Silicon single crystal manufacturing method, and silicon single crystal manufacturing apparatus

The silicon single crystal manufacturing method and apparatus address the challenge of stabilizing oxygen concentration by using a heater with uneven heat distribution and varying thermal conductivity in the heat insulating material, ensuring stable convection modes and improved efficiency without altering conventional equipment, thus enhancing yield and reducing waste.

WO2024224694A1PCT designated stage expired Publication Date: 2024-10-31SUMCO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/047291
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-12-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing silicon single crystal manufacturing methods using the MCZ method face challenges in stabilizing oxygen concentration due to random convection modes in the silicon melt, which are influenced by the thermal environment and equipment variations, requiring complex adjustments to heating sections and component configurations.

Method used

A silicon single crystal manufacturing method and apparatus that employs a cylindrical heater with uneven heat generation distribution and a heat insulating material with varying thermal conductivity, using high and low resistance support electrodes to fix the convection mode of the silicon melt by controlling the magnetic field's impact on the crucible's temperature distribution, allowing for stable oxygen concentration without significant changes to conventional equipment.

Benefits of technology

This approach stabilizes the convection mode and oxygen concentration in silicon single crystals, improving yield, energy efficiency, and reducing waste while maintaining a conventional device configuration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023047291_31102024_PF_FP_ABST
    Figure JP2023047291_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This silicon single crystal manufacturing method comprises, using a silicon single crystal manufacturing apparatus comprising a cylindrical heater surrounding a crucible, and first to fourth support electrodes supporting the heater, the heater comprising first to fourth heat generation parts, the first support electrode connecting the first and second heat generation parts to the positive electrode of a power supply, the second support electrode connecting the second and third heat generation parts to the negative electrode of the power supply, the third support electrode connecting the third and fourth heat generation parts to the positive electrode, the fourth support electrode connecting the fourth and first heat generation parts to the negative electrode, and at least one support electrode out of the first to fourth support electrodes being composed of a thin support electrode at least a part of which having a thickness smaller than that of the remaining support electrodes: heating the crucible, while being rotated, in a state in which the heat generation distribution of the heater is non-uniform to generate a silicon melt; and starting application of a horizontal magnetic field to the silicon melt to grow a silicon single crystal.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon single crystal manufacturing method and silicon single crystal manufacturing apparatus

[0001] The present invention relates to a method for producing a silicon single crystal and an apparatus for producing a silicon single crystal.

[0002] As a method for producing silicon single crystals, the MCZ (magnetically coupled Czochralski) method, in which a horizontal magnetic field is applied to a silicon melt, is sometimes used. When a horizontal magnetic field is applied to a silicon melt using the MCZ method, the direction of convection in the silicon melt in a virtual plane perpendicular to the direction of application of the horizontal magnetic field may be clockwise (hereinafter, sometimes referred to as a "right vortex mode") or counterclockwise (hereinafter, sometimes referred to as a "left vortex mode").

[0003] Whether the convection mode is the right-handed vortex mode or the left-handed vortex mode is random, and the concentration of oxygen incorporated into the silicon single crystal varies depending on the convection mode and the furnace environment. In order to obtain a silicon single crystal with a stable oxygen concentration, it is important to control the convection mode of the silicon melt during pulling. For this reason, various methods for controlling the convection mode of the silicon melt in the crucible have been studied (see, for example, Patent Document 1).

[0004] Patent Document 1 discloses a method for eliminating variations in oxygen concentration due to the convection mode by making the thermal environment in the furnace of a manufacturing apparatus asymmetrical with respect to the central axis of the crucible, thereby fixing the convection mode to one of a right-handed vortex mode and a left-handed vortex mode. Specifically, Patent Document 1 discloses a method using a heating unit in which the heat generation amount of a first heating region on one side in the left-right direction of an imaginary plane perpendicular to the direction of application of a horizontal magnetic field in the silicon melt is set to a different value from the heat generation amount of a second heating region on the other side.

[0005] Patent Literature 1 discloses that one method for differentiating the heat generation amounts of the first and second heating regions is to vary the contact resistance of a power supply unit that supplies power to the heat-generating portions of the first and second heating regions. The methods for differentiating the contact resistance include varying the total number of electrical resistance adjustment members interposed between the terminals and electrodes connected to the heat-generating portions of the first and second heating regions, varying the fastening force of fastening means that fasten the terminals and electrodes connected to the heat-generating portions of the first and second heating regions, and varying the material or thickness of adhesive layers that join the terminals and electrodes connected to the heat-generating portions of the first and second heating regions.

[0006] Patent document 1 also discloses another method for differentiating the heat generation amounts of the first heating area and the second heating area, which is to make at least one of the length and total number of slits provided in the first and second heating areas different.

[0007] Japanese Patent Application Laid-Open No. 2022-102247

[0008] However, in the method of varying the contact resistance value disclosed in Patent Document 1, when the contact resistance value is set to a desired value, the convection mode of the silicon melt may change from the desired state due to the influence of variations in work, deterioration of components, etc. Furthermore, the method of varying at least one of the length and total number of slits disclosed in Patent Document 1 requires a heating unit with a special shape.

[0009] The present invention aims to provide a silicon single crystal manufacturing method and silicon single crystal manufacturing apparatus that can manufacture silicon single crystals with a stable oxygen concentration without significantly changing the configuration of conventional apparatuses.

[0010] The method for producing a silicon single crystal of the present invention is a method for producing a silicon single crystal by using a silicon single crystal production apparatus to pull up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, the silicon single crystal production apparatus comprising: a crucible for accommodating the silicon melt; a heater formed in a cylindrical shape surrounding the crucible and arranged so that the central axis of the cylinder is positioned coaxially with the central axis of the crucible; and first, second, third and fourth support electrodes formed in a rod shape from a conductive material and supporting the heater, the heater comprising a first heating portion, a second heating portion, a third heating portion and a fourth heating portion having the same heating characteristics and arranged in a circumferential direction of the crucible; the first support electrode connecting the first heating portion and the second heating portion to a positive electrode of a power source; the second support electrode connecting the second heating portion and the third heating portion to a negative electrode of the power source or a ground; the electrodes connect the third heating element and the fourth heating element to the positive electrode, and the fourth supporting electrode connects the fourth heating element and the first heating element to the negative electrode or the earth, and at least one of the first supporting electrode, the second supporting electrode, the third supporting electrode, and the fourth supporting electrode is configured as a thin-diameter supporting electrode having at least a portion thinner than the remaining supporting electrodes; and the method for producing a silicon single crystal includes a silicon melt producing step of heating the silicon raw material in the rotating crucible while the heater has a non-uniform heat generation distribution to produce the silicon melt, a magnetic field applying step of starting to apply the horizontal magnetic field to the silicon melt, and a growing step of growing the silicon single crystal by pulling up a seed crystal immersed in the silicon melt once the direction of convection of the silicon melt in an imaginary plane perpendicular to a central magnetic field line of the horizontal magnetic field has been fixed in one direction.

[0011] In the silicon single crystal manufacturing method of the present invention, it is preferable that the silicon single crystal manufacturing apparatus is provided with a cylindrical heat insulating material that surrounds the heater and is configured to cause the heat extraction distribution to the heater to be non-uniform.

[0012] In the method for producing a silicon single crystal of the present invention, it is preferable that the heat insulating material is configured so as to have a uniform thermal conductivity throughout, and is arranged so that the central axis of the heat insulating material is not positioned on the same axis as the central axis of the crucible.

[0013] In the method for producing a silicon single crystal of the present invention, it is preferable that the heat insulating material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and that the central axis of the heat insulating material is positioned on the same axis as the central axis of the crucible.

[0014] In the method for producing a silicon single crystal of the present invention, the first support electrode, the second support electrode, the third support electrode, the fourth support electrode, and the heat insulating material are preferably configured such that, when R (rpm) is the rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt and T (minutes) is the time from the start of application of the horizontal magnetic field until the horizontal magnetic field, having a magnetic field strength that fixes the direction of convection, acts on the silicon melt, the maximum heating temperature position, where the heating temperature for the crucible is the highest, in a plan view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field line and includes the central axis of the crucible, and the angle θ (°) formed by the first horizontal imaginary line and a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position satisfies the following formula (1): θ=360×R×T (1)

[0015] The silicon single crystal manufacturing apparatus of the present invention is a silicon single crystal manufacturing apparatus that pulls up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, and includes: a crucible that contains the silicon melt; a heater that is formed in a cylindrical shape surrounding the crucible and is arranged so that the central axis of the cylinder is positioned on the same axis as the central axis of the crucible; and first, second, third, and fourth support electrodes that are formed in a rod shape from a conductive material and support the heater, and the heater has first, second, third, and fourth heating portions that have the same heating characteristics and are arranged in a circumferential direction of the crucible. The device is provided with a heating section, wherein the first support electrode connects the first heating section and the second heating section to the positive electrode of a power source, the second support electrode connects the second heating section and the third heating section to the negative electrode of the power source or earth, the third support electrode connects the third heating section and the fourth heating section to the positive electrode, and the fourth support electrode connects the fourth heating section and the first heating section to the negative electrode or earth, and at least one of the first support electrode, the second support electrode, the third support electrode and the fourth support electrode is composed of a thin-diameter support electrode having at least a portion thinner than the remaining support electrodes.

[0016] The silicon single crystal manufacturing apparatus of the present invention preferably includes a cylindrical heat insulating material surrounding the heater, the heat insulating material being configured to provide a non-uniform heat extraction distribution to the heater.

[0017] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the insulating material is configured so that the thermal conductivity is uniform throughout, and that the central axis of the insulating material is not positioned on the same axis as the central axis of the crucible.

[0018] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the insulating material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and that the central axis of the insulating material is positioned on the same axis as the central axis of the crucible.

[0019] In the silicon single crystal manufacturing apparatus of the present invention, the first support electrode, the second support electrode, the third support electrode, the fourth support electrode, and the heat insulating material are preferably configured such that, when R (rpm) is the rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt and T (minutes) is the time from the start of application of the horizontal magnetic field until the horizontal magnetic field, having a magnetic field strength that fixes the direction of convection, acts on the silicon melt, the maximum heating temperature position, where the heating temperature for the crucible is the highest, in a plan view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field line of the horizontal magnetic field and includes the central axis of the crucible, and the angle θ (°) formed by the first horizontal imaginary line and a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position satisfies the following formula (2): θ=360×R×T (2)

[0020] FIG. 1 is a longitudinal sectional view showing a schematic configuration of a silicon single crystal manufacturing apparatus according to an embodiment; FIG. 2 is a plan view schematic showing a heater, a heat insulator, and a magnetic field application unit according to an embodiment; FIG. 3 is a perspective view of a heater according to an embodiment; FIG. 4 is a side view showing a low-resistance support electrode and a high-resistance support electrode according to an embodiment; FIG. 5 is an equivalent circuit diagram of a heater and a power supply unit according to an embodiment; FIG. 6 is an explanatory diagram of a preferred configuration of first to fourth support electrodes and heat insulators according to an embodiment, and a plan view showing a maximum heating temperature position; FIG. 7 is an explanatory diagram of a preferred configuration of first to fourth support electrodes and heat insulators according to an embodiment, and a graph showing the relationship between the elapsed time from the start of application of a horizontal magnetic field and magnetic field strength; FIG. 8 is a block diagram of a main part of a silicon single crystal manufacturing apparatus according to an embodiment; FIG. 9 is a flowchart showing a method for manufacturing a silicon single crystal according to an embodiment; FIG. 10 is a plan view showing the position of a high-temperature melt region according to an example; FIG. 11 is a graph showing the incidence of each convection mode in a comparative example and examples 1 to 8 according to an example;

[0021] [Embodiments] [Configuration of Silicon Single Crystal Manufacturing Apparatus] First, the configuration of a silicon single crystal manufacturing apparatus according to an embodiment of the present invention will be described. FIG. 1 is a vertical cross-sectional view showing the schematic configuration of the silicon single crystal manufacturing apparatus. FIG. 2 is a plan view showing a heater, a heat insulating material, and a magnetic field application unit. FIG. 3 is a perspective view of the heater. FIG. 4 is a side view showing a low-resistance support electrode and a high-resistance support electrode. FIG. 5 is an equivalent circuit diagram of a heater and a power supply unit. FIG. 6A is an explanatory diagram of a preferred configuration of first to fourth support electrodes and heat insulating material, and is a plan view showing the maximum heating temperature position. FIG. 6B is an explanatory diagram of a preferred configuration of first to fourth support electrodes and heat insulating material, and is a graph showing the relationship between the elapsed time from the start of application of a horizontal magnetic field and the magnetic field strength. FIG. 7 is a block diagram of the main parts of the silicon single crystal manufacturing apparatus.

[0022] 1 is an apparatus for producing a silicon single crystal SM by the MCZ method, and pulls up a silicon single crystal SM having a neck portion SM1, a shoulder portion SM2, a body portion SM3, and a tail portion (not shown) while applying a horizontal magnetic field to a silicon melt M. The silicon single crystal production apparatus 1 includes a chamber 2 that forms an outer shell, a crucible 3 disposed in the center of the chamber 2, a heater 4 disposed around the inside of the crucible 3, and a temperature measurement unit 15.

[0023] The crucible 3 has a double structure consisting of an outer graphite crucible 3A and an inner quartz crucible 3B, and the quartz crucible 3B contains silicon melt M. The graphite crucible 3A and the quartz crucible 3B are cylindrical containers with bottoms, and are circular in plan view from above. The crucible 3 is fixed to the upper end of a support shaft 5 that can rotate and move up and down.

[0024] The heater 4 is a graphite heater formed in a substantially cylindrical shape and arranged around the crucible 3. A cylindrical heat insulating material 6 is provided outside the heater 4 along the inner surface of the chamber 2. The heat insulating material 6 is configured so that the thermal conductivity of the entire material is uniform.

[0025] A pulling shaft 7 is disposed above the crucible 3 and is coaxial with the support shaft 5. The pulling shaft 7 is formed of a wire or the like. A seed crystal SC is attached to the lower end of the pulling shaft 7.

[0026] A cylindrical thermal shield 8 is disposed within the chamber 2, surrounding the silicon single crystal SM being grown above the silicon melt M in the crucible 3. The thermal shield 8 blocks radiant heat from the silicon melt M, the sidewall of the crucible 3, and the heater to the silicon single crystal SM being grown, thereby suppressing a temperature rise in the silicon single crystal SM.

[0027] A gas inlet 2A is provided at the top of the chamber 2 to introduce an inert gas such as argon gas into the chamber 2. An exhaust port 2B is provided at the bottom of the chamber 2 to suck and exhaust gas from the chamber 2 by driving a vacuum pump (not shown).

[0028] The temperature measurement unit 15 measures the temperatures of the first measurement point P1 and the second measurement point P2. The radial positions of the first measurement point P1 and the second measurement point P2 are between the outer peripheral surface of the silicon single crystal SM to be grown and the inner peripheral surface of the opening of the thermal shield 8. As will be described later, the convection mode of the silicon melt M can be confirmed by measuring the temperatures of the first measurement point P1 and the second measurement point P2. For example, if the convection direction of the silicon melt M is fixed clockwise in FIG. 1 by heating the silicon melt M with the heater 4, that is, if the convection mode of the silicon melt M becomes a right-handed vortex mode, the measured temperature of the first measurement point P1 will be higher than the measured temperature of the second measurement point P2. On the other hand, if the convection direction of the silicon melt M is fixed counterclockwise by heating the silicon melt M with the heater 4, that is, if the convection mode becomes a left-handed vortex mode, the measured temperature of the first measurement point P1 will be lower than the measured temperature of the second measurement point P2.

[0029] The temperature measurement unit 15 includes a pair of reflecting units 15A and a pair of radiation thermometers 15B. The reflecting units 15A are installed inside the chamber 2. The reflecting units 15A are preferably installed so that the angle between the reflecting surface 15C and the horizontal plane is 40° or more and 50° or less. The radiation thermometers 15B are installed outside the chamber 2. The radiation thermometers 15B receive radiant light L incident through a quartz window 2C (see FIG. 1 ) provided in the chamber 2, and measure the temperatures of the first measurement point P1 and the second measurement point P2 in a non-contact manner.

[0030] As shown in FIG. 2 , the silicon single crystal manufacturing apparatus 1 further includes a magnetic field application unit 16. The magnetic field application unit 16 includes a first magnetic body 16A and a second magnetic body 16B, each of which is configured as an electromagnetic coil. The first magnetic body 16A and the second magnetic body 16B are disposed outside the chamber 2 so as to face each other across the crucible 3. The magnetic field application unit 16 applies a horizontal magnetic field such that, in a plan view, a central magnetic field line 16C passing through the central axis of the coil intersects with the central axis 3C of the crucible 3 (hereinafter, sometimes referred to as the "crucible central axis 3C") and is directed from the second magnetic body 16B toward the first magnetic body 16A (the upward direction indicated by the arrow indicating the central magnetic field line 16C in FIG. 2 , and the direction from the front to the back of the page in FIG. 1 ).

[0031] The heater 4 is arranged so that its central axis 4C (hereinafter sometimes referred to as the "heater central axis 4C") is coaxial with the crucible central axis 3C. On the other hand, the heat insulating material 6 is arranged so that its central axis 6C (hereinafter sometimes referred to as the "heater central axis 4C") is not coaxial with the crucible central axis 3C and the heater central axis 4C. In other words, the heater 4 is arranged so that the gap between the heater 4 and the crucible 3 is uniform in the circumferential direction of the crucible 3. Furthermore, the heat insulating material 6 is arranged so that the gap between the heater 4 and the heat insulating material 6 is nonuniform in the circumferential direction of the heater 4. Due to this arrangement of the heater 4 and the heat insulating material 6, the heat removal distribution from the heater 4 by the heat insulating material 6 becomes nonuniform in the circumferential direction of the crucible 3.

[0032] As shown in Figures 2 and 3, the heater 4 includes a heat generating portion 40, which is a cylindrical graphite heater. The heat generating portion 40 is formed with a uniform thickness over the entire circumference. The heat generating portion 40 has a plurality of upper slits 41 extending downward from the upper end and a plurality of lower slits 42 extending upward from the lower end, which are formed alternately in the circumferential direction. Each upper slit 41 and each lower slit 42 has the same width and the same cutting depth in the vertical direction. The spacing between the upper slits 41 and the lower slits 42 is also uniform over the entire circumference of the heater 4.

[0033] The heating section 40 is divided into four parts by a first vertical imaginary plane VF1 and a second vertical imaginary plane VF2 that are orthogonal to each other and include the heater central axis 4C. The heating section 40 includes a first heating section 40A, a second heating section 40B, a third heating section 40C, and a fourth heating section 40D, each of which has the same heating characteristics. The same heating characteristics mean that the same parts generate heat at the same temperature when the same amount of power is supplied. The first heating section 40A to the fourth heating section 40D have the same total number of upper slits 41 and lower slits 42. In this embodiment, each of the first heating section 40A to the fourth heating section 40D has two upper slits 41 and three lower slits 42, for a total of five upper slits 41 and five lower slits 42. Thus, the resistance values ​​of the first heating section 40A to the fourth heating section 40D, which have the same shape, are the same. The heater 4 is disposed so that the heater central axis 4C is coaxial with the crucible central axis 3C and so that the central magnetic field line 16C overlaps the first vertical imaginary plane VF1 in plan view. Note that the heater 4 may be disposed so that the central magnetic field line 16C does not overlap the first vertical imaginary plane VF1 in plan view.

[0034] The silicon single crystal manufacturing apparatus 1 includes a power supply unit 9 that supplies power to the heat generating unit 40. The power supply unit 9 includes a first terminal 91A, a second terminal 91B, a third terminal 91C, and a fourth terminal 91D, a first support electrode 92A, a second support electrode 92B, a third support electrode 92C, and a fourth support electrode 92D, and four nuts 93A, 93B, 93C, and 93D. The first terminal 91A to the fourth terminal 91D are arranged at 90° intervals along the circumferential direction of the heat generating unit 40. The first terminal 91A to the fourth terminal 91D extend downward from the lower end of a portion of the heat generating unit 40 that is partitioned by the two lower slits 42, and are formed integrally with the heat generating unit 40. The first to fourth terminals 91A to 91D have connection portions 911A to 911D that are bent at right angles from their lower ends inward, and through holes 912A to 912D are formed in the connection portions 911A to 911D. In other words, the heater 4 is constructed using a graphite heater in which the cylindrical heat generating portion 40, which is the heater element, and the first to fourth terminals 91A to 91D, which are heater legs, are integrally molded.

[0035] As shown in FIG. 3 , the first support electrode 92A to the fourth support electrode 92D are rod-shaped electrodes made of conductive carbon. Of the first support electrode 92A to the fourth support electrode 92D, one to three are low-resistance support electrodes 92L, as shown in the upper diagram of FIG. 4 , and the remaining support electrodes are high-resistance support electrodes 92H, which serve as small-diameter support electrodes, as shown in the lower diagram of FIG. 4 . The low-resistance support electrode 92L includes an electrode body 921L, a clamping portion 922, a male threaded portion 923, and a power supply connection portion 924. The electrode body 921L is formed in a cylindrical shape. The clamping portion 922 is formed in a cylindrical shape with a larger diameter and a shorter height than the electrode body 921L, and is provided at one axial end of the electrode body 921L. The male threaded portion 923 is provided to extend from the clamping portion 922 to the opposite side of the electrode body 921L. The power supply connection portion 924 is provided at the other axial end of the electrode body 921L. The high-resistance support electrode 92H is configured to include a small-diameter electrode body 921H instead of the electrode body 921L. The small-diameter electrode body 921H is formed in a generally cylindrical shape with at least a portion of its diameter smaller than that of the electrode body 921L, and is configured so that the resistance value of the high-resistance support electrode 92H is higher than that of the low-resistance support electrode 92L. The diameter of the narrowest portion of the small-diameter electrode body 921H is preferably 50 mm or more from the perspective of supporting the heater 4. As is well known, the resistance values ​​of the low-resistance support electrode 92L and the high-resistance support electrode 92H can be set to desired values ​​by adjusting the diameter or length of the electrode body 921L and the small-diameter electrode body 921H. The first to fourth support electrodes 92A to 92D, each formed of a high-resistance support electrode 92H or a low-resistance support electrode 92L, have carbon nuts 93A to 93D screwed onto male threaded portions 923 inserted into through holes 912A to 912D of the terminals 91A to 91D, and the terminals 91A to 91D are clamped between the nuts 93A to 93D and the clamping portions 922, thereby electrically connecting the terminals 91A to 91D and supporting the heater 4.

[0036] 5 , the power supply unit 9 further includes a power supply 94, a first anode wiring 95A, a first cathode wiring 95B, a second anode wiring 95C, and a second cathode wiring 95D. One ends of the first and second anode wirings 95A and 95C are connected to the power supply connectors 924 of the first and third support electrodes 92A and 92C, for example, via connectors not shown, and the other ends are connected to the anode of the power supply 94. One ends of the first and second cathode wirings 95B and 95D are connected to the power supply connectors 924 of the second and fourth support electrodes 92B and 92D, for example, via connectors not shown, and the other ends are connected to the cathode of the power supply 94. The other ends of the first and second cathode wirings 95B and 95D may be connected to ground.

[0037] 5 , for example, if the fourth support electrode 92D is configured as a high-resistance support electrode 92H and the first to third support electrodes 92A to 92C are configured as low-resistance support electrodes 92L, the current flowing from the power source 94 to the fourth support electrode 92D will be smaller than the current flowing from the power source 94 to the second support electrode 92B. As a result, the first and second heating elements 40A and 40B generate heat at a higher temperature than the third and fourth heating elements 40C and 40D, and the heat distribution will be non-uniform in the circumferential direction of the crucible 3. In this way, by configuring one to three of the first to fourth support electrodes 92A to 92D as high-resistance support electrodes 92H, the position at which the heating temperature of the crucible 3 is highest in a plan view (hereinafter sometimes referred to as the "maximum heating temperature position") can be set at a desired position. As described above, the insulating material 6 is arranged so that the insulating material central axis 6C is not coaxial with the crucible central axis 3C and the heater central axis 4C, and is configured so that the heat extraction distribution from the heater 4 is non-uniform in the circumferential direction of the crucible 3. Therefore, by adjusting the position of the high-resistance support electrode 92H relative to the crucible 3 and the position where the gap between the insulating material 6 and the heater 4 is smallest, the maximum heating temperature of the crucible 3 and the position of the maximum heating temperature can be more precisely adjusted. Note that, hereinafter, the state in which the heat generation distribution of the heater 4 and the heat extraction distribution from the heater 4 by the insulating material 6 are adjusted to heat the crucible 3 so that a position of the maximum heating temperature exists may be referred to as a "non-uniform heating state." On the other hand, a state in which the crucible 3 is heated so that there is no maximum heating temperature position, that is, a state in which the crucible 3 is heated so that the heating distribution of the crucible 3 is uniform in the circumferential direction of the crucible 3, is sometimes referred to as a "uniform heating state."

[0038] Here, because the thermal conductivity of the crucible 3 is high and the thickness of the entire crucible 3 is uniform, the temperature of the crucible 3 heated in a non-uniform heating state by the heater 4 changes continuously. Therefore, the region heated to the highest temperature at the highest heating temperature position of the silicon melt M (hereinafter sometimes referred to as the "high-temperature melt region") and the region heated to the lowest temperature (hereinafter sometimes referred to as the "low-temperature melt region") face each other across the center of the silicon melt M. The positions of the high-resistance support electrode 92H and the heat insulating material 6 relative to the crucible 3 are preferably set so that the melt temperature difference, calculated by subtracting the temperature of the high-temperature melt region from the temperature of the low-temperature melt region, is 3°C or more, more preferably 5°C or more. A melt temperature difference of 3°C or more makes it easier to fix the convection mode to one mode regardless of the timing of application of the horizontal magnetic field, and a melt temperature difference of 5°C or more makes it easier to fix the convection mode to one mode regardless of the timing of application of the horizontal magnetic field.

[0039] 1 and 2, the first support electrode 92A to the fourth support electrode 92D and the heat insulator 6 are preferably configured so that the first portion 31A and the second portion 31B of the crucible 3, which are located on either side of the first vertical imaginary plane VF1, receive different amounts of heat. More preferably, the first support electrode 92A to the fourth support electrode 92D and the heat insulator 6 are configured so that, as shown in FIG. 6A, the maximum heating temperature position 3MA, at which the crucible 3 is heated to the highest temperature in a plan view, is located on the right side of the crucible central axis 3C and on the opposite side of the rotation direction D1 of the crucible 3 with respect to a first horizontal imaginary line VL1 that is perpendicular to the central magnetic field line 16C and includes the crucible central axis 3C, and the angle θ (°) formed by the first horizontal imaginary line VL1 and a second horizontal imaginary line VL2 connecting the crucible central axis 3C and the maximum heating temperature position 3MA satisfies the following formula (3): Alternatively, the first to fourth support electrodes 92A to 92D and the heat insulating material 6 are more preferably configured so that a maximum heating temperature position 3MB, at which the heating temperature of the crucible 3 is highest in a plan view, is located on the left side of the crucible central axis 3C and is located in the opposite direction of the rotation direction D1 with respect to the first horizontal imaginary line VL1, and the angle θ (°) formed between the first horizontal imaginary line VL1 and a second horizontal imaginary line VL3 connecting the crucible central axis 3C and the maximum heating temperature position 3MB satisfies the following formula (3): θ=360×R×T (3) In formula (3), R is the rotation speed (rpm) of the crucible 3 when a horizontal magnetic field is applied to the silicon melt M. T is the time (minutes) from the start of application of the horizontal magnetic field until the horizontal magnetic field having a magnetic field strength at which the convection direction is fixed (hereinafter, may be referred to as "convection direction fixed magnetic field strength K1") acts on the silicon melt M. The convection direction fixed magnetic field strength K1 is 0.05 tesla (500 gauss) or more and 0.15 tesla (1500 gauss) or less.

[0040] Here, the reason why the first support electrode 92A to the fourth support electrode 92D and the heat insulating material 6 are configured so that the maximum heating temperature positions 3MA and 3MB are located at the positions shown in FIG. 6A will be explained. If the crucible 3 is heated in a uniform heating state, the silicon melt M in the crucible 3 is heated uniformly throughout the entire circumferential direction of the crucible 3. In this case, convection occurs in the silicon melt M, rising near the side of the crucible 3 and descending near the center. When no horizontal magnetic field is applied to the silicon melt M, the position of the downward flow changes chaotically due to instability of the convection, and may deviate from the center of the crucible 3. When application of a horizontal magnetic field is started to the silicon melt M in such a state so that the magnetic field strength reaches a predetermined magnetic field strength K2, the magnitude of the magnetic field acting on the silicon melt M increases in proportion to the elapsed time from the start of application, as shown in FIG. 6B. When the horizontal magnetic field with the convection direction fixed magnetic field intensity K1 acts on the silicon melt M, the rotation of the downward flow in the rotation direction D1 is constrained, and eventually the direction of the convection in an imaginary plane perpendicular to the application direction of the horizontal magnetic field is fixed. When the crucible 3 is heated in this uniform heating state, the horizontal magnetic field is applied in a state in which the position of the downward flow is changing randomly, and therefore the convection mode changes to a right-handed vortex mode or a left-handed vortex mode depending on the timing of the application.

[0041] On the other hand, when the crucible 3 is heated in a non-uniform heating state, even in a state where no horizontal magnetic field is applied to the silicon melt M, an upward flow of the silicon melt M is stably generated on the right side of the crucible 3 and a downward flow is stably generated on the left side of the crucible 3, or an upward flow is stably generated on the left side of the crucible 3 and a downward flow is stably generated on the right side of the crucible 3, and the position of the downward flow does not change randomly as in the case where the crucible 3 is heated in a uniform heating state. Furthermore, the high-temperature melt region rotates in the rotation direction D1 as the crucible 3 rotates at the rotation speed R (rpm). In other words, the region where the upward flow of the silicon melt M is generated moves from the vicinity of the maximum heating temperature positions 3MA, 3MB in the rotation direction D1 at the rotation speed R (rpm). As described above, since the maximum heating temperature position 3MA is set to satisfy the above formula (3), when a horizontal magnetic field with a convection-direction fixed magnetic field intensity K1 acts on the silicon melt M after T minutes from the start of application of the horizontal magnetic field, regardless of the timing of application of the horizontal magnetic field, the rotation of the upward flow in the rotation direction D1 is constrained with the melt high-temperature region overlapping the first horizontal virtual line VL1 in a plan view, and eventually the convection is fixed to the counterclockwise direction, resulting in a left-handed vortex mode. Furthermore, since the maximum heating temperature position 3MB is also set to satisfy the above formula (3), when a horizontal magnetic field with a convection-direction fixed magnetic field intensity K1 acts on the silicon melt M after T minutes from the start of application of the horizontal magnetic field, regardless of the timing of application of the horizontal magnetic field, when a horizontal magnetic field with a convection-direction fixed magnetic field intensity K1 acts on the silicon melt M after T minutes from the start of application of the horizontal magnetic field, the rotation of the upward flow in the rotation direction D1 is constrained with the melt high-temperature region overlapping the first horizontal virtual line VL1 in a plan view, and eventually the convection is fixed to the clockwise direction, resulting in a right-handed vortex mode. In this way, by applying a horizontal magnetic field with a fixed magnetic field strength K1 in the convection direction to the silicon melt M when the high-temperature melt region overlaps the first horizontal virtual line VL1, a left vortex mode or a right vortex mode can be generated more stably than when applying a horizontal magnetic field with a fixed magnetic field strength K1 in the convection direction to the silicon melt M when the high-temperature melt region does not overlap the first horizontal virtual line VL1.

[0042] 7, silicon single crystal manufacturing apparatus 1 further includes a raw material supply unit 18, a crucible rotation drive unit 19, a pull-up drive unit 20, an input unit 21, a memory unit 22, and a control unit 23. A power supply 94, a radiation thermometer 15B, a magnetic field application unit 16, the raw material supply unit 18, the crucible rotation drive unit 19, the pull-up drive unit 20, the input unit 21, and the memory unit 22 are connected to the control unit 23 so as to be able to send and receive various types of information.

[0043] The power supply 94 supplies power to the heating unit 40 via the power supply unit 9 under the control of the control unit 23. The radiation thermometer 15B outputs a signal corresponding to the measurement result to the control unit 23. The magnetic field application unit 16 applies a horizontal magnetic field of a predetermined strength to the silicon melt M under the control of the control unit 23. The raw material supply unit 18 charges the silicon raw material into the crucible 3 under the control of the control unit 23. The crucible rotation drive unit 19 rotates the crucible 3 at a predetermined speed in a predetermined direction under the control of the control unit 23. The pulling drive unit 20 raises and lowers the pulling shaft 7 under the control of the control unit 23. Furthermore, the pulling drive unit 20 rotates the pulling shaft 7 at a predetermined speed in the opposite direction to or the same direction as the rotation direction of the support shaft 5 under the control of the control unit 23.

[0044] The input unit 21 is configured by, for example, a touch panel or physical buttons. The input unit 21 is used to input various settings, and outputs signals corresponding to the input operations to the control unit 23.

[0045] The storage unit 22 is configured by a well-known storage device such as a hard disk drive (HDD), etc. The storage unit 22 stores various information necessary for controlling the pulling of the silicon single crystal SM.

[0046] The control unit 23 includes a CPU (Central Processing Unit). The control unit 23 controls the pulling of the silicon single crystal SM by causing the CPU to execute a program stored in the storage unit 22.

[0047] [Method for Manufacturing Silicon Single Crystal] Next, a method for manufacturing a silicon single crystal SM using the silicon single crystal manufacturing apparatus 1 will be described. Fig. 8 is a flowchart showing the method for manufacturing a silicon single crystal. In this embodiment, the first to fourth support electrodes 92A to 92D and the heat insulator 6 are configured so that the maximum heating temperature position is the maximum heating temperature position 3MA shown in Fig. 6A.

[0048] First, an operator operates the input unit 21 to input pulling conditions for the silicon single crystal SM to be manufactured. The control unit 23 acquires the input pulling conditions as shown in FIG. 8 (Step S1). The control unit 23 then performs the silicon single crystal SM manufacturing process based on the acquired pulling conditions. Specifically, the control unit 23 maintains an inert gas atmosphere under reduced pressure inside the chamber 2, turns off the heater 4 (no power is supplied to the heater 4), and controls the raw material supply unit 18 to charge the silicon raw material into the crucible 3 while not applying a horizontal magnetic field. The control unit 23 then controls the crucible rotation drive unit 19 to rotate the crucible 3 in the rotation direction D1 at a rotation speed R (Step S2).

[0049] Next, the control unit 23 controls the power supply 94 to heat the crucible 3 in a non-uniform heating state using the heat generating unit 40 of the heater 4, thereby melting the silicon raw material and generating a silicon melt M (step S3: silicon melt generating step). In step S3, when all of the silicon raw material is melted, the region in which an upward flow is generated in the silicon melt M moves in the rotation direction D1 at a rotation speed R (rpm) from a position near the maximum heating temperature position 3MA.

[0050] Thereafter, the control unit 23 controls the magnetic field application unit 16 to start applying a horizontal magnetic field to the silicon melt M so that the magnetic field strength becomes a predetermined magnetic field strength K2 (e.g., 0.3 Tesla) (step S4: magnetic field application step). When the horizontal magnetic field with a convection direction fixed magnetic field strength K1 (e.g., 0.1 Tesla) acts on the silicon melt M by the process of step S4, the convection of the silicon melt M is fixed counterclockwise and becomes a left-handed vortex mode.

[0051] Next, the control unit 23 determines whether the convection mode of the silicon melt M has been fixed to the left-handed vortex mode based on a signal corresponding to the measurement result from the radiation thermometer 15B (step S5: convection direction confirmation step). If the control unit 23 determines that the convection mode has not been fixed to the left-handed vortex mode (step S5: NO), it performs the process of step S5 again after a predetermined time has elapsed. On the other hand, if the control unit 23 determines that the convection mode has been fixed to the left-handed vortex mode (step S6: YES), it controls the pull-up drive unit 20 to grow a silicon single crystal SM while continuing to apply the horizontal magnetic field (step S6: growth step). In step S6, the pull-up drive unit 20, under the control of the control unit 23, raises and lowers the pull-up shaft 7 so as to deposit the seed crystal SC in the silicon melt M and then pull up the seed crystal SC, thereby growing the silicon single crystal SM.

[0052] Effects of the Embodiment In the silicon single crystal manufacturing apparatus 1, the first to fourth heating elements 40A to 40D of the heater 4 are electrically connected to the power source 94, and at least one of the first to fourth supporting electrodes 92A to 92D supporting the heater 4 is configured as a high-resistance supporting electrode 92H. By configuring the first to fourth supporting electrodes 92A to 92D in this manner, the current flowing through the high-resistance supporting electrode 92H can be made smaller than the current flowing through the low-resistance supporting electrode 92L, thereby making the heating temperatures of the first to fourth heating elements 40A to 40D non-uniform. This allows the crucible 3 to be heated in a non-uniform heating state, and a downward flow of the silicon melt M can be generated in a stable position. Therefore, by applying a horizontal magnetic field to the silicon melt M generated in a stable position of the downward flow, the convection mode of the silicon melt M can be fixed in a desired state, and a silicon single crystal SM with a stable oxygen concentration can be manufactured. Furthermore, since silicon single crystal SM with a stable oxygen concentration can be produced, the yield of silicon single crystal SM can be improved, and energy efficiency, production efficiency, and waste reduction can be achieved. Furthermore, since a non-uniform heating state can be achieved simply by using the high-resistance support electrode 92H as at least one of the first to fourth support electrodes 92A to 92D, a conventional heater 4 can be used, and there is no need to significantly modify the conventional device configuration. Furthermore, the resistance value of the high-resistance support electrode 92H can be adjusted significantly by simply adjusting the diameter of the small-diameter electrode body 921H, making it easy to achieve the desired non-uniform heating state.

[0053] [Modifications] Although an embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and various improvements and design changes that do not deviate from the gist of the present invention are also included in the present invention.

[0054] When a plurality of the first to fourth support electrodes 92A to 92D are configured as high resistance support electrodes 92H, the resistance value of at least one high resistance support electrode 92H may be higher than the resistance values ​​of the other high resistance support electrodes 92H.

[0055] The insulating material 6 may be arranged so that its central axis 6C is coaxial with the crucible central axis 3C and the heater central axis 4C, thereby providing a uniform heat transfer distribution for the crucible 3. While the configuration using an insulating material 6 with a uniform overall thermal conductivity has been exemplified, a cylindrical insulating material configured so that the thermal conductivity of one portion is different from that of the other portions may be arranged so that the central axis of the insulating material is coaxial with the crucible central axis 3C and the heater central axis 4C, thereby providing a non-uniform heat transfer distribution for the crucible 3. In this case, the thermal conductivity of the insulating material may or may not be set to satisfy the above formula (3).

[0056] Next, examples of the present invention will be described, but the present invention is not limited to these examples.

[0057] [Experimental Conditions] [Definition of the Position of the Melt High-Temperature Region] Positions A to H, which represent the positions of the melt high-temperature region in a planar view, were defined as shown in Fig. 9. Position A is a position where the angle between a reference line extending forward in the application direction of the central magnetic field line 16C from the center of the silicon melt M in a planar view and a level line extending from the center of the silicon melt M to position A is 0°. Positions B, C, D, E, F, G, and H are positions rotated by 45°, 90°, 135°, 180°, 225°, 270°, and 315° clockwise from position A.

[0058] Comparative Example First, the silicon single crystal manufacturing apparatus 1 according to the above embodiment was prepared. Then, all of the first through fourth support electrodes 92A through 92D were made the same thickness, and the insulator 6 was positioned so that the insulator central axis 6C was coaxial with the crucible central axis 3C and the heater central axis 4C. In the comparative example, the crucible 3 was heated uniformly, so that high-temperature and low-temperature melt regions did not occur in the silicon melt M. In other words, under the conditions of the comparative example, the melt temperature difference was 0°C. Then, by performing steps S1 through S6 of the above-described method for manufacturing a silicon single crystal SM, a silicon single crystal SM having a straight body portion SM3 with a diameter of 300 mm and a length of 2000 mm was grown. The rotation direction D1 of the crucible 3 is counterclockwise in FIG. 9 .

[0059] Examples 1 to 16 In Examples 1 to 8, the insulator 6 was positioned so that its central axis 6C was coaxial with the crucible central axis 3C and the heater central axis 4C. The thicknesses of the first to fourth support electrodes 92A to 92D were adjusted so that the melt high-temperature regions were located at positions A, B, C, D, E, F, G, and H, respectively, and the melt temperature difference was 3°C. Silicon single crystals SM were grown under the same conditions as in Examples 1 to 8. In Examples 9 to 16, the position of the insulator 6 relative to the crucible 3 and heater 4 was adjusted so that the melt high-temperature regions were located at positions A, B, C, D, E, F, G, and H, respectively, and the melt temperature difference was 5°C.

[0060] [Evaluation] Before starting the growth of silicon single crystals SM in the comparative example and examples 1 to 16, a horizontal magnetic field was applied at random timing after the generation of silicon melt M to observe the convection modes, and the occurrence rate of each convection mode and the stability of the generated vortices were evaluated. The occurrence rate of each convection mode is shown in Table 1 below and in Figures 10A and 10B, and the evaluation results of the vortex stability are shown in Table 1.

[0061]

[0062] In the comparative example, as shown in Table 1 and Figures 10A and 10B, the occurrence rates of the right vortex mode and the left vortex mode were almost the same. Furthermore, in the comparative example, the direction of the vortex, once fixed, reversed with a probability of 10% or more. The reason for this result is thought to be that the crucible 3 was heated in a uniform heating state, causing the position of the downward flow to change randomly, resulting in the right vortex mode or the left vortex mode changing depending on the timing of application of the horizontal magnetic field.

[0063] On the other hand, in Examples 1 to 8, as shown in Table 1 and Figure 10A, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 10% or more, and it was confirmed that, compared to the comparative example, the convection mode was more easily fixed to one mode regardless of the timing of application of the horizontal magnetic field. The reason for this result is thought to be that the crucible 3 was heated in a non-uniform heating state, which fixed the position of the downward flow, thereby increasing the probability that the convection mode would be fixed to one mode regardless of the timing of application of the horizontal magnetic field.

[0064] In particular, in Examples 3, 4, 6, and 7, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 30% or more, and it was confirmed that it was easier to fix one convection mode regardless of the timing of application of the horizontal magnetic field compared to Examples 1, 2, 5, and 8. Furthermore, in Examples 1, 2, and 5, the direction of a vortex once fixed reversed with a probability of 10% or more, but in Examples 3, 4, 6 to 8, the probability that the direction of a vortex once fixed would reverse was less than 10%.

[0065] From a comparison between the comparative example and Examples 1 to 8, it was confirmed that by adjusting at least the thickness of the first support electrode 92A to the fourth support electrode 92D among the thicknesses of the first support electrode 92A to the fourth support electrode 92D and the position of the heat insulating material 6 so that the melt temperature difference is 3°C or more, it is possible to easily fix the convection mode to one mode, and that it is possible to produce silicon single crystals with a stable oxygen concentration without significantly changing the conventional device configuration.

[0066] Furthermore, in Examples 9 to 16, as shown in Table 1 and FIG. 10B , the difference between the incidence rates of right-handed vortex modes and left-handed vortex modes was 40% or more, confirming that, compared with the comparative example and Examples 1 to 8, the convection direction was more easily fixed in one direction, regardless of the timing of application of the horizontal magnetic field. Furthermore, in Examples 9 to 16, the probability that the direction of the vortex once fixed would reverse was less than 10%. The reason for this result is thought to be that the melt temperature difference was larger than in Examples 1 to 8, which resulted in the generation of a stronger downward flow than in Examples 1 to 8, and the position of the downward flow was fixed, thereby increasing the probability that the convection direction would be fixed in one direction, regardless of the timing of application of the horizontal magnetic field.

[0067] In particular, in Examples 10 to 12 and 14 to 16, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 70% or more, and it was confirmed that the convection direction was more easily fixed in one direction regardless of the timing of application of the horizontal magnetic field compared to Examples 9 and 13. The reason for this result is thought to be that in Examples 9 and 13, the melt high-temperature region was located on central magnetic field line 16C in a planar view, so that the downward flow generated on the opposite side of the melt cooling region with respect to the center of the silicon melt M occurred in the vicinity of central magnetic field line 16C, whereas in Examples 10 to 12 and 14 to 16, the melt high-temperature region was located to the right or left of central magnetic field line 16C in a planar view, so that the downward flow occurred in a region away from central magnetic field line 16C, which further increased the probability that the convection direction was fixed in one direction regardless of the timing of application of the horizontal magnetic field compared to Examples 9 and 13.

[0068] Furthermore, in Examples 11, 12, 15, and 16, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 100%, confirming that, compared to Examples 10 and 14, it was easier to fix the direction of convection in one direction regardless of the timing of application of the horizontal magnetic field. The reason for this result is believed to be as follows. As described above, the high-temperature melt region rotates in the rotation direction D1 as the crucible 3 rotates. Furthermore, the high-temperature melting point region in Example 10 is located forward in the rotation direction D1 relative to the high-temperature melting point regions in Examples 11 and 12, and the high-temperature melting point region in Example 14 is located forward in the rotation direction D1 relative to the high-temperature melting point regions in Examples 15 and 16. For this reason, the position of the high melting point region when a horizontal magnetic field of 0.1 Tesla, which is the convection direction fixed magnetic field strength K1, is applied in Examples 11, 12, 15, and 16, is closer to the first horizontal virtual line VL1 than in Examples 10 and 14, which is thought to be because the probability of the convection direction being fixed in one direction is further increased regardless of the timing of application of the horizontal magnetic field.

[0069] Furthermore, in Examples 12 and 16, the direction of the vortex once fixed does not reverse, and it was confirmed that a right-handed vortex mode or a left-handed vortex mode can be stably generated more easily, regardless of the timing of application of the horizontal magnetic field, than in Examples 11 and 15. The reason for this result is thought to be that the high-melting-point region in Example 11 is located forward in the direction of rotation D1 with respect to the high-melting-point region in Example 12, and the high-melting-point region in Example 15 is located forward in the direction of rotation D1 with respect to the high-melting-point region in Example 16. Therefore, when a horizontal magnetic field of 0.1 Tesla is applied in Examples 12 and 16, the position of the high-melting-point region is closer to the first horizontal virtual line VL1 than in Examples 11 and 15, making it easier to stably generate a right-handed vortex mode or a left-handed vortex mode, regardless of the timing of application of the horizontal magnetic field.

[0070] A comparison of Examples 1 to 8 with Examples 9 to 16 confirmed that by adjusting the thicknesses of the first to fourth support electrodes 92A to 92D and the positions of the thermal insulator 6 so that the melt temperature difference is 5°C or more, it is possible to more easily fix the convection mode to one mode, and to produce silicon single crystals with a more stable oxygen concentration without significantly modifying the conventional device configuration. Note that it is believed that results similar to those of this example can be obtained even if a cylindrical thermal insulator configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion is used instead of the thermal insulator 6 having a uniform thermal conductivity overall.

[0071] The silicon single crystal manufacturing method and silicon single crystal manufacturing apparatus of the present invention can manufacture silicon single crystals with a stable oxygen concentration without making major changes to the configuration of conventional equipment, thereby improving the yield of silicon single crystals, improving energy efficiency, improving production efficiency, and reducing waste.

[0072] 1...silicon single crystal manufacturing apparatus, 3...crucible, 3C...crucible central axis, 3MA, 3MB...maximum heating temperature position, 4...heater, 40A...first heating section, 40B...second heating section, 40C...third heating section, 40D...fourth heating section, 4C...heater central axis, 6...insulating material, 6C...insulating material central axis, 92A...first supporting electrode, 92B...second supporting electrode, 92C...third supporting electrode, 92D...fourth supporting electrode, 92H...high-resistance supporting electrode (narrow-diameter supporting electrode), 94...power source, M...silicon melt, SM...silicon single crystal, VL1...first horizontal imaginary line, VL2, VL3...second horizontal imaginary lines.

Claims

1. A method for producing a silicon single crystal, comprising: using a silicon single crystal production apparatus to pull up a silicon single crystal while applying a horizontal magnetic field to a silicon melt; the silicon single crystal production apparatus comprising: a crucible for accommodating the silicon melt; a heater formed in a cylindrical shape surrounding the crucible, the central axis of the cylinder being positioned coaxially with the central axis of the crucible; and a first supporting electrode, a second supporting electrode, a third supporting electrode and a fourth supporting electrode formed in a rod shape from a conductive material and supporting the heater; the heater comprises a first heating portion, a second heating portion, a third heating portion and a fourth heating portion which have the same heating characteristics and are aligned in the circumferential direction of the crucible; the first supporting electrode connects the first heating portion and the second heating portion to a positive electrode of a power source; the second supporting electrode connects the second heating portion and the third heating portion to a negative electrode of the power source or to earth; and the third supporting electrode connects the third heating portion and the fourth heating portion to the positive electrode; the fourth support electrode connects the fourth heating portion and the first heating portion to the negative electrode or the earth, and at least one of the first support electrode, the second support electrode, the third support electrode and the fourth support electrode is configured as a thin-diameter support electrode having at least a portion thinner than the remaining support electrodes, and the method for producing a silicon single crystal comprises: a silicon melt producing step of heating the silicon raw material in the rotating crucible in a state where the heat generation distribution of the heater is non-uniform to produce the silicon melt; a magnetic field application step of starting to apply the horizontal magnetic field to the silicon melt; and a growing step of growing the silicon single crystal by pulling up a seed crystal immersed in the silicon melt when the direction of convection of the silicon melt in a virtual plane perpendicular to a central magnetic field line of the horizontal magnetic field is fixed in one direction.

2. A method for producing silicon single crystals as described in claim 1, wherein the silicon single crystal production apparatus is provided with an insulating material formed in a cylindrical shape surrounding the heater and configured to cause the heat extraction distribution to the heater to be non-uniform.

3. A method for producing silicon single crystals as described in claim 2, wherein the insulating material is configured so as to have a uniform thermal conductivity throughout, and is arranged so that the central axis of the insulating material is not coaxial with the central axis of the crucible.

4. A method for producing silicon single crystals as described in claim 2, wherein the insulating material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and the central axis of the insulating material is positioned coaxially with the central axis of the crucible.

5. A method for producing a silicon single crystal according to any one of claims 2 to 4, wherein the first support electrode, the second support electrode, the third support electrode, the fourth support electrode and the heat insulating material are configured such that, when a rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt is R (rpm) and a time from when the application of the horizontal magnetic field is started until the horizontal magnetic field, having a magnetic field strength at which the direction of convection is fixed, acts on the silicon melt is T (minutes), a maximum heating temperature position at which the heating temperature for the crucible is the highest in a planar view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field line and includes the central axis of the crucible, and an angle θ (°) formed by a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position and the first horizontal imaginary line satisfies the following formula (1): θ=360×R×T… (1) 6. A silicon single crystal manufacturing apparatus for pulling up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, comprising: a crucible for accommodating the silicon melt; a heater formed in a cylindrical shape surrounding the crucible and arranged so that the central axis of the cylinder is coaxial with the central axis of the crucible; and a first supporting electrode, a second supporting electrode, a third supporting electrode and a fourth supporting electrode formed in a rod shape from a conductive material and supporting the heater, wherein the heater comprises a first heating portion, a second heating portion, a third heating portion and a fourth heating portion having the same heating characteristics and arranged in a circumferential direction of the crucible, the first supporting electrode connects the first heating portion and the second heating portion to a positive electrode of a power source, the second supporting electrode connects the second heating portion and the third heating portion to a negative electrode or earth of the power source, and the third supporting electrode connects the third heating portion and the fourth heating portion to the positive electrode, the fourth support electrode connects the fourth heating portion and the first heating portion to the negative electrode or the earth, and at least one of the first support electrode, the second support electrode, the third support electrode and the fourth support electrode is composed of a thin-diameter support electrode having at least a portion thinner than the remaining support electrodes.

7. A silicon single crystal manufacturing apparatus as claimed in claim 6, further comprising a heat insulating material formed in a cylindrical shape surrounding said heater and configured so that the heat extraction distribution from said heater is non-uniform.

8. A silicon single crystal manufacturing apparatus as described in claim 7, wherein the heat insulating material is configured so as to have a uniform thermal conductivity throughout, and is arranged so that the central axis of the heat insulating material is not coaxial with the central axis of the crucible.

9. A silicon single crystal manufacturing apparatus as described in claim 7, wherein the heat insulating material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and the central axis of the heat insulating material is positioned coaxially with the central axis of the crucible.

10. The silicon single crystal manufacturing apparatus according to any one of claims 7 to 9, wherein the first support electrode, the second support electrode, the third support electrode, the fourth support electrode and the heat insulating material are configured such that, when a rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt is R (rpm) and a time from when the application of the horizontal magnetic field is started to when the horizontal magnetic field acts on the silicon melt, T (minutes), a maximum heating temperature position where the heating temperature for the crucible is the highest in a planar view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field line of the horizontal magnetic field and includes the central axis of the crucible, and an angle θ (°) between a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position and the first horizontal imaginary line satisfies the following formula (2): θ=360×R×T… (2)

Citation Information

Patent Citations

  • Special-shaped graphite electrode column capable of reducing power consumption

    CN217307913U

  • Graphite heater for manufacturing single crystal, single crystal manufacturing unit, and manufacturing method of single crystal

    JP2004315292A

  • Silicon single crystal production apparatus, and silicon single crystal production method using the same

    JP2014189468A

  • Production method for silicon monocrystal and production method for silicon wafer

    JP2023040824A