Powder composition and method for preparing neodymium-iron-boron magnet
By using uniform mixing and hydrogen breaking treatment of Nd, Pr and Cu, Al, Ga, Zn and NdFeB alloy powder in NdFeB magnets, combined with grain boundary diffusion technology, the NdFeB magnets are solved at a high level. The problems of unstable coercive force and inconsistent demagnetization behavior at working temperature achieve higher squareness and stability.
Patent Information
- Application Number
- PCT/CN2024/087643
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-29
- Filing Date
- 2024-04-13
- Publication Date
- 2024-11-07
AI Technical Summary
The existing neodymium iron boron magnets have unstable coercive forces at high working temperatures, and the gradient distribution of heavy rare earths leads to inconsistent demagnetization behavior, affecting the squareness and stability of the magnets.
Using a powder composition, the alloy powder containing Nd, Pr and Cu, Al, Ga, Zn is uniformly mixed with the neodymium iron boron alloy powder, and the airflow grinding is carried out after hydrogen breaking, orientation molding and sintering, combined with grain boundary diffusion technology, Optimize the diffusion depth and distribution of heavy rare earths.
It significantly improves the squareness and stability of neodymium iron boron magnets, reduces the surface accumulation of heavy rare earths, improves the anti-demagnetization ability of the magnets, and enables the magnets to exhibit better performance at high temperatures.
Smart Images

Figure CN2024087643_07112024_PF_FP_ABST
Abstract
Description
Powder composition and method for preparing NdFeB magnet Technical Field
[0001] The present disclosure belongs to the field of rare earth permanent magnet materials and specifically relates to a powder composition and a method for preparing a neodymium iron boron magnet. Background Art
[0002] In order to improve the coercivity of the magnet, heavy rare earth (HRE = Dy / Tb) is used to partially replace Nd2Fe 14 Nd in B forms high magnetocrystalline anisotropy (Nd, HRE)2Fe 14 B to improve the coercive force has become a common method in the industry. Although the addition of heavy rare earth elements can greatly improve the coercive force of the magnet, the atomic magnetic moment of Dy / Tb and the atomic magnetic moment of Fe are arranged in antiparallel, resulting in a sharp drop in the remanence and magnetic energy product of the magnet. The heavy rare earth grain boundary diffusion method can effectively improve the thermal stability of the magnet and is currently the main method for preparing high operating temperature magnets required for permanent magnet motors. The advantage of grain boundary diffusion technology is that the added rare earth elements are mainly distributed at the grain boundaries. Therefore, the heavy rare earth content can be significantly reduced while improving the coercive force and maintaining the remanence, thereby reducing the dependence of high-stability NdFeB magnets on heavy rare earths.
[0003] The diffusion depth of heavy rare earth inside the magnet is limited, the magnet thickness is less than 6mm, and the gradient distribution of heavy rare earth causes the coercive force in different areas inside the magnet to also show a gradient distribution pattern, resulting in inconsistent demagnetization behavior in different areas of the magnet, which worsens the squareness of the magnet demagnetization curve.
[0004] Furthermore, the diffusion depth of heavy rare earth elements within the magnet is anisotropic, meaning that the diffusion depth achieved by grain boundary diffusion parallel to the easy magnetization direction is greater than that achieved by diffusion perpendicular to the easy magnetization direction. To ensure both the diffusion depth and the magnitude of the increase in coercivity, the diffusion depth of heavy rare earth elements along the oriented direction is less than 6mm, and the diffusion depth along the non-oriented direction is even less.
[0005] Summary of the Invention
[0006] In one aspect of the present disclosure, a powder composition is provided, comprising a first powder component and a second powder component, wherein:
[0007] The first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R, and 0 <x≤90;
[0008] The second powder component is raw material neodymium iron boron alloy powder.
[0009] According to certain preferred embodiments of the present disclosure, the first powder component is an alloy hydrogen-fragmented powder obtained by hydrogen-fragmenting an alloy body.
[0010] According to certain preferred embodiments of the present disclosure, the second powder component is NdFeB hydrogen-crushed powder obtained by hydrogen-crushing a raw material NdFeB alloy.
[0011] According to certain preferred embodiments of the present disclosure, the powder composition is obtained by hydrogen-cracking an alloy body from which the first powder component can be obtained and a raw material NdFeB alloy from which the second powder component can be obtained.
[0012] According to certain preferred embodiments of the present disclosure, the powder composition is obtained by uniformly mixing the first powder component and the second powder component.
[0013] According to certain preferred embodiments of the present disclosure, the mass ratio of the first powder component to the second powder component in the powder composition is y:100, wherein 0.5≤y≤2.
[0014] According to certain preferred embodiments of the present disclosure, the uniform mixing comprises subjecting the mixture to jet milling.
[0015] According to certain preferred embodiments of the present disclosure, the average particle size of the first powder component is 3 μm-5 μm.
[0016] According to certain preferred embodiments of the present disclosure, the average particle size of the second powder component is 3 μm-5 μm.
[0017] According to certain preferred embodiments of the present disclosure, the particle size dispersion of the powder composition is no greater than 2.
[0018] In another aspect of the present disclosure, a method for preparing a NdFeB magnet is provided, the method comprising sequentially grinding, orientation molding, sintering, and optionally grain boundary diffusion a powder composition to obtain the NdFeB magnet, wherein the composition comprises a first powder component and a second powder component, wherein:
[0019] The first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R, and 0 <x≤90;
[0020] The second powder component is raw material neodymium iron boron alloy powder.
[0021] According to certain preferred embodiments of the present disclosure, the first powder component is an alloy hydrogen-fragmented powder obtained by hydrogen-fragmenting an alloy body.
[0022] According to certain preferred embodiments of the present disclosure, the second powder component is NdFeB hydrogen-crushed powder obtained by hydrogen-crushing a raw material NdFeB alloy.
[0023] According to certain preferred embodiments of the present disclosure, the powder composition is obtained by hydrogen-cracking an alloy body from which the first powder component can be obtained and a raw material NdFeB alloy from which the second powder component can be obtained.
[0024] According to certain preferred embodiments of the present disclosure, the powder composition is obtained by uniformly mixing the first powder component and the second powder component.
[0025] According to certain preferred embodiments of the present disclosure, the mass ratio of the first powder component to the second powder component in the powder composition is y:100, wherein 0.5≤y≤2.
[0026] According to certain preferred embodiments of the present disclosure, the uniform mixing comprises subjecting the mixture to jet milling.
[0027] According to certain preferred embodiments of the present disclosure, the average particle size of the first powder component is 3 μm-5 μm.
[0028] According to certain preferred embodiments of the present disclosure, the average particle size of the second powder component is 3 μm-5 μm.
[0029] According to certain preferred embodiments of the present disclosure, the particle size dispersion of the powder composition is no greater than 2. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 (a) Backscattering structure diagram of the substrate perpendicular to the easy magnetization direction before diffusion in Example 1; (b) Backscattering structure diagram of the substrate parallel to the easy magnetization direction before diffusion in Example 1; (c) Backscattering structure diagram of the substrate perpendicular to the easy magnetization direction before diffusion in Example 42; (d) Backscattering structure diagram of the substrate parallel to the easy magnetization direction before diffusion in Example 42.
[0031] Figure 2 (a) is an electron probe image of the Tb element in the cross section of the magnet after heavy rare earth diffusion in Example 1, and (b) is an electron probe image of the Tb element in the cross section of the magnet after heavy rare earth diffusion in Example 42. DETAILED DESCRIPTION
[0032] In this disclosure, the knee coercive force H k It is the reverse magnetic field strength required when the magnetization intensity of permanent magnetic material drops to 90% of the remanence during the demagnetization process.
[0033] In this disclosure, the intrinsic coercive force H cj The reverse magnetic field strength required to reduce the residual magnetization to zero.
[0034] In the present disclosure, the squareness H k / H cj is defined as the ratio of the knee point coercivity to the intrinsic coercivity.
[0035] In the present disclosure, the squareness reflects the demagnetization resistance ability of the magnet and affects the working stability of the magnet. The closer the squareness of the magnet is to 1, the less likely the magnet is to lose magnetism and the more stable it is in the working environment.
[0036] In the present disclosure, "preferred" represents one of the optional embodiments, which does not necessarily have to be better than other optional embodiments.
[0037] The present disclosure relates to a powder composition, the composition comprising a first powder component and a second powder component, wherein the first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100 - x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0 ≤ x ≤ 90, preferably 0 < x ≤ 90; the second powder component is a raw neodymium iron boron alloy powder. In an embodiment of the present disclosure, the powder composition of the present disclosure is suitable for preparing a substrate with smaller heavy rare earth diffusion anisotropy, and thus can be used for further manufacturing a rare earth permanent magnet material with excellent properties.
[0038] The present disclosure provides a powder composition, the composition comprising a first powder component and a second powder component, wherein the first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100 - x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0 ≤ x ≤ 90, preferably 0 < x ≤ 90; the second powder component is a raw neodymium iron boron alloy powder.
[0039] In some embodiments of the present disclosure, the first powder component is an alloy hydrogenated and cracked powder obtained by hydrogenating and cracking an alloy body.
[0040] In some embodiments of the present disclosure, the second powder component is a neodymium iron boron hydrogenated and cracked powder obtained by hydrogenating and cracking a raw neodymium iron boron alloy.
[0041] In some embodiments of the present disclosure, the powder composition is obtained by co-hydrogenating and cracking an alloy body capable of obtaining the first powder component and a raw neodymium iron boron alloy capable of obtaining the second powder component.
[0042] In some embodiments of the present disclosure, the composition is obtained by uniformly mixing the first powder component and the second powder component.
[0043] In some embodiments of the present disclosure, the mass ratio of the first powder component to the second powder component in the powder composition is 0.5:100 to 2:100, preferably 1:100 to 1.8:100, preferably 1.4:100 to 1.6:100, preferably 1.5.
[0044] In some embodiments of the present disclosure, the uniform mixing comprises jet milling the mixture.
[0045] In some embodiments of the present disclosure, the average particle size of the first powder component is 3 μm-5 μm, preferably 3.5-4.5 μm, preferably 4 μm.
[0046] In some embodiments of the present disclosure, the average particle size of the second powder component is 3 μm to 5 μm, preferably 3.5 to 4.5 μm, preferably 4 μm.
[0047] In some embodiments of the present disclosure, the powder composition has a particle size discreteness of no greater than 2, preferably no greater than 1.5, preferably no greater than 1.4, preferably no greater than 1.3, preferably no greater than 1.2, preferably no greater than 1.1, preferably no greater than 1.0, preferably no greater than 0.9, preferably no greater than 0.8, preferably no greater than 0.7, preferably no greater than 0.6, preferably no greater than 0.5, preferably no greater than 0.4, preferably no greater than 0.3, preferably no greater than 0.2, preferably no greater than 0.1.
[0048] The present disclosure provides a method for preparing a NdFeB magnet, which comprises diffusing a heavy rare earth element in a direction parallel to and / or perpendicular to the easy magnetization direction of a substrate.
[0049] In some embodiments of the present disclosure, the heavy rare earth is one or both of Dy and Tb.
[0050] In other embodiments of the present disclosure, the heavy rare earth may also be one or more selected from the group consisting of gadolinium (Gd), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y) and scandium (Sc), or a combination of one or more thereof with one or both of Dy and Tb.
[0051] In some embodiments of the present disclosure, the diffusion depth is greater than or equal to 6 mm, preferably greater than or equal to 7 mm, preferably greater than or equal to 8 mm, preferably greater than or equal to 9 mm, preferably greater than or equal to 10 mm.
[0052] In some embodiments of the present disclosure, the substrate is a sintered neodymium iron boron substrate with a difference in the grain boundary area fraction parallel to the easy magnetization direction and perpendicular to the easy magnetization direction less than 2%, preferably the difference in the grain boundary area fraction ≤ 1%, preferably the difference in the grain boundary area fraction ≤ 0.5%, preferably the difference in the grain boundary area fraction ≤ 0.2%
[0053] In some embodiments of the present disclosure, it further includes sintering a powder composition obtained by mixing a raw neodymium iron boron alloy powder and an alloy powder composed of R and M to obtain the substrate, where the mass ratio of R to M is x:(100 - x), R is one or more of Nd and Pr, M is a combination of one or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0 ≤ x ≤ 90, preferably 0 < x ≤ 90, preferably 80 ≤ x ≤ 90, preferably 86 ≤ x ≤ 88, preferably x = 87%.
[0054] In some embodiments of the present disclosure, it further includes thoroughly grinding and mixing the raw neodymium iron boron alloy powder and the alloy powder to obtain a milled powder composition.
[0055] In some embodiments of the present disclosure, it further includes orienting and shaping the milled powder composition.
[0056] In some embodiments of the present disclosure, sintering is directly performed after orienting and shaping the powder composition.
[0057] In some embodiments of the present disclosure, a static pressure process is not included, and the static pressure process includes but is not limited to oil cooling.
[0058] In some embodiments of the present disclosure, sintering is directly performed without going through a static pressure process after orienting and shaping the powder composition.
[0059] In some embodiments of the present disclosure, the grinding method includes but is not limited to grinding using a jet mill.
[0060] In some embodiments of the present disclosure, the grinding method includes but is not limited to grinding using a jet pulverizer.
[0061] In some embodiments of the present disclosure, it includes hydrogenating the alloy body to obtain the alloy powder.
[0062] In some embodiments of the present disclosure, the alloy body is in the form of regular or irregular ingots, blocks, strips, granules or powders.
[0063] In some embodiments of the present disclosure, it includes hydrogenating the raw neodymium iron boron alloy to obtain the raw neodymium iron boron alloy powder.
[0064] In some embodiments of the present disclosure, the raw material NdFeB alloy is in the form of regular or irregular ingots, blocks, bars, particles or powders.
[0065] In some embodiments of the present disclosure, the raw material NdFeB alloy is obtained by sintering.
[0066] In some embodiments of the present disclosure, the raw material NdFeB alloy powder is a main phase material.
[0067] In some embodiments of the present disclosure, the mass percentage of the main phase material is higher than 90% of the material, preferably higher than 95%, preferably higher than 98%, and preferably the mass percentage of the main phase material is 97.5%-99.5%.
[0068] In some embodiments of the present disclosure, the diffusion is a grain boundary diffusion process using a heavy rare earth diffusion source.
[0069] In some embodiments of the present disclosure, the grain boundary diffusion treatment is performed by a magnetron sputtering method.
[0070] In some embodiments of the present disclosure, the grain boundary diffusion treatment is performed by coating, printing, or bonding methods.
[0071] In some embodiments of the present disclosure, the squareness of the magnet is greater than 0.8, preferably ≥0.82, preferably ≥0.83, preferably ≥0.84, preferably ≥0.85, preferably ≥0.86, preferably ≥0.87, preferably ≥0.88, preferably ≥0.89, preferably ≥0.9, preferably ≥0.91, preferably ≥0.92.
[0072] In some embodiments of the present disclosure, the hydrogen cracking temperature is 250-400°C, preferably 260-350°C, preferably 280-320°C, preferably 300°C.
[0073] In some embodiments of the present disclosure, the hydrogen pressure is 0.05-0.15 MPa, preferably 0.07-0.13 MPa, preferably 0.09-0.11 MPa, preferably 0.1 MPa.
[0074] In some embodiments of the present disclosure, the hydrogen cracking time is 5-15 h, preferably 7-13 h, preferably 9-11 h, preferably 10 h, preferably 7 h, preferably 5 h.
[0075] In some embodiments of the present disclosure, the average particle size of the rare earth alloy hydrogen-cracked powder and the raw material NdFeB alloy powder after grinding is 2-5 μm, preferably 3-5 μm, preferably 3.5-4.5 μm, preferably 4 μm.
[0076] In some embodiments of the present disclosure, the mass ratio of the alloy powder to the raw material NdFeB alloy powder is 0.5:100 to 2:100, preferably 1:100 to 1.8:100, preferably 1.4:100 to 1.6:100, preferably 1.5.
[0077] In some embodiments of the present disclosure, the sintering temperature is 1000-1100°C, preferably 1030-1090°C, preferably 1040-1080°C, preferably 1045-1070°C, preferably 1065°C, preferably 1060°C, preferably 1050°C.
[0078] In some embodiments of the present disclosure, the sintering time is 3-10 hours.
[0079] In some embodiments of the present disclosure, the grain boundary diffusion treatment includes a first heat treatment and a second heat treatment, the first heat treatment is performed before the second heat treatment, and the treatment temperature of the first heat treatment is higher than the treatment temperature of the second heat treatment.
[0080] In some embodiments of the present disclosure, the first heat treatment is performed at 800-950°C, preferably 850-950°C, preferably 900-940°C, preferably 920-930°C, preferably 925°C.
[0081] In some embodiments of the present disclosure, the time of the first heat treatment is 3-40 h, preferably 10-40 h, preferably 14 h-40 h, preferably 14 h, preferably 40 h.
[0082] In some embodiments of the present disclosure, the second heat treatment is performed at 450-550°C, preferably 480-530°C, preferably 500-520°C, preferably 510°C.
[0083] In some embodiments of the present disclosure, the time of the second heat treatment is 3-10 h, preferably 3-6 h, preferably 3-5 h, preferably 3 h, preferably 5 h.
[0084] In some embodiments of the present disclosure, the diffusion amount of heavy rare earth is 0.2%-2%, preferably 0.3%-1.5%, preferably 0.4%-1.2%, preferably 0.5%-1%, preferably 0.5%, 0.75% or 1%.
[0085] The present disclosure provides a neodymium iron boron magnet prepared according to the method of the present disclosure.
[0086] The present disclosure provides a NdFeB magnet comprising heavy rare earth elements diffused along an easy magnetization direction parallel to and / or perpendicular to a substrate.
[0087] In some embodiments of the present disclosure, the raw material NdFeB alloy powder is a NdFeB hydrogen-crushed powder obtained by hydrogen-crushing the raw material NdFeB alloy.
[0088] In some embodiments of the present disclosure, the raw material NdFeB alloy contains Nd, Fe and B, and the raw material NdFeB alloy also contains or does not contain one or more of Pr, Tb, Co, Ca, Cu, Al, and Zr, wherein the mass fraction of Nd is 10%-30%, the mass fraction of Fe is less than or equal to 72%, and the mass fraction of B is less than or equal to 1%.
[0089] In some embodiments of the present disclosure, the composition of the raw material NdFeB alloy is expressed as mass fraction as a subscript. 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 .
[0090] The present disclosure provides a NdFeB substrate, which is in a sintered state, wherein the difference between the crystal interface area fractions of the substrate parallel to the easy magnetization direction and perpendicular to the easy magnetization direction is less than 2%.
[0091] In some embodiments of the present disclosure, the substrate comprises blocky agglomerated rare earth-rich phase. In some embodiments of the present disclosure, the average particle size of the rare earth-rich phase particles is less than 2.4 microns, preferably less than 2.3 microns, preferably less than 2.2 microns, preferably less than 2.1 microns, preferably less than 2.0 microns, and preferably less than 1.9 microns.
[0092] In some embodiments of the present disclosure, the proportion of rare earth-rich phase particles having a particle size greater than 3 microns in all the rare earth-rich phase particles is less than 20%, preferably less than 19%, preferably less than 18%, preferably less than 17%, preferably less than 16%, preferably less than 15%, preferably less than 14%, preferably less than 13%, preferably less than 12%, preferably less than 11%, and preferably less than 10%.
[0093] In some embodiments of the present disclosure, the NdFeB substrate comprises grain boundaries, the width of the grain boundaries is less than 0.5 micrometers, preferably less than 0.3 micrometers, preferably less than 0.1 micrometers, and the length of the grain boundaries is 0.5 to 6 micrometers.
[0094] In some embodiments of the present disclosure, after diffusing the heavy rare earth for 8 mm along the easy magnetization direction perpendicular to the substrate, the squareness of the resulting magnet is greater than or equal to 0.85, preferably ≥0.82, preferably ≥0.83, preferably ≥0.84, preferably ≥0.85, preferably ≥0.86, preferably ≥0.87, preferably ≥0.88, preferably ≥0.89, preferably ≥0.9, preferably ≥0.91, and preferably ≥0.92.
[0095] In some embodiments of the present disclosure, heavy rare earth is diffused along a direction perpendicular to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 6 mm, preferably greater than or equal to 7 mm, preferably greater than or equal to 8 mm, preferably greater than or equal to 9 mm, and preferably greater than or equal to 10 mm.
[0096] In some embodiments of the present disclosure, the heavy rare earth is diffused along the easy magnetization direction parallel to the substrate, and the diffusion depth is greater than or equal to 6 mm, preferably greater than or equal to 7 mm, preferably greater than or equal to 8 mm, preferably greater than or equal to 9 mm, preferably greater than or equal to 10 mm.
[0097] In some embodiments of the present disclosure, the substrate is obtained by sintering a powder composition obtained by mixing a raw material neodymium iron boron alloy powder with an alloy powder consisting of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0≤x≤90, preferably 80≤x≤90, preferably 86≤x≤88, and preferably x=87%.
[0098] Example
[0099] The present disclosure will be further described in detail below in conjunction with the embodiments of the accompanying drawings, but the present disclosure is not limited to these embodiments. The following embodiments are for illustrative purposes only and should not be used to limit the scope of the present disclosure and the claims.
[0100] Examples 1-6
[0101] The elements Nd and Al were mixed according to the Nd:Al mass ratio in Table 1. The mixed raw materials were placed in an arc melting furnace and smelted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-broken powder was mixed with a Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B0.95 The NdFeB hydrogen-crushed powders were mixed uniformly at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to obtain the NdFeB substrate. A heavy rare earth diffusion source was diffused parallel to the easy magnetization direction of the NdFeB substrate via magnetron sputtering. The heavy rare earth Tb diffusion thickness in the diffusion direction was 6mm, and the heavy rare earth Tb diffusion content was 1%. Heat treatment was then performed at 925°C for 14 hours and at 510°C for 3 hours to produce high-performance NdFeB magnets with excellent squareness.
[0102] Table 1
[0103] Examples 7-12
[0104] The elements Nd and Al were mixed according to the Nd:Al mass ratio in Table 2. The mixed raw materials were placed in an arc melting furnace and smelted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-broken powder was mixed with a Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 NdFeB hydrogen-crushed powders were mixed at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. Heavy rare earth diffusion sources were diffused perpendicular to the easy magnetization direction of the NdFeB substrate via magnetron sputtering. The Tb diffusion thickness in the diffusion direction was 8mm, and the Tb diffusion content was 1%. Heat treatments were then performed at 925°C for 40 hours and 510°C for 3 hours, resulting in high-performance NdFeB magnets with excellent squareness.
[0105] Table 2
[0106] Examples 13-16
[0107] The elements Nd and Al are added in a ratio of 87:13. 87 Al 13The prepared raw materials are placed in an arc melting furnace and smelted in an argon atmosphere to obtain a rare earth alloy ingot; the rare earth alloy ingot is hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa; the rare earth alloy hydrogen-broken powder is mixed with a composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 NdFeB hydrogen-crushed powders were mixed at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4 μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. Heavy rare earth (Tb) diffusion sources were diffused perpendicular to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness is shown in Table 3, and the Tb diffusion content was 1%. Heat treatments at 925°C for 40 hours and 510°C for 3 hours produced high-performance NdFeB magnets with excellent squareness.
[0108] Table 3
[0109] Examples 17-21
[0110] The elements Nd and Al are mixed in a ratio of 87:13. 87 Al 13 The prepared raw materials are placed in an arc melting furnace and smelted in an argon atmosphere to obtain a rare earth alloy ingot; the rare earth alloy ingot is hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa; the rare earth alloy hydrogen-broken powder is mixed with a composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95NdFeB hydrogen-crushed powders were mixed at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4 μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. Heavy rare earth (Tb) diffusion sources were diffused parallel to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness is shown in Table 4, and the Tb diffusion content was 1%. Heat treatments at 925°C for 40 hours and 510°C for 3 hours produced high-performance NdFeB magnets with excellent squareness.
[0111] Table 4
[0112] Examples 22-26
[0113] The elements Pr and Cu were placed in an arc melting furnace according to the Pr:Cu mass ratio shown in Table 5, and the prepared raw materials were placed in an argon atmosphere and melted to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-destructed for 5 hours at a temperature of 350°C and a hydrogen pressure of 0.15 MPa. The rare earth alloy hydrogen-destructed powder and NdFeB hydrogen-destructed powder were uniformly mixed in a mass ratio of 1:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-destructed powder and sintered NdFeB hydrogen-destructed powder after jet milling was 3 μm. The sintered NdFeB magnetic powder after jet milling and the rare earth alloy powder were oriented and formed into a green compact, which was sintered at 1060°C for 5 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was applied by coating to the grain boundary diffusion parallel to the easy magnetization direction of the NdFeB substrate. The thickness of the heavy rare earth Dy diffusion direction was 10 mm, and the heavy rare earth Dy diffusion amount was 0.75%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 14 hours and at 510°C for 3 hours.
[0114] Table 5
[0115] Examples 27-31
[0116] The elements Nd and Zn were placed in an arc melting furnace according to the Nd:Zn mass ratio in Table 6, and the prepared raw materials were placed in an argon atmosphere and melted to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-destructed for 10 hours at a temperature of 250°C and a hydrogen pressure of 0.08 MPa. The rare earth alloy hydrogen-destructed powder and NdFeB hydrogen-destructed powder were uniformly mixed in a mass ratio of 2:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-destructed powder and sintered NdFeB hydrogen-destructed powder after jet milling was 5 μm. The sintered NdFeB magnetic powder and rare earth alloy powder after jet milling were oriented and formed into a green compact, which was sintered at 1050°C for 10 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was subjected to grain boundary diffusion treatment perpendicular to the easy magnetization direction of the NdFeB substrate by magnetron sputtering. The thickness of the heavy rare earth Dy diffusion direction was 8 mm, and the heavy rare earth Dy diffusion amount was 0.5%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 10 h and at 510°C for 5 h.
[0117] Table 6
[0118] Examples 32-36
[0119] The elements Pr and Cu were placed in an arc melting furnace with a Pr:Cu mass ratio of 80:20, and the prepared raw materials were placed in an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-decomposed for 5 hours at a temperature of 350°C and a hydrogen pressure of 0.15 MPa. The rare earth alloy hydrogen-decomposed powder and NdFeB hydrogen-decomposed powder were uniformly mixed in a mass ratio of 1:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-decomposed powder and sintered NdFeB hydrogen-decomposed powder after jet milling was 3 μm. The sintered NdFeB magnetic powder after jet milling and the rare earth alloy powder were oriented and formed into a green compact, which was sintered at 1060°C for 5 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was treated by grain boundary diffusion parallel to the easy magnetization direction of the NdFeB substrate by a coating method. The thickness of the heavy rare earth Dy diffusion direction is shown in Table 7, and the heavy rare earth Dy diffusion amount is 0.75%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 14 hours and at 510°C for 3 hours.
[0120] Table 7
[0121] Examples 37-41
[0122] The elements Nd and Zn were placed in an arc melting furnace with a Nd:Zn mass ratio of 80:20, and the prepared raw materials were placed in an argon atmosphere to obtain a rare earth alloy ingot; the rare earth alloy ingot was hydrogen-decomposed for 10 hours at a temperature of 250°C and a hydrogen pressure of 0.08 MPa; the rare earth alloy hydrogen-decomposed powder and NdFeB hydrogen-decomposed powder were uniformly mixed in a mass ratio of 2:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-decomposed powder and sintered NdFeB hydrogen-decomposed powder after jet milling was 5 μm; the sintered NdFeB magnetic powder and rare earth alloy powder after jet milling were oriented and formed into a green compact, and then sintered at 1050°C for 10 hours to obtain an NdFeB substrate; a heavy rare earth diffusion source was subjected to grain boundary diffusion treatment perpendicular to the easy magnetization direction of the NdFeB substrate by magnetron sputtering. The thickness of the heavy rare earth Dy diffusion direction was shown in Table 8, and the heavy rare earth Dy diffusion amount was 0.5%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 10 h and at 510°C for 5 h.
[0123] Table 8
[0124] Example 42
[0125] The sintered NdFeB magnetic powder (composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 After orientation molding, the compact was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth (Tb) diffusion source was diffused parallel to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness in the direction of the heavy rare earth (Tb) diffusion was 6 mm, and the Tb diffusion content was 1%. The NdFeB magnet was then heat treated at 925°C for 14 hours and at 510°C for 3 hours.
[0126] Example 43
[0127] The sintered NdFeB magnetic powder (composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95After orientation molding, the compact was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth (Tb) diffusion source was diffused perpendicular to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness was 8 mm and the Tb diffusion content was 1%. The NdFeB magnet was then heat treated at 925°C for 40 hours and then at 510°C for 3 hours.
[0128] Example 44
[0129] The sintered NdFeB magnetic powder (composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 After orientation molding, the compact was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth (Tb) diffusion source was diffused perpendicular to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness in the direction of diffusion was 10 mm, and the Tb diffusion content was 1%. The NdFeB magnet was then heat treated at 925°C for 40 hours and at 510°C for 3 hours.
[0130] Table 9
[0131] Comparing Figure 1(a)-(d), we can find that the introduction of R x M 100-x After alloying, the difference in the grain boundary phase content in different directions of the substrate is reduced, which effectively improves the anisotropy of the grain boundary phase distribution of the substrate and forms a continuous and narrow grain boundary inside the substrate. The electron probe results (Figure 2) show that the Tb element has a great influence on the growth of the R x M 100-x The alloy has a deeper diffusion depth in the matrix, the accumulation of heavy rare earth on the surface is significantly reduced, and the concentration gradient inside the magnet is slowed down. x M 100-x The alloyed NdFeB diffused magnets exhibited even better squareness. For a 10 mm thick substrate, the squareness of the magnets after Tb diffusion perpendicular to the easy magnetization direction still reached 0.92, significantly better than the 0.77 in Example 83.
[0132] By comparing the magnetic performance data of the embodiment and the comparative example, it can be seen that by introducing R x M 100-xBy regulating the distribution morphology and content of the grain boundary phase in different directions of the substrate, the squareness of the diffusion magnet is effectively improved, the accumulation of Tb elements on the surface of the magnet is reduced, and the utilization rate of heavy rare earths is effectively improved.
[0133] Examples 45-47
[0134] The elements Nd and Al were mixed in a mass ratio of Nd:Al of 87:13, and the mixed raw materials were placed in an arc melting furnace and melted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-decomposed for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-decomposed powder was uniformly mixed with NdFeB hydrogen-decomposed powder having the composition shown in Table 10 in a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-decomposed powder and sintered NdFeB hydrogen-decomposed powder after jet milling was 4 μm. The sintered NdFeB magnetic powder after jet milling and the rare earth alloy powder were oriented and formed into a green compact, which was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was subjected to grain boundary diffusion treatment parallel to the easy magnetization direction of the NdFeB substrate by magnetron sputtering. The thickness of the heavy rare earth Tb diffusion direction was 6 mm, and the heavy rare earth Tb diffusion amount was 1%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 14 hours and at 510°C for 3 hours.
[0135] Table 10
[0136] Examples 48-49
[0137] The elements Nd and Al were mixed in a mass ratio of 87:13. The mixed raw materials were placed in an arc melting furnace and smelted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-broken powder was mixed with a Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95The NdFeB hydrogen-crushed powders were mixed uniformly according to the mass ratios specified in Table 11 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4 μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. A heavy rare earth diffusion source was diffused parallel to the easy magnetization direction of the NdFeB substrate via magnetron sputtering. The heavy rare earth Tb diffusion thickness in the diffusion direction was 6 mm, and the heavy rare earth Tb diffusion content was 1%. Heat treatment was then performed at 925°C for 14 hours and at 510°C for 3 hours, resulting in a high-performance NdFeB magnet with excellent squareness.
[0138] Table 11
[0139] The average particle size and particle size dispersion of the powder compositions obtained in Examples 1-49 were measured to obtain the measurement results shown in Table 12. The difference in the crystal interface area fraction parallel to the easy magnetization direction and perpendicular to the easy magnetization direction, the average particle size of the rare earth-rich phase particles, the proportion of rare earth-rich phase particles with a particle size greater than 3 μm to the total rare earth-rich phase particles, the grain boundary width, and the grain boundary length of the substrates obtained in Examples 1-49 were measured to obtain the measurement results shown in Tables 13-14.
[0140] Table 12
[0141] Table 13
[0142] Table 14
[0143] The above embodiments are intended only to illustrate the technical concepts and features of the present disclosure. Their purpose is to enable those skilled in the art to understand the contents of the present disclosure and implement them accordingly. They are not intended to limit the scope of protection of the present disclosure. Any equivalent changes or modifications made in accordance with the spirit of the present disclosure shall be included in the scope of protection of the present disclosure.
Claims
1. A powder composition, comprising a first powder component and a second powder component, wherein: The first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0 <x≤90; The second powder component is a raw material NdFeB alloy powder.
2. The powder composition according to claim 1, wherein the first powder component is an alloy hydrogen-fractured powder obtained by hydrogen-fractured an alloy body.
3. The powder composition according to claim 1, wherein the second powder component is a NdFeB hydrogen-crushed powder obtained by hydrogen-crushing a raw material NdFeB alloy.
4. The powder composition according to claim 1, wherein the powder composition is obtained by hydrogen cracking an alloy body from which the first powder component can be obtained and a raw material NdFeB alloy from which the second powder component can be obtained. 5 . The powder composition according to claim 2 , which is obtained by uniformly mixing the first powder component and the second powder component. 6 . The powder composition according to claim 1 , wherein a mass ratio of the first powder component to the second powder component in the powder composition is y:100, wherein 0.5≤y≤2.
7. The powder composition according to claim 5, wherein the uniform mixing comprises jet milling the mixture.
8. The powder composition according to claim 1, wherein the average particle size of the first powder component is 3 μm to 5 μm.
9. The powder composition according to claim 1, wherein the average particle size of the second powder component is 3 μm to 5 μm.
10. The powder composition according to any one of claims 8 to 9, wherein the particle size dispersion of the powder composition is not greater than 2.
11. A method for preparing a neodymium iron boron magnet, the method comprising sequentially grinding, orientation molding, sintering and optionally grain boundary diffusion a powder composition to obtain the neodymium iron boron magnet, wherein the composition comprises a first powder component and a second powder component, wherein: The first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0 <x≤90; The second powder component is a raw material NdFeB alloy powder. 12 . The method for preparing a NdFeB magnet according to claim 11 , wherein the first powder component is an alloy hydrogen-cracked powder obtained by hydrogen-cracked an alloy body.
13. The method for preparing a NdFeB magnet according to claim 11, wherein the second powder component is NdFeB hydrogen-crushed powder obtained by hydrogen-crushing a raw material NdFeB alloy.
14. The method for preparing a NdFeB magnet according to claim 11, wherein the powder composition is obtained by hydrogen cracking an alloy body capable of obtaining the first powder component and a raw material NdFeB alloy capable of obtaining the second powder component. 15 . The method for preparing a NdFeB magnet according to claim 12 , wherein the powder composition is obtained by uniformly mixing the first powder component and the second powder component. 16 . The method for preparing a NdFeB magnet according to claim 11 , wherein the mass ratio of the first powder component to the second powder component in the powder composition is y:100, wherein 0.5≤y≤2. 17 . The method for preparing a NdFeB magnet according to claim 15 , wherein the uniform mixing comprises jet milling the mixture. 18 . The method for preparing a NdFeB magnet according to claim 11 , wherein the average particle size of the first powder component is 3 μm-5 μm.
19. The method for preparing a NdFeB magnet according to claim 11, wherein the average particle size of the second powder component is 3 μm-5 μm. 20 . The method for preparing a NdFeB magnet according to claim 18 , wherein the particle size dispersion of the powder composition is not greater than 2.
Citation Information
Patent Citations
Highly magnetic rapid quenching neodymium iron boron magnetic powder and preparation method thereof
CN109599236A
Preparation method of neodymium iron boron anisotropic bonded magnetic powder
CN111354524A
Neodymium-iron-boron magnet material and preparation method thereof
CN115020057A
Powder composition
CN116543994A
Cited By
Neodymium-iron-boron magnet and preparation method thereof
CN121439430A