temperature is the temperature measured on the surface of the friction layer caused by the laser:
[0020] In the selected assignments it is possible to use the pure
[0021] To avoid the formation of martensite, which is detrimental to the strength of the brake disc.
[0022] Furthermore, it is preferably provided that the power of the laser during processing of the surface of the friction layer is 4000 to 7000 watts, preferably 5000 to 6000 watts. This power makes it possible to harden the friction layer to a depth of approximately 0.5 to 1 mm to a hardness of approximately 500 to 600 HV or more. This laser power is particularly advantageous at the above-mentioned laser beam speeds.
[0023] The axis of the laser beam, which is guided over the surface of the friction layer, is preferably arranged substantially perpendicular to the surface of the friction layer. This enables uniform processing of the friction layer. Preferably, the axis of the laser beam is arranged substantially perpendicular to the surface of the friction layer throughout the entire hardening process.
[0024] The distance between the surface of the friction layer and the front of the laser device (working distance) is preferably between approximately 100 mm and 400 mm, particularly preferably between 200 and 300 mm, in particular approximately 250 mm.
[0025] To ensure in a simple manner that the entire surface of the friction layer is hardened, it is preferably provided that the laser beam is guided in a meandering pattern over the surface of the friction layer, as seen in plan view. This allows, on the one hand, the surface of the friction layer to be systematically scanned and, on the other hand, no area of the surface of the friction layer is exposed (directly) to the laser beam more than once, thereby shortening the duration of laser hardening without negatively affecting the quality of the hardening.
[0026] Alternatively, it is preferably provided that the laser beam is guided in a ring shape over the surface of the friction layer, as seen in plan view. This is particularly preferred if the friction layer of the friction ring is ring-shaped. If the laser beam on the surface of the friction layer is smaller than the width of the friction layer, it is particularly preferably provided that the laser beam is guided in a spiral shape over the surface of the friction layer. This enables rapid processing of the friction layer, which at the same time ensures that the entire friction layer is covered completely. The laser beam can be started at the largest diameter of the friction ring or the surface of the friction ring and then guided in the direction of the smallest diameter of the friction ring or the surface of the friction ring, or vice versa at the smallest diameter of the friction ring orthe surface of the friction ring and then guided in the direction of the largest diameter of the friction ring or the surface of the friction ring.
[0027] During processing, either the laser device (either in whole or in part) can be moved relative to the friction ring, or the friction ring can be moved relative to the laser device. A combination of these two movements is also possible.
[0028] Furthermore, it is preferably provided that the friction layer is cooled in a third step. Particularly preferably, the friction layer is actively cooled. This further improves hardening. Cooling can be achieved, for example, using compressed air. In most cases, however, active cooling of the friction layer is not necessary, since the heat can be dissipated from the heated areas sufficiently quickly due to the only local heating.
[0029] For the efficient hardening of brake discs of conventional size, it is preferably provided that the width of the laser beam, measured on the surface of the friction layer, is 5 to 50 mm, particularly preferably 20 to 35 mm.
[0030] Particularly good results are achieved with the hardening process according to the invention if, as is preferably provided, regions of the surface of the friction layer which have already been processed with the laser beam in a first operation are processed again by the laser beam in a second operation. It is particularly preferably provided that the laser beam in the second operation overlaps with the regions of the friction layer processed in the first operation. During laser hardening, the center of the processed surface is usually hardened particularly well, whilst the edge regions of the processed surface are hardened less well. In order to prevent this effect from leading to inhomogeneous hardening of the friction layer, the edge region can be exposed to the laser beam again, as a result of which the hardening in this region is improved. The overlap can be, for example, 10% to 50%, preferably 20% to 40%, of the width of the laser beam or.of the surface of the friction surface machined by the laser beam. If the width of the laser beam remains unchanged between the first and second pass, 10% to 50%, or 20% to 40%, of the width of the surface machined in the first pass is machined again in a second pass. This allows for sufficient hardening, even in the edge areas, while simultaneously reducing the machining speed as little as possible.
[0031] Overlapping can be achieved particularly easily with meandering or spiral processing.
[0032] The invention further relates to a friction ring manufactured by a method according to the invention. The friction ring has at least one hardened friction layer. Preferably, the friction ring has two friction layers formed on opposite surfaces of the friction ring.
[0033] The invention further relates to a brake disc comprising a friction ring produced by a method according to the invention. The friction ring can, for example, be connected to a retaining element, which is preferably arranged in a central opening of the friction ring.
[0034] The invention is explained in more detail below with reference to an exemplary embodiment shown schematically in the drawing. In this drawing: Fig. 1 shows a brake element according to the invention, Fig. 2 is a schematic representation of a method according to the invention for hardening a friction ring in a side view, Fig. 3 is a schematic representation of a friction ring during a first method according to the invention in a plan view, Fig. 4 is a schematic representation of a friction ring during a second method according to the invention in a plan view, Fig. 5 is a first diagram of the hardness distribution in a friction ring according to the invention and Fig. 6 is a second diagram of the hardness distribution in a friction ring according to the invention. Fig. 1 shows a brake disc 1 according to the invention, comprising a friction ring 2 and a holding element 3. The friction ring 1 has a friction layer 4 formed on both sides.During operation, during a braking process, the friction layer 4 interacts with a brake pad, e.g., brake blocks, to decelerate the moving brake disc 1. With this design, brake pads can be arranged on both sides of the friction ring 2 in order to exert pressure on both sides of the brake disc 1 and thus brake it.
[0035] Fig. 2 shows a schematic representation of a method according to the invention for hardening a friction layer 4 according to the invention of the friction ring 2. The friction ring 2 is designed, for example, as gray cast iron, in particular as EN GJL 150. A laser device 5 processes the friction layer 4 of the friction ring 2 with a laser beam 6. The axis of the laser beam 6 runs perpendicular to the surface of the friction layer 4. The friction layer 4 has, for example, a depth 7 (measured from the surface) of 0.6 mm. The laser beam 6 hardens the friction layer 4 at least to a depth 7, for example to at least 600 HV. The elements phosphorus, chromium, manganese, silicon, copper and / or zinc are preferably arranged in the friction layer. Furthermore, preferably, alternatively or additionally, the elements phosphorus, chromium, manganese, silicon, copper and / or zinc are added to the friction layer during laser hardening, for example via the laser beam 6.This creates a particularly hard friction layer 4 which is both less susceptible to wear and less susceptible to corrosion and therefore has a longer service life. Fig. 3 shows a schematic plan view of a friction ring 2 with a friction layer 4, wherein a laser beam 6 is guided along a meandering path 8 over part of the friction layer 4 of the friction ring 2. According to this pattern, the laser beam 6 can be guided over the entire friction layer 4. Since the laser beam 6 is wider on the surface of the friction layer 4 than the path 8 shown, the entire friction layer 4 can be machined as shown.
[0036] Fig. 4 schematically shows a friction ring 2 with a friction layer 4 in a plan view, wherein a laser beam 6 is guided along a spiral path 8 over a part of the friction layer 4 of the friction ring 2.
[0037] Fig. 5 shows a first diagram of the hardness of a friction ring 2 according to the invention in the region of the friction layer 4. The distance from the surface of the friction layer 4, i.e. the depth, is plotted on the x-axis 9, which ranges from 0 to 0.7 mm. The y-axis 10 shows the microhardness (HV0.05) in a range from 200 to 1000 HV. It can be seen that the hardness is constantly (well) above 600 HV down to a depth 7 of approximately 0.56 mm, with hardness levels of up to approximately 1,000 HV being reached. The hardness curve begins at approximately 900 HV, measured just below the surface. The hardness then increases slightly over time, reaching a minimum of approximately 700 HV at a depth of approximately 0.12 mm. Subsequently, the hardness increases again to a range of approximately 900 HV to 1,000 HV, until it decreases again at a depth of more than 0.5 mm.Near the surface, the hardness is 910 HV, at a depth of 0.2 mm, 920 HV, and at a depth of 0.5 mm, 960 HV. In this example, a friction layer of a friction ring made of gray cast iron (EN GJL 150) was hardened using a laser power of 6000 W and a laser scanning speed of 1.5 m / min. The friction layer of the friction ring already contained silicon and manganese before the second step.
[0038] Fig. 6 shows a second hardness curve of a friction ring 2 according to the invention in the area of the friction layer 4. The hardness curve starts at 600 HV determined just below the surface of the friction layer, increases to approximately 1,000 HV, and drops again at a depth of approximately 0.43 mm. In this example, too, a constant microhardness of more than 600 HV is achieved down to a depth of more than 0.5 mm. On or near the surface, the hardness is 620 HV, at a depth of 0.2 mm it is 980 HV, and at a depth of 0.5 mm it is 850 HV. In this example, a friction layer of a friction ring made of gray cast iron (EN GJL 150) was hardened with a laser power of 6,000 W and a laser scanning speed of 1.5 m / min. The friction layer of the friction ring already comprised silicon and manganese before the second step.
[0039] The distance between the front of the laser device and the surface of the friction layer 4 of the friction ring 2 was approximately 250 mm in the examples shown in Fig. 5 and Fig. 6. During the hardening process shown in Fig. 5, only one laser path was used, whereas during the hardening process shown in Fig. 6, an overlap was created.
Claims
Patent claims:
1. A method for hardening a friction ring (2), in which in a first step a friction ring (2) is provided which has a friction layer (4), and in a second step a laser beam (6) is guided over the entire surface of the friction layer (4) with the aid of a laser (5), characterized in that the friction layer (4) after the second step comprises phosphorus, chromium, copper, manganese, silicon and / or zinc, the surface of the friction layer (4) being hardened by the laser beam (6).
2. Method according to claim 1, characterized in that the friction layer (4) before the second step comprises phosphorus, chromium, manganese, silicon, copper and / or zinc.
3. Method according to claim 2, characterized in that the friction layer (4) before the second step comprises 0.05 to 1.12 wt.% phosphorus, 0.1 to 0.4 wt.% chromium, 0.2 to 0.8 wt.% copper and / or 0.2 to 0.8 wt.% zinc.
4. Method according to claim 1, 2 or 3, characterized in that manganese, silicon and / or chromium is added to the friction layer (4) during the second step.
5. The method according to claim 4, characterized in that a material comprising 10 to 20 wt.% manganese, 8 to 16 wt.% silicon and / or 6 to 12 wt.% chromium is supplied to the friction layer (4) during the second step.
6. Method according to one of claims 1 to 5, characterized in that the laser beam (6) is provided with a Speed of 1 to 100 m / min over the surface of the friction layer (4).
7. Method according to one of claims 1 to 6, characterized in that the friction layer (4) after the second step comprises silicon and / or manganese.
8. Method according to one of claims 1 to 7, characterized in that the power of the laser (5) during the processing of the surface of the friction layer (4) is 4000 to 7000 watts.
9. Method according to one of claims 1 to 8, characterized in that the laser beam (6) is guided in a meandering manner over the surface of the friction layer (4).
10. Method according to one of claims 1 to 9, characterized in that the friction layer (4) is cooled in a third step.
11. Method according to one of claims 1 to 10, characterized in that the width of the laser beam (6), measured on the surface of the friction layer (4), is 5 to 50 mm.
12. Method according to one of claims 1 to 11, characterized in that areas of the surface of the friction layer (4) which have already been machined with the laser beam (8) in a first operation are machined again by the laser beam (8) in a second operation.
13. Friction ring manufactured according to a method according to any one of claims 1 to 12.
14. Brake disc comprising a friction ring according to claim
Citation Information
Patent Citations
Laser hardening of disc brake rotors
GB2373792A
Method for manufacturing friction material
EP3812441A1