Single crystal furnace and preparation method for monocrystalline silicon

By setting up multiple water cooling zones and mass flow controllers in the single crystal furnace to control the temperature and flow of the water cooling zone, the problem of unstable water cooling jacket temperature during the growth of single crystal silicon rods is solved, and the longitudinal temperature gradient of the thermal field is achieved. Stable, reducing defects in single crystal silicon.

WO2024221935A1PCT designated stage expired Publication Date: 2024-10-31XIAN ESWIN MATERIAL TECHNOLOGY CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/136676
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-12-06
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The temperature of the water-cooling jacket in the existing single crystal furnace is unstable, resulting in many defects in the single crystal silicon rod during the growth process. The type and distribution of defects are affected by the longitudinal temperature gradient change of the thermal field and cannot be effectively controlled.

Method used

Design a single crystal furnace that contains multiple independent water-cooling zones and mass flow controllers. By controlling the cooling water flow and temperature of different water-cooling zones respectively, the longitudinal temperature gradient of the thermal field is stabilized and adapted to changes in the position of the crucible and the single crystal. The growth process of silicon rods.

Benefits of technology

By zoning the temperature and flow rate of the water-cooling zone, the longitudinal temperature gradient changes during crystal growth are reduced, the smooth transition of the temperature zone is achieved, the defects of single crystal silicon are reduced, and the preparation quality is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023136676_31102024_PF_FP_ABST
    Figure CN2023136676_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A single crystal furnace and a preparation method for monocrystalline silicon, relating to the technical field of semiconductor manufacturing. The single crystal furnace comprises a furnace body; a crucible supporting assembly is arranged in the furnace body; a crucible is arranged at the upper part of the crucible supporting assembly; a flow guide tube is arranged directly above the crucible; a heater is arranged between the inner wall of the furnace body and the periphery of the crucible; a seed crystal pulling mechanism is arranged at the top of the furnace body. The single crystal furnace further comprises: a water cooling structure located on the side of the flow guide tube away from the crucible supporting assembly, the water cooling structure comprising a plurality of mutually independent water cooling areas that are sequentially arranged in the direction away from the flow guide tube; and a mass flow controller used for respectively controlling the flow and the temperature of cooling water in different water cooling areas.
Need to check novelty before this filing date? Find Prior Art

Description

Single crystal furnace and method for preparing single crystal silicon

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims priority to Chinese Patent Application No. 202310473614.0 filed in China on April 27, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the field of semiconductor manufacturing technology, and in particular to a single crystal furnace and a method for preparing single crystal silicon. Background Art

[0004] Polycrystalline silicon is the primary raw material for producing solar photovoltaic and semiconductor products. The Czochralski (Cz) process is one of the most commonly used methods for producing single-crystal silicon. High-purity solid polycrystalline silicon feedstock is melted in a crucible in a crystal growth furnace (i.e., a single crystal furnace) to form a melt. A seed crystal is lowered into contact with the molten melt in a rotating crucible by a seed crystal lifting mechanism. The seed crystal is then pulled out according to a specific process, and the melt solidifies around the seed crystal to form a single-crystal silicon rod.

[0005] The defect properties of single crystal silicon rods are sensitively dependent on the growth and cooling conditions of the crystal. The single crystal furnace includes a water-cooling jacket, which can achieve the stability of the longitudinal temperature gradient of the thermal field. However, in the related art, in the melting stage, due to the low position of the crucible, the temperature of the water-cooling jacket is also relatively low, resulting in a large longitudinal temperature gradient of the thermal field, and volatiles are easily accumulated on the water-cooling jacket; and in the later stage of the single crystal equal diameter, due to the high position of the crucible, the crystal is closer to the water-cooling jacket, resulting in an increase in the temperature of the water-cooling jacket, so the longitudinal temperature gradient of the thermal field is small. In other words, the change in the position of the single crystal silicon rod makes the temperature of the water-cooling jacket not constant, so the longitudinal temperature gradient of the thermal field is also unstable, and the stable growth of the single crystal silicon rod cannot be guaranteed, resulting in more defects in the prepared single crystal silicon.

[0006] Summary of the Invention

[0007] In order to solve the above technical problems, the present disclosure provides a single crystal furnace and a method for preparing single crystal silicon, which can reduce defects in the prepared single crystal silicon.

[0008] In order to achieve the above objectives, the technical solutions adopted in the embodiments of the present disclosure are:

[0009] A single crystal furnace, comprising a furnace body, a crucible support assembly disposed within the furnace body, a crucible disposed on top of the crucible support assembly, a guide tube disposed directly above the crucible, a heater disposed between an inner wall of the furnace body and an outer periphery of the crucible, a seed crystal pulling mechanism disposed on top of the furnace body, and the single crystal furnace further comprising:

[0010] a water cooling structure located on a side of the guide tube away from the crucible support assembly, the water cooling structure comprising a plurality of mutually independent water cooling zones, the plurality of water cooling zones being sequentially arranged in a direction away from the guide tube;

[0011] Mass flow controllers are used to control the flow and temperature of cooling water in different water cooling zones.

[0012] In some embodiments, the mass flow controller is specifically used to control the temperature of the cooling water in the multiple water cooling zones to gradually decrease and / or the flow rate of the cooling water in the multiple water cooling zones to gradually increase in a direction away from the guide tube before the growth of the single crystal silicon rod.

[0013] In some embodiments, the temperature difference between adjacent water cooling zones is 1.5°C-2.5°C.

[0014] In some embodiments, the mass flow controller is specifically used to control the temperature of the cooling water in the multiple water-cooling zones to gradually decrease, and / or the flow rate of the cooling water in the multiple water-cooling zones to gradually increase as the crucible moves in a direction close to the guide tube during the growth of the single crystal silicon rod.

[0015] In some embodiments, the mass flow controller is also used to obtain a defect evaluation result of the single crystal silicon rod after the growth of the single crystal silicon rod is completed, and adjust the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod.

[0016] In some embodiments, the mass flow controller is specifically used to reduce the temperature of the cooling water in the water cooling zone and / or increase the flow rate of the cooling water in the water cooling zone when V-rich defects exist in the single crystal silicon rod; and to increase the temperature of the cooling water in the water cooling zone and / or reduce the flow rate of the cooling water in the water cooling zone when N-rich defects exist in the single crystal silicon rod.

[0017] In some embodiments, the water cooling structure includes three water cooling zones.

[0018] The present disclosure also provides a method for preparing single crystal silicon, which is applied to the single crystal furnace described above. The method includes:

[0019] Before the growth of the single crystal silicon rod, the temperature of the cooling water in the multiple water cooling zones is gradually reduced and / or the flow rate of the cooling water in the multiple water cooling zones is gradually increased in a direction away from the guide tube by controlling the mass flow controller.

[0020] In some embodiments, the method further comprises:

[0021] During the growth of the single crystal silicon rod, as the crucible moves in a direction close to the guide tube, the temperature of the cooling water in the multiple water cooling zones is gradually reduced and / or the flow rate of the cooling water in the multiple water cooling zones is gradually increased by controlling the mass flow controller.

[0022] In some embodiments, the method further comprises:

[0023] After the growth of the single crystal silicon rod is completed, obtaining a defect evaluation result of the single crystal silicon rod;

[0024] The flow rate and / or temperature of the cooling water in the water cooling zone is adjusted according to the defect evaluation result of the single crystal silicon rod.

[0025] In some embodiments, adjusting the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod includes:

[0026] When V-rich defects exist in the single crystal silicon rod, lowering the temperature of the cooling water in the water cooling zone and / or increasing the flow rate of the cooling water in the water cooling zone;

[0027] When N-rich defects exist in the single crystal silicon rod, the temperature of the cooling water in the water cooling zone is increased and / or the flow rate of the cooling water in the water cooling zone is reduced.

[0028] The beneficial effects of the present disclosure are:

[0029] In this embodiment, the water cooling structure includes multiple independent water cooling zones, and the mass flow controller can respectively control the flow rate and temperature of the cooling water in different water cooling zones. In this way, during the growth of single crystal silicon rods, by zoning the temperature and flow rate of different water cooling zones, the longitudinal temperature gradient change during crystal growth can be reduced, and a smooth transition of temperature zones can be achieved, thereby achieving the stability of the longitudinal temperature gradient of the thermal field, thereby reducing the defects of the prepared single crystal silicon. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] FIG1 is a schematic structural diagram of a single crystal furnace according to an embodiment of the present disclosure;

[0031] FIG2 is a schematic flow chart showing a method for preparing single crystal silicon according to an embodiment of the present disclosure.

[0032] Reference numerals 1 single crystal silicon rod; 2 water cooling structure; 3 guide tube; 4 heater; 5 graphite crucible; 6 quartz crucible; 7 silicon solution; 8 crucible support assembly; 9 mass flow controller; 10 cooling water supply unit. DETAILED DESCRIPTION

[0033] To further clarify the objectives, technical solutions, and advantages of the embodiments of the present disclosure, the technical solutions of the embodiments of the present disclosure are described below in conjunction with the accompanying drawings. It should be understood that the described embodiments are only a portion of the embodiments of the present disclosure, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the described embodiments of the present disclosure are intended to fall within the scope of protection of the present disclosure.

[0034] The defect properties of single crystals are sensitively dependent on the growth and cooling conditions of the crystals, so the types and distribution of defects formed during the growth process can be controlled by adjusting the thermal environment near the growth interface.

[0035] Growth defects are classified into several categories: vacancy-type defects and interstitial-type defects. They result from the accumulation of vacancy or interstitial point defects that begin with a concentration exceeding the equilibrium concentration. The formation of growth defects is closely related to the V / G ratio, where V is the growth rate and G is the temperature gradient of the crystal near the growth interface. Vacancy-type defects form when the V / G ratio exceeds a critical value, while interstitial defects form when the V / G ratio falls below a critical value. Therefore, the type, size, and density of defects present in a crystal grown in a specific thermal zone are influenced by the pull rate. The cooling rate of the crystal is controlled between the solidification temperature and approximately 1000°C, a range within which defect nuclei form and grow during the thermal treatment as molten silicon solidifies into a single crystal. In this way, silicon interstitials or vacancies diffuse toward the sides of the ingot or are accelerated to coalesce, suppressing the supersaturation of interstitials or vacancies below the critical value at which accumulation occurs. Temperature variations across regions of an ingot grown using the Czochralski method are minimized within a temperature range of 1000°C to 1100°C. More specifically, the temperature variation within the single crystal silicon ingot within regions of the ingot having a temperature between 1000°C and 1100°C does not exceed 20°C / cm. Optionally, temperature variation is controlled vertically at the periphery of the ingot. Furthermore, when the ingot is at a temperature between 1000°C and 1100°C, the temperature of the growing ingot is controlled such that the temperature gradient between the center and periphery of the ingot differs by no more than 1.5°C / cm.

[0036] A key component in a single crystal furnace is the water-cooling jacket, which stabilizes the longitudinal temperature gradient of the thermal field. However, the water-cooling jacket designed in the related art has a simple structure, and the cooling water flow and temperature cannot be adjusted, making it impossible to maximize the cooling effect. During the melting stage, due to the low position of the crucible, the heat of the crucible has less impact on the water-cooling jacket, causing the water-cooling jacket temperature to be low, resulting in a large longitudinal temperature gradient in the thermal field and volatiles easily accumulating on the water-cooling jacket. In the later stage of the single crystal isodiameter, due to the high position of the crucible and the proximity of the crystal to the water-cooling jacket, the heat of the crucible affects the water-cooling jacket, causing the temperature of the water-cooling jacket to rise and the longitudinal temperature gradient of the thermal field to be small. In other words, the change in the position of the single crystal makes the temperature of the water-cooling jacket not constant, and therefore the longitudinal temperature gradient of the thermal field is also unstable, making it impossible to ensure the stable growth of the single crystal. In addition, the water-cooling jacket is only a component through which the cooling water flows. There is no control measure for the cooling water in the water-cooling jacket. Therefore, the cooling water flowing through the water-cooling jacket is not fully utilized and most of it is wasted. The temperature of the water-cooling jacket cannot be controlled at a constant temperature, and the longitudinal temperature gradient of the thermal field required for single crystal growth cannot be controlled.

[0037] The present disclosure provides a single crystal furnace and a method for preparing single crystal silicon, which can reduce defects in the prepared single crystal silicon.

[0038] The present disclosure provides a single crystal furnace, as shown in FIG1 , comprising a furnace body, a crucible support assembly 8 disposed in the furnace body, a crucible disposed on the upper portion of the crucible support assembly 8, the crucible comprising a graphite crucible 5 and a quartz crucible 6 located within the graphite crucible 5, a silicon solution 7 contained in the quartz crucible 6, a guide tube 3 disposed directly above the crucible, a heater 4 disposed between the inner wall of the furnace body and the outer periphery of the crucible, a seed crystal pulling mechanism disposed on the top of the furnace body, and the single crystal furnace further comprising:

[0039] a water-cooling structure 2 located on a side of the guide tube 3 away from the crucible support assembly 8, the water-cooling structure 2 comprising a plurality of mutually independent water-cooling zones, the plurality of water-cooling zones being sequentially arranged in a direction away from the guide tube 3;

[0040] The mass flow controller (MFC) 9 is used to control the flow rate and temperature of the cooling water in different water cooling zones.

[0041] In this embodiment, the water-cooling structure 2 includes multiple independent water-cooling zones, and the mass flow controller 9 can respectively control the flow and temperature of the cooling water in different water-cooling zones. In this way, during the growth process of the single crystal silicon rod 1, by zoning the temperature and flow of different water-cooling zones, the longitudinal temperature gradient change during crystal growth can be reduced, and a smooth transition of the temperature zones can be achieved, thereby achieving the stability of the longitudinal temperature gradient of the thermal field, thereby reducing the defects of the prepared single crystal silicon.

[0042] In this embodiment, the water cooling structure 2 may include two independent water cooling zones, three independent water cooling zones, or more independent water cooling zones.

[0043] In this embodiment, the mass flow controller 9 is connected to the cooling water supply unit 10, and can control the flow rate and temperature of the cooling water in different water cooling zones; in this way, before the growth of the single crystal silicon rod 1, the mass flow controller 9 can set the flow rate and temperature of the cooling water in different water cooling zones; during the growth process of the single crystal silicon rod 1, as the position of the single crystal silicon rod 1 changes, the mass flow controller 9 can also adjust the flow rate and temperature of the cooling water in different water cooling zones to achieve the stability of the longitudinal temperature gradient of the thermal field, thereby reducing the defects of the prepared single crystal silicon.

[0044] In this embodiment, the mass flow controller 9 can control the temperature of the cooling water in the multiple water-cooling zones to gradually decrease and / or the flow rate of the cooling water in the multiple water-cooling zones to gradually increase before the growth of the single crystal silicon rod 1 in a direction away from the guide tube 3, so as to achieve a longitudinal temperature gradient of the thermal field. In this embodiment, only the temperature of the cooling water in the multiple water-cooling zones can be adjusted, or only the flow rate of the cooling water in the multiple water-cooling zones can be adjusted, or both the temperature and flow rate of the cooling water in the multiple water-cooling zones can be adjusted. Among them, a decrease in the temperature of the cooling water in the water-cooling zone will reduce the ambient temperature near the water-cooling zone, and an increase in the temperature of the cooling water in the water-cooling zone will increase the ambient temperature near the water-cooling zone; a decrease in the flow rate of the cooling water in the water-cooling zone will increase the ambient temperature near the water-cooling zone, and an increase in the flow rate of the cooling water in the water-cooling zone will reduce the ambient temperature near the water-cooling zone.

[0045] In some embodiments, as shown in FIG1 , the water-cooling structure 2 includes three independent water-cooling zones: zone A, zone B, and zone C. Before the growth of the single crystal silicon rod 1 begins, the mass flow controller 9 controls the temperatures of the cooling water introduced into zones A, B, and C to be different. The temperature of the cooling water in zone A is higher than that in zone B, and the temperature of the cooling water in zone B is higher than that in zone C. This achieves a longitudinal temperature gradient in the thermal field.

[0046] The temperature difference between adjacent water-cooling zones may be 1.5-2.5°C, such as 1.5°C, 1.6°C, 1.7°C, 1.8°C, 1.9°C, 2.0°C, 2.1°C, 2.2°C, 2.3°C, 2.4°C or 2.5°C. Optionally, the temperature difference between adjacent water-cooling zones may be 2.0°C, which is beneficial to reducing the formation of defects in the single crystal silicon rod 1.

[0047] Of course, the cooling water flow rate in zone A can also be controlled to be lower than that in zone B, and the cooling water flow rate in zone B can be controlled to be lower than that in zone C, which also helps to achieve the longitudinal temperature gradient of the thermal field.

[0048] During the growth of the single crystal silicon rod 1, as the seed crystal pulling mechanism pulls the single crystal silicon rod 1, the position of the crucible gradually moves up and approaches the water-cooling structure 2. The heat of the crucible will affect the heat of the water-cooling structure 2. In order to ensure the stability of the longitudinal temperature gradient of the thermal field, it is necessary to adjust the temperature and flow rate of the cooling water in multiple water-cooling zones. Specifically, as the crucible moves in the direction close to the guide tube 3, the temperature of the cooling water in the multiple water-cooling zones is controlled to gradually decrease, and / or the flow rate of the cooling water in the multiple water-cooling zones is gradually increased. This can offset the influence of the heat of the crucible and is beneficial to the stability of the longitudinal temperature gradient of the thermal field.

[0049] The mass flow controller 9 can be set in advance for the flow rates and temperatures of Zone A, Zone B, and Zone C corresponding to the different positions of the single crystal silicon rod 1 during the growth process of the single crystal silicon rod 1. For example, position 1 corresponds to: the flow rate of Zone A is L1 and the temperature is T1; the flow rate of Zone B is L2 and the temperature is T2; the flow rate of Zone C is L3 and the temperature is T3. Position 2 corresponds to: the flow rate of Zone A is L4 and the temperature is T4; the flow rate of Zone B is L5 and the temperature is T5; the flow rate of Zone C is L6 and the temperature is T6. Then, when the single crystal silicon rod 1 moves to position 1, the flow rate of Zone A can be controlled to be L1 and the temperature to be T1; the flow rate of Zone B can be controlled to be L2 and the temperature to be T2; the flow rate of Zone C can be controlled to be L3 and the temperature to be T3. When the single crystal silicon rod 1 moves to position 2, the flow rate of Zone A can be controlled to be L4 and the temperature to be T4; the flow rate of Zone B can be controlled to be L5 and the temperature to be T5; the flow rate of Zone C can be controlled to be L6 and the temperature to be T6.

[0050] In this embodiment, only the temperature of the cooling water in the multiple water-cooling zones may be adjusted, only the flow rate of the cooling water in the multiple water-cooling zones may be adjusted, or both the temperature and flow rate of the cooling water in the multiple water-cooling zones may be adjusted.

[0051] In some embodiments, the mass flow controller 9 is also used to obtain the defect evaluation result of the single crystal silicon rod 1 after the growth of the single crystal silicon rod 1 is completed, and adjust the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod 1.

[0052] The defect properties of a single crystal are related to the crystal's cooling conditions. By adjusting the thermal environment near the growth interface, the types and distribution of defects formed during the growth process can be controlled. Therefore, after the growth of the single crystal silicon ingot 1 is completed, the flow rate and / or temperature of the cooling water in the water-cooling zone can be adjusted based on the defects of the single crystal silicon ingot 1 to control and optimize the longitudinal temperature gradient of the thermal field. Adjustment can be performed on only the temperature of the cooling water in the multiple water-cooling zones, on only the flow rate of the cooling water in the multiple water-cooling zones, or on both the temperature and flow rate of the cooling water in the multiple water-cooling zones.

[0053] In some embodiments, the mass flow controller 9 is specifically used to reduce the temperature of the cooling water in the water cooling zone and / or increase the flow rate of the cooling water in the water cooling zone when V-rich defects exist in the single crystal silicon rod 1; and to increase the temperature of the cooling water in the water cooling zone and / or reduce the flow rate of the cooling water in the water cooling zone when N-rich defects exist in the single crystal silicon rod 1.

[0054] When a V-rich defect exists in the single crystal silicon rod 1, it indicates that the ambient temperature of the growth interface of the single crystal silicon rod 1 is relatively high. Therefore, the ambient temperature of the growth interface of the single crystal silicon rod 1 can be lowered by lowering the temperature of the cooling water in the water cooling zone and / or increasing the flow rate of the cooling water in the water cooling zone, thereby improving the V-rich defect; when an N-rich defect exists in the single crystal silicon rod 1, it indicates that the ambient temperature of the growth interface of the single crystal silicon rod 1 is relatively low. Therefore, the ambient temperature of the growth interface of the single crystal silicon rod 1 can be increased by increasing the temperature of the cooling water in the water cooling zone and / or decreasing the flow rate of the cooling water in the water cooling zone, thereby improving the N-rich defect.

[0055] The present disclosure also provides a method for preparing single crystal silicon, which is applied to the single crystal furnace described above. The method includes:

[0056] Before the single crystal silicon rod 1 grows, the temperature of the cooling water in the multiple water cooling zones is gradually reduced and / or the flow rate of the cooling water in the multiple water cooling zones is gradually increased by controlling the mass flow controller 9 in a direction away from the guide tube 3 .

[0057] In this embodiment, the water-cooling structure 2 includes multiple independent water-cooling zones, and the mass flow controller 9 can respectively control the flow and temperature of the cooling water in different water-cooling zones. In this way, during the growth process of the single crystal silicon rod 1, by zoning the temperature and flow of different water-cooling zones, the longitudinal temperature gradient change during crystal growth can be reduced, and a smooth transition of the temperature zones can be achieved, thereby achieving the stability of the longitudinal temperature gradient of the thermal field, thereby reducing the defects of the prepared single crystal silicon.

[0058] In this embodiment, the mass flow controller 9 is connected to the cooling water supply unit 10, and can control the flow rate and temperature of the cooling water in different water cooling zones; in this way, before the growth of the single crystal silicon rod 1, the mass flow controller 9 can set the flow rate and temperature of the cooling water in different water cooling zones; during the growth process of the single crystal silicon rod 1, as the position of the single crystal silicon rod 1 changes, the mass flow controller 9 can also adjust the flow rate and temperature of the cooling water in different water cooling zones to achieve the stability of the longitudinal temperature gradient of the thermal field, thereby reducing the defects of the prepared single crystal silicon.

[0059] In this embodiment, the mass flow controller 9 can control the cooling water in the multiple water-cooling zones to gradually decrease in temperature and / or gradually increase in flow rate before the growth of the single crystal silicon ingot 1, in a direction away from the flow guide tube 3, thereby achieving a longitudinal temperature gradient in the thermal field. In this embodiment, only the temperature of the cooling water in the multiple water-cooling zones can be adjusted, only the flow rate of the cooling water in the multiple water-cooling zones can be adjusted, or both the temperature and flow rate of the cooling water in the multiple water-cooling zones can be adjusted.

[0060] In some embodiments, the method further comprises:

[0061] During the growth of the single crystal silicon rod, as the crucible moves in a direction close to the guide tube, the temperature of the cooling water in the multiple water cooling zones is gradually reduced and / or the flow rate of the cooling water in the multiple water cooling zones is gradually increased by controlling the mass flow controller.

[0062] During the growth of the single crystal silicon rod 1, as the seed crystal pulling mechanism pulls the single crystal silicon rod 1, the position of the crucible gradually moves up and approaches the water-cooling structure 2. The heat of the crucible will affect the heat of the water-cooling structure 2. In order to ensure the stability of the longitudinal temperature gradient of the thermal field, it is necessary to adjust the temperature and flow rate of the cooling water in multiple water-cooling zones. Specifically, as the crucible moves in the direction close to the guide tube 3, the temperature of the cooling water in the multiple water-cooling zones is controlled to gradually decrease, and / or the flow rate of the cooling water in the multiple water-cooling zones is gradually increased. This can offset the influence of the heat of the crucible and is beneficial to the stability of the longitudinal temperature gradient of the thermal field.

[0063] In this embodiment, only the temperature of the cooling water in the multiple water-cooling zones may be adjusted, only the flow rate of the cooling water in the multiple water-cooling zones may be adjusted, or both the temperature and flow rate of the cooling water in the multiple water-cooling zones may be adjusted.

[0064] In some embodiments, as shown in FIG2 , the method further includes:

[0065] Step 101: After the growth of the single crystal silicon rod is completed, obtaining a defect evaluation result of the single crystal silicon rod;

[0066] Step 102: adjusting the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod.

[0067] The defect properties of a single crystal are related to the crystal's cooling conditions. By adjusting the thermal environment near the growth interface, the types and distribution of defects formed during the growth process can be controlled. Therefore, after the growth of the single crystal silicon ingot 1 is completed, the flow rate and / or temperature of the cooling water in the water-cooling zone can be adjusted based on the defects of the single crystal silicon ingot 1 to control and optimize the longitudinal temperature gradient of the thermal field. Adjustment can be performed on only the temperature of the cooling water in the multiple water-cooling zones, on only the flow rate of the cooling water in the multiple water-cooling zones, or on both the temperature and flow rate of the cooling water in the multiple water-cooling zones.

[0068] In some embodiments, adjusting the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod includes:

[0069] When V-rich defects exist in the single crystal silicon rod, lowering the temperature of the cooling water in the water cooling zone and / or increasing the flow rate of the cooling water in the water cooling zone;

[0070] When N-rich defects exist in the single crystal silicon rod, the temperature of the cooling water in the water cooling zone is increased and / or the flow rate of the cooling water in the water cooling zone is reduced.

[0071] When a V-rich defect exists in the single crystal silicon rod 1, it indicates that the ambient temperature of the growth interface of the single crystal silicon rod 1 is relatively high. Therefore, the ambient temperature of the growth interface of the single crystal silicon rod 1 can be lowered by lowering the temperature of the cooling water in the water cooling zone and / or increasing the flow rate of the cooling water in the water cooling zone, thereby improving the V-rich defect; when an N-rich defect exists in the single crystal silicon rod 1, it indicates that the ambient temperature of the growth interface of the single crystal silicon rod 1 is relatively low. Therefore, the ambient temperature of the growth interface of the single crystal silicon rod 1 can be increased by increasing the temperature of the cooling water in the water cooling zone and / or decreasing the flow rate of the cooling water in the water cooling zone, thereby improving the N-rich defect.

[0072] It should be noted that the various embodiments in this specification are described in a progressive manner. Similar parts between the various embodiments can be referred to in conjunction with each other. Each embodiment focuses on the differences from other embodiments. In particular, since the embodiments are generally similar to the product embodiments, the description is relatively simple. For relevant parts, refer to the partial description of the product embodiments.

[0073] Unless otherwise defined, the technical or scientific terms used in this disclosure should have the usual meanings understood by persons of ordinary skill in the field to which this disclosure belongs. The words "first", "second" and similar terms used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Words such as "include" or "comprise" mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Words such as "connect" or "connected" are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0074] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being “on” or “under” another element, it can be “directly on” or “under” the other element or intervening elements may be present.

[0075] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0076] The above description is merely a specific embodiment of the present disclosure, but the scope of protection of the present disclosure is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this disclosure should be included in the scope of protection of the present disclosure. Therefore, the scope of protection of the present disclosure should be based on the scope of protection of the claims.

Claims

1. A single crystal furnace, comprising a furnace body, a crucible support assembly is arranged in the furnace body, a crucible is arranged on the upper part of the crucible support assembly, a guide tube is arranged directly above the crucible, a heater is arranged between the inner wall of the furnace body and the outer periphery of the crucible, a seed crystal pulling mechanism is arranged on the top of the furnace body, and the single crystal furnace also includes: A water cooling structure located at a side of the guide tube away from the crucible support assembly, the water cooling structure comprising a plurality of water cooling zones that are independent of each other, and the plurality of water cooling zones are sequentially arranged in a direction away from the guide tube; Mass flow controllers are used to control the flow and temperature of cooling water in different water cooling zones.

2. The single crystal furnace according to claim 1, wherein: The mass flow controller is specifically used to control the temperature of the cooling water in the multiple water cooling zones to gradually decrease and / or the flow rate of the cooling water in the multiple water cooling zones to gradually increase in a direction away from the guide tube before the growth of the single crystal silicon rod.

3. The single crystal furnace according to claim 2, wherein: The temperature difference between adjacent water cooling zones is 1.5°C-2.5°C.

4. The single crystal furnace according to claim 1, wherein: The mass flow controller is specifically used to control the temperature of the cooling water in the multiple water cooling zones to gradually decrease and / or the flow rate of the cooling water in the multiple water cooling zones to gradually increase as the crucible moves in a direction close to the guide tube during the growth of the single crystal silicon rod.

5. The single crystal furnace according to claim 1, wherein: The mass flow controller is also used to obtain a defect evaluation result of the single crystal silicon rod after the growth of the single crystal silicon rod is completed, and adjust the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod.

6. The single crystal furnace according to claim 5, wherein: The mass flow controller is specifically used to reduce the temperature of the cooling water in the water cooling zone and / or increase the flow rate of the cooling water in the water cooling zone when V-rich defects exist in the single crystal silicon rod; and to increase the temperature of the cooling water in the water cooling zone and / or reduce the flow rate of the cooling water in the water cooling zone when N-rich defects exist in the single crystal silicon rod.

7. The single crystal furnace according to claim 1, wherein: The water cooling structure includes three water cooling zones.

8. A method for preparing single crystal silicon, applied to the single crystal furnace according to any one of claims 1 to 7, the method comprising: Before the growth of the single crystal silicon rod, the mass flow control The device controls the temperature of the cooling water in the multiple water-cooling zones to gradually decrease, and / or the flow rate of the cooling water in the multiple water-cooling zones to gradually increase.

9. The method for preparing single crystal silicon according to claim 8, wherein: The method further comprises: When the single crystal silicon rod grows, as the crucible moves in a direction close to the guide tube, the temperature of the cooling water in the multiple water cooling zones is gradually reduced and / or the flow rate of the cooling water in the multiple water cooling zones is gradually increased by controlling the mass flow controller.

10. The method for preparing single crystal silicon according to claim 8, wherein: The method further comprises: After the growth of the single crystal silicon rod is completed, obtaining a defect evaluation result of the single crystal silicon rod; The flow rate and / or temperature of the cooling water in the water cooling zone is adjusted according to the defect evaluation result of the single crystal silicon rod.

11. The method for preparing single crystal silicon according to claim 10, wherein: The adjusting the flow rate and / or temperature of the cooling water in the water cooling zone according to the defect evaluation result of the single crystal silicon rod comprises: When the single crystal silicon rod has a V-rich defect, lowering the temperature of the cooling water in the water cooling zone and / or increasing the flow rate of the cooling water in the water cooling zone; When N-rich defects exist in the single crystal silicon rod, the temperature of cooling water in the water cooling zone is increased and / or the flow rate of cooling water in the water cooling zone is reduced.

Citation Information

Patent Citations

  • Crystal growth furnace

    CN112877776A

  • Single crystal furnace and preparation method of monocrystalline silicon

    CN116479522A

  • Method for producing silicon single crystal and device therefor

    JP1994247788A