Neodymium-iron-boron substrate and preparation method for neodymium-iron-boron magnet
By optimizing the grain boundary structure and heavy rare earth diffusion direction of the neodymium iron bo base material, the problems of insufficient coercive force and inconsistent demagnetization of the neodymium iron bo magnet at high working temperatures are solved, and the squareness and stability of the magnet are improved.
Patent Information
- Application Number
- PCT/CN2024/087644
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-29
- Filing Date
- 2024-04-13
- Publication Date
- 2024-11-07
AI Technical Summary
The existing neodymium iron boron magnets have insufficient coercive force and inconsistent demagnetization behavior at high working temperatures, resulting in low squareness and affecting stability.
By preparing a neodymium iron boron substrate, the grain boundary area fraction parallel to the easy magnetization direction and perpendicular to the easy magnetization direction is less than 2%, and heavy rare earth diffusion is carried out in different directions, with a depth greater than or equal to 8mm, combined with Nd, Pr, Alloy powders of Cu, Al, Ga, Zn and other elements are sintered to form an optimized grain boundary diffusion structure.
The squareness of the neodymium iron boron magnet is significantly improved, which is greater than or equal to 0.85, which improves the anti-demagnetization ability and stability of the magnet, reduces the dependence on heavy rare earths, and improves the thermal stability of the magnet.
Smart Images

Figure CN2024087644_07112024_PF_FP_ABST
Abstract
Description
NdFeB substrate and method for preparing NdFeB magnet Technical Field
[0001] The present disclosure belongs to the field of rare earth permanent magnet materials and specifically relates to a NdFeB substrate and a method for preparing a NdFeB magnet. Background Art
[0002] In order to improve the coercivity of the magnet, heavy rare earth (HRE = Dy / Tb) is used to partially replace Nd2Fe 14 Nd in B forms high magnetocrystalline anisotropy (Nd, HRE)2Fe 14 B to improve the coercive force has become a common method in the industry. Although the addition of heavy rare earth elements can greatly improve the coercive force of the magnet, the atomic magnetic moment of Dy / Tb and the atomic magnetic moment of Fe are arranged in antiparallel, resulting in a sharp drop in the remanence and magnetic energy product of the magnet. The heavy rare earth grain boundary diffusion method can effectively improve the thermal stability of the magnet and is currently the main method for preparing high operating temperature magnets required for permanent magnet motors. The advantage of grain boundary diffusion technology is that the added rare earth elements are mainly distributed at the grain boundaries. Therefore, the heavy rare earth content can be significantly reduced while improving the coercive force and maintaining the remanence, thereby reducing the dependence of high-stability NdFeB magnets on heavy rare earths.
[0003] The diffusion depth of heavy rare earth inside the magnet is limited, the magnet thickness is less than 6mm, and the gradient distribution of heavy rare earth causes the coercive force in different areas inside the magnet to also show a gradient distribution pattern, resulting in inconsistent demagnetization behavior in different areas of the magnet, which worsens the squareness of the magnet demagnetization curve.
[0004] Furthermore, the diffusion depth of heavy rare earth elements within the magnet is anisotropic, meaning that the diffusion depth achieved by grain boundary diffusion parallel to the easy magnetization direction is greater than that achieved by diffusion perpendicular to the easy magnetization direction. To ensure both the diffusion depth and the magnitude of the increase in coercivity, the diffusion depth of heavy rare earth elements along the oriented direction is less than 6mm, and the diffusion depth along the non-oriented direction is even less.
[0005] Summary of the Invention
[0006] In one aspect of the present disclosure, a NdFeB substrate is provided. The substrate is in a sintered state, wherein the crystal interface area fraction of the substrate parallel to the easy magnetization direction and perpendicular to the easy magnetization direction is less than 2%.
[0007] According to certain preferred embodiments of the present disclosure, the substrate comprises a massive agglomerated rare earth-rich phase.
[0008] According to certain preferred embodiments of the present disclosure, the average particle size of the rare earth-rich phase particles is less than 2.4 microns.
[0009] According to certain preferred embodiments of the present disclosure, the proportion of rare earth-rich phase particles having a particle size greater than 3 microns in all the rare earth-rich phase particles is less than 20%.
[0010] According to certain preferred embodiments of the present disclosure, the NdFeB substrate comprises grain boundaries, the width of the grain boundaries is less than 0.5 micrometers, and the length of the grain boundaries is 0.5 to 6 micrometers.
[0011] According to certain preferred embodiments of the present disclosure, the substrate is obtained by sintering a powder composition obtained by mixing a raw material NdFeB alloy powder with an alloy powder consisting of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R, and 0 <x≤90。
[0012] In another aspect of the present disclosure, a method for preparing a NdFeB magnet is provided, the method comprising performing grain boundary diffusion treatment on a NdFeB substrate to obtain the NdFeB magnet, wherein the NdFeB substrate is in a sintered state, and the crystal interface area fraction of the substrate parallel to the easy magnetization direction and perpendicular to the easy magnetization direction is less than 2%.
[0013] According to certain preferred embodiments of the present disclosure, the heavy rare earth is diffused 8 mm along a direction perpendicular to the easy magnetization direction of the substrate, so that the squareness of the obtained NdFeB magnet is greater than or equal to 0.85.
[0014] According to certain preferred embodiments of the present disclosure, the heavy rare earth is diffused along a direction perpendicular to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 8 mm.
[0015] According to certain preferred embodiments of the present disclosure, the heavy rare earth is diffused in a direction parallel to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 8 mm.
[0016] According to certain preferred embodiments of the present disclosure, the heavy rare earth is one or both of Dy and Tb.
[0017] According to certain preferred embodiments of the present disclosure, the NdFeB substrate is obtained by sintering a powder composition obtained by mixing a raw NdFeB alloy powder with an alloy powder consisting of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R, and 0 <x≤90。 BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 (a) Backscattering structure diagram of the substrate perpendicular to the easy magnetization direction before diffusion in Example 1; (b) Backscattering structure diagram of the substrate parallel to the easy magnetization direction before diffusion in Example 1; (c) Backscattering structure diagram of the substrate perpendicular to the easy magnetization direction before diffusion in Example 42; (d) Backscattering structure diagram of the substrate parallel to the easy magnetization direction before diffusion in Example 42.
[0019] Figure 2 (a) is an electron probe image of the Tb element in the cross section of the magnet after heavy rare earth diffusion in Example 1, and (b) is an electron probe image of the Tb element in the cross section of the magnet after heavy rare earth diffusion in Example 42. DETAILED DESCRIPTION
[0020] In the present disclosure, unless otherwise specified, the expression “the area fraction of the crystal boundaries parallel to the easy magnetization direction and perpendicular to the easy magnetization direction in the substrate is less than 2%” means that the difference between the area fraction of the grain boundaries parallel to the easy magnetization direction in the NdFeB substrate and the area fraction of the grain boundaries perpendicular to the easy magnetization direction in the NdFeB substrate is less than 2%.
[0021] In this disclosure, the knee coercive force H k It is the reverse magnetic field strength required when the magnetization intensity of permanent magnetic material drops to 90% of the remanence during the demagnetization process.
[0022] In this disclosure, the intrinsic coercive force H cj The reverse magnetic field strength required to reduce the residual magnetization to zero.
[0023] In this disclosure, the squareness H k / H cj It is defined as the ratio of the knee coercivity to the intrinsic coercivity.
[0024] In this disclosure, squareness reflects the magnet's ability to resist demagnetization and affects its operating stability. The closer the squareness of a magnet is to 1, the less likely it is to lose magnetism and the more stable it is in its operating environment.
[0025] In this disclosure, "preferred" means one of the alternative embodiments, which is not necessarily preferred over other alternative embodiments.
[0026] The present disclosure relates to a NdFeB substrate, the substrate being in a sintered state, wherein the difference in the grain boundary area fraction between the direction parallel to the easy magnetization direction and the direction perpendicular to the easy magnetization direction of the substrate is ≤1%. In an embodiment of the present disclosure, the NdFeB substrate of the present disclosure is obtained by sintering a powder composition obtained by mixing raw NdFeB alloy powder with an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100 - x), R is one or more of Nd and Pr, M is a combination of one or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0≤x≤90, preferably 0<x≤90. In an embodiment of the present disclosure, the substrate of the present disclosure can be used to further manufacture a rare earth permanent magnet material with excellent performance.
[0027] The present disclosure provides a NdFeB substrate, the substrate being in a sintered state, wherein the difference in the grain boundary area fraction between the direction parallel to the easy magnetization direction and the direction perpendicular to the easy magnetization direction of the substrate is less than 2%.
[0028] In some embodiments of the present disclosure, the substrate contains massive agglomerated rare earth-rich phases.
[0029] In some embodiments of the present disclosure, the average particle size of the rare earth-rich phase particles is less than 2.4 microns, preferably less than 2.3 microns, preferably less than 2.2 microns, preferably less than 2.1 microns, preferably less than 2.0 microns, preferably less than 1.9 microns.
[0030] In some embodiments of the present disclosure, the proportion of rare earth-rich phase particles with a particle size greater than 3 microns in all the rare earth-rich phase particles is less than 20%, preferably less than 19%, preferably less than 18%, preferably less than 17%, preferably less than 16%, preferably less than 15%, preferably less than 14%, preferably less than 13%, preferably less than 12%, preferably less than 11%, preferably less than 10%.
[0031] In some embodiments of the present disclosure, the NdFeB substrate contains grain boundaries, the width of the grain boundaries is less than 0.5 microns, preferably less than 0.3 microns, preferably less than 0.1 microns, and the length of the grain boundaries is 0.5 to 6 microns.
[0032] In some embodiments of the present disclosure, after diffusing heavy rare earths 8 mm along the direction perpendicular to the easy magnetization direction of the substrate, the squareness of the obtained magnet is greater than or equal to 0.85, preferably ≥0.82, preferably ≥0.83, preferably ≥0.84, preferably ≥0.85, preferably ≥0.86, preferably ≥0.87, preferably ≥0.88, preferably ≥0.89, preferably ≥0.9, preferably ≥0.91, preferably ≥0.92.
[0033] In some embodiments of the present disclosure, heavy rare earth is diffused along a direction perpendicular to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 6 mm, preferably greater than or equal to 7 mm, preferably greater than or equal to 8 mm, preferably greater than or equal to 9 mm, preferably greater than or equal to 10 mm.
[0034] In some embodiments of the present disclosure, heavy rare earth is diffused along a direction parallel to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 6 mm, preferably greater than or equal to 7 mm, preferably greater than or equal to 8 mm, preferably greater than or equal to 9 mm, preferably greater than or equal to 10 mm.
[0035] In some embodiments of the present disclosure, the heavy rare earth is one or both of Dy and Tb.
[0036] In some embodiments of the present disclosure, the substrate is obtained by sintering a powder composition obtained by mixing raw neodymium-iron-boron alloy powder with an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100 - x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0 ≤ x ≤ 90, preferably 0 < x ≤ 90, preferably 80 ≤ x ≤ 90, preferably 86 ≤ x ≤ 88, preferably x = 87%.
[0037] The present disclosure provides a method for preparing a neodymium-iron-boron magnet, the method including diffusing heavy rare earth along a direction parallel to and / or perpendicular to the easy magnetization direction of the substrate.
[0038] In some other embodiments of the present disclosure, the heavy rare earth may also be one or more selected from the group consisting of gadolinium (Gd), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y), and scandium (Sc), or a combination of one or more of them with one or both of Dy and Tb.
[0039] In some embodiments of the present disclosure, the diffusion depth is greater than or equal to 6 mm, preferably greater than or equal to 7 mm, preferably greater than or equal to 8 mm, preferably greater than or equal to 9 mm, preferably greater than or equal to 10 mm.
[0040] In some embodiments of the present disclosure, the substrate is a sintered neodymium-iron-boron substrate with a difference in the grain boundary area fraction parallel to the easy magnetization direction and perpendicular to the easy magnetization direction less than 2%, preferably the difference in the grain boundary area fraction ≤ 1%, preferably the difference in the grain boundary area fraction ≤ 0.5%, preferably the difference in the grain boundary area fraction ≤ 0.2%.
[0041] In some embodiments of the present disclosure, the substrate is obtained by sintering a powder composition obtained by mixing a raw material NdFeB alloy powder with an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0≤x≤90, preferably 80≤x≤90, preferably 86≤x≤88, and preferably x=87%.
[0042] In some embodiments of the present disclosure, the process further comprises grinding and mixing the raw NdFeB alloy powder and the alloy powder to obtain a ground powder composition.
[0043] In some embodiments of the present disclosure, the milled powder composition is further oriented and shaped.
[0044] In some embodiments of the present disclosure, sintering is performed directly after orienting the powder composition into a shape.
[0045] In some embodiments of the present disclosure, a static pressure process is not included, and the static pressure process includes but is not limited to oil cooling.
[0046] In some embodiments of the present disclosure, sintering is performed directly after the powder composition is oriented and shaped without going through an static pressing process.
[0047] In some embodiments of the present disclosure, the grinding method includes but is not limited to grinding using a jet mill.
[0048] In some embodiments of the present disclosure, the grinding method includes but is not limited to grinding using a jet mill.
[0049] In some embodiments of the present disclosure, the alloy body is subjected to hydrogen cracking to obtain the alloy powder.
[0050] In some embodiments of the present disclosure, the alloy body is in the form of a regular or irregular ingot, block, strip, granule or powder.
[0051] In some embodiments of the present disclosure, the raw material NdFeB alloy is hydrogen-crushed to obtain the raw material NdFeB alloy powder.
[0052] In some embodiments of the present disclosure, the raw material NdFeB alloy is in the form of regular or irregular ingots, blocks, bars, particles or powders.
[0053] In some embodiments of the present disclosure, the raw material NdFeB alloy is obtained by sintering.
[0054] In some embodiments of the present disclosure, the raw material NdFeB alloy powder is a main phase material.
[0055] In some embodiments of the present disclosure, the mass percentage of the main phase material is higher than 90% of the material, preferably higher than 95%, preferably higher than 98%, and preferably the mass percentage of the main phase material is 97.5%-99.5%.
[0056] In some embodiments of the present disclosure, the diffusion is a grain boundary diffusion process using a heavy rare earth diffusion source.
[0057] In some embodiments of the present disclosure, the grain boundary diffusion treatment is performed by a magnetron sputtering method.
[0058] In some embodiments of the present disclosure, the grain boundary diffusion treatment is performed by coating, printing, or bonding methods.
[0059] In some embodiments of the present disclosure, the squareness of the magnet is greater than 0.8, preferably ≥0.82, preferably ≥0.83, preferably ≥0.84, preferably ≥0.85, preferably ≥0.86, preferably ≥0.87, preferably ≥0.88, preferably ≥0.89, preferably ≥0.9, preferably ≥0.91, preferably ≥0.92.
[0060] In some embodiments of the present disclosure, the hydrogen cracking temperature is 250-400°C, preferably 260-350°C, preferably 280-320°C, preferably 300°C.
[0061] In some embodiments of the present disclosure, the hydrogen pressure is 0.05-0.15 MPa, preferably 0.07-0.13 MPa, preferably 0.09-0.11 MPa, preferably 0.1 MPa.
[0062] In some embodiments of the present disclosure, the hydrogen cracking time is 5-15 h, preferably 7-13 h, preferably 9-11 h, preferably 10 h, preferably 7 h, preferably 5 h.
[0063] In some embodiments of the present disclosure, the average particle size of the rare earth alloy hydrogen-cracked powder and the raw material NdFeB alloy powder after grinding is 2-5 μm, preferably 3-5 μm, preferably 3.5-4.5 μm, preferably 4 μm.
[0064] In some embodiments of the present disclosure, the mass ratio of the alloy powder to the raw material NdFeB alloy powder is 0.5:100 to 2:100, preferably 1:100 to 1.8:100, preferably 1.4:100 to 1.6:100, preferably 1.5.
[0065] In some embodiments of the present disclosure, the sintering temperature is 1000-1100°C, preferably 1030-1090°C, preferably 1040-1080°C, preferably 1045-1070°C, preferably 1065°C, preferably 1060°C, preferably 1050°C.
[0066] In some embodiments of the present disclosure, the sintering time is 3-10 hours.
[0067] In some embodiments of the present disclosure, the grain boundary diffusion treatment includes a first heat treatment and a second heat treatment, the first heat treatment is performed before the second heat treatment, and the treatment temperature of the first heat treatment is higher than the treatment temperature of the second heat treatment.
[0068] In some embodiments of the present disclosure, the first heat treatment is performed at 800-950°C, preferably 850-950°C, preferably 900-940°C, preferably 920-930°C, preferably 925°C.
[0069] In some embodiments of the present disclosure, the time of the first heat treatment is 3-40 h, preferably 10-40 h, preferably 14 h-40 h, preferably 14 h, preferably 40 h.
[0070] In some embodiments of the present disclosure, the second heat treatment is performed at 450-550°C, preferably 480-530°C, preferably 500-520°C, preferably 510°C.
[0071] In some embodiments of the present disclosure, the time of the second heat treatment is 3-10 h, preferably 3-6 h, preferably 3-5 h, preferably 3 h, preferably 5 h.
[0072] In some embodiments of the present disclosure, the diffusion amount of heavy rare earth is 0.2%-2%, preferably 0.3%-1.5%, preferably 0.4%-1.2%, preferably 0.5%-1%, preferably 0.5%, 0.75% or 1%.
[0073] The present disclosure provides a neodymium iron boron magnet prepared according to the method of the present disclosure.
[0074] The present disclosure provides a NdFeB magnet comprising heavy rare earth elements diffused along an easy magnetization direction parallel to and / or perpendicular to a substrate.
[0075] In some embodiments of the present disclosure, the raw material NdFeB alloy powder is a NdFeB hydrogen-crushed powder obtained by hydrogen-crushing the raw material NdFeB alloy.
[0076] In some embodiments of the present disclosure, the raw material NdFeB alloy contains Nd, Fe and B, and the raw material NdFeB alloy also contains or does not contain one or more of Pr, Tb, Co, Ca, Cu, Al, and Zr, wherein the mass fraction of Nd is 10%-30%, the mass fraction of Fe is less than or equal to 72%, and the mass fraction of B is less than or equal to 1%.
[0077] In some embodiments of the present disclosure, the composition of the raw material NdFeB alloy is expressed as mass fraction as a subscript. 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 .
[0078] The present disclosure provides a powder composition, which comprises a first powder component and a second powder component, wherein the first powder component is an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R and 0≤x≤90; and the second powder component is a raw material neodymium iron boron alloy powder.
[0079] In some embodiments of the present disclosure, the first powder component is an alloy hydrogen-cracked powder obtained by hydrogen-cracked an alloy body.
[0080] In some embodiments of the present disclosure, the second powder component is a NdFeB hydrogen-crushed powder obtained by hydrogen-crushing a raw NdFeB alloy.
[0081] In some embodiments of the present disclosure, the powder composition is obtained by hydrogen cracking an alloy body that can obtain the first powder component and a raw material NdFeB alloy that can obtain the second powder component.
[0082] In some embodiments of the present disclosure, the composition is obtained by uniformly mixing the first powder component and the second powder component.
[0083] In some embodiments of the present disclosure, the mass ratio of the first powder component to the second powder component in the powder composition is 0.5:100 to 2:100, preferably 1:100 to 1.8:100, preferably 1.4:100 to 1.6:100, preferably 1.5.
[0084] In some embodiments of the present disclosure, the uniform mixing comprises jet milling the mixture.
[0085] In some embodiments of the present disclosure, the average particle size of the first powder component is 3 μm-5 μm, preferably 3.5-4.5 μm, preferably 4 μm.
[0086] In some embodiments of the present disclosure, the average particle size of the second powder component is 3 μm to 5 μm, preferably 3.5 to 4.5 μm, preferably 4 μm.
[0087] In some embodiments of the present disclosure, the powder composition has a particle size discreteness of no greater than 2, preferably no greater than 1.5, preferably no greater than 1.4, preferably no greater than 1.3, preferably no greater than 1.2, preferably no greater than 1.1, preferably no greater than 1.0, preferably no greater than 0.9, preferably no greater than 0.8, preferably no greater than 0.7, preferably no greater than 0.6, preferably no greater than 0.5, preferably no greater than 0.4, preferably no greater than 0.3, preferably no greater than 0.2, preferably no greater than 0.1.
[0088] Example
[0089] The present disclosure will be further described in detail below in conjunction with the embodiments of the accompanying drawings, but the present disclosure is not limited to these embodiments. The following embodiments are for illustrative purposes only and should not be used to limit the scope of the present disclosure and the claims.
[0090] Examples 1-6
[0091] The elements Nd and Al were mixed according to the Nd:Al mass ratio in Table 1. The mixed raw materials were placed in an arc melting furnace and smelted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-broken powder was mixed with a Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95The NdFeB hydrogen-crushed powders were mixed uniformly at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to obtain the NdFeB substrate. A heavy rare earth diffusion source was diffused parallel to the easy magnetization direction of the NdFeB substrate via magnetron sputtering. The heavy rare earth Tb diffusion thickness in the diffusion direction was 6mm, and the heavy rare earth Tb diffusion content was 1%. Heat treatment was then performed at 925°C for 14 hours and at 510°C for 3 hours to produce high-performance NdFeB magnets with excellent squareness.
[0092] Table 1
[0093] Examples 7-12
[0094] The elements Nd and Al were mixed according to the Nd:Al mass ratio in Table 2. The mixed raw materials were placed in an arc melting furnace and smelted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-broken powder was mixed with a Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 NdFeB hydrogen-crushed powders were mixed at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. Heavy rare earth diffusion sources were diffused perpendicular to the easy magnetization direction of the NdFeB substrate via magnetron sputtering. The Tb diffusion thickness in the diffusion direction was 8mm, and the Tb diffusion content was 1%. Heat treatments were then performed at 925°C for 40 hours and 510°C for 3 hours, resulting in high-performance NdFeB magnets with excellent squareness.
[0095] Table 2
[0096] Examples 13-16
[0097] The elements Nd and Al are added in a ratio of 87:13. 87 Al 13The prepared raw materials are placed in an arc melting furnace and smelted in an argon atmosphere to obtain a rare earth alloy ingot; the rare earth alloy ingot is hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa; the rare earth alloy hydrogen-broken powder is mixed with a composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 NdFeB hydrogen-crushed powders were mixed at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4 μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. Heavy rare earth (Tb) diffusion sources were diffused perpendicular to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness is shown in Table 3, and the Tb diffusion content was 1%. Heat treatments at 925°C for 40 hours and 510°C for 3 hours produced high-performance NdFeB magnets with excellent squareness.
[0098] Table 3
[0099] Examples 17-21
[0100] The elements Nd and Al are added in a ratio of 87:13. 87 Al 13 The prepared raw materials are placed in an arc melting furnace and smelted in an argon atmosphere to obtain a rare earth alloy ingot; the rare earth alloy ingot is hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa; the rare earth alloy hydrogen-broken powder is mixed with a composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95NdFeB hydrogen-crushed powders were mixed at a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4 μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. Heavy rare earth (Tb) diffusion sources were diffused parallel to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness is shown in Table 4, and the Tb diffusion content was 1%. Heat treatments at 925°C for 40 hours and 510°C for 3 hours produced high-performance NdFeB magnets with excellent squareness.
[0101] Table 4
[0102] Examples 22-26
[0103] The elements Pr and Cu were placed in an arc melting furnace according to the Pr:Cu mass ratio shown in Table 5, and the prepared raw materials were placed in an argon atmosphere and melted to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-destructed for 5 hours at a temperature of 350°C and a hydrogen pressure of 0.15 MPa. The rare earth alloy hydrogen-destructed powder and NdFeB hydrogen-destructed powder were uniformly mixed in a mass ratio of 1:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-destructed powder and sintered NdFeB hydrogen-destructed powder after jet milling was 3 μm. The sintered NdFeB magnetic powder after jet milling and the rare earth alloy powder were oriented and formed into a green compact, which was sintered at 1060°C for 5 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was applied by coating to the grain boundary diffusion parallel to the easy magnetization direction of the NdFeB substrate. The thickness of the heavy rare earth Dy diffusion direction was 10 mm, and the heavy rare earth Dy diffusion amount was 0.75%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 14 hours and at 510°C for 3 hours.
[0104] Table 5
[0105] Examples 27-31
[0106] The elements Nd and Zn were placed in an arc melting furnace according to the Nd:Zn mass ratio in Table 6, and the prepared raw materials were placed in an argon atmosphere and melted to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-destructed for 10 hours at a temperature of 250°C and a hydrogen pressure of 0.08 MPa. The rare earth alloy hydrogen-destructed powder and NdFeB hydrogen-destructed powder were uniformly mixed in a mass ratio of 2:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-destructed powder and sintered NdFeB hydrogen-destructed powder after jet milling was 5 μm. The sintered NdFeB magnetic powder and rare earth alloy powder after jet milling were oriented and formed into a green compact, which was sintered at 1050°C for 10 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was subjected to grain boundary diffusion treatment perpendicular to the easy magnetization direction of the NdFeB substrate by magnetron sputtering. The thickness of the heavy rare earth Dy diffusion direction was 8 mm, and the heavy rare earth Dy diffusion amount was 0.5%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 10 h and at 510°C for 5 h.
[0107] Table 6
[0108] Examples 32-36
[0109] The elements Pr and Cu were placed in an arc melting furnace with a Pr:Cu mass ratio of 80:20, and the prepared raw materials were placed in an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-decomposed for 5 hours at a temperature of 350°C and a hydrogen pressure of 0.15 MPa. The rare earth alloy hydrogen-decomposed powder and NdFeB hydrogen-decomposed powder were uniformly mixed in a mass ratio of 1:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-decomposed powder and sintered NdFeB hydrogen-decomposed powder after jet milling was 3 μm. The sintered NdFeB magnetic powder after jet milling and the rare earth alloy powder were oriented and formed into a green compact, which was sintered at 1060°C for 5 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was treated by grain boundary diffusion parallel to the easy magnetization direction of the NdFeB substrate by a coating method. The thickness of the heavy rare earth Dy diffusion direction is shown in Table 7, and the heavy rare earth Dy diffusion amount is 0.75%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 14 hours and at 510°C for 3 hours.
[0110] Table 7
[0111] Examples 37-41
[0112] The elements Nd and Zn were placed in an arc melting furnace with a Nd:Zn mass ratio of 80:20, and the prepared raw materials were placed in an argon atmosphere to obtain a rare earth alloy ingot; the rare earth alloy ingot was hydrogen-decomposed for 10 hours at a temperature of 250°C and a hydrogen pressure of 0.08 MPa; the rare earth alloy hydrogen-decomposed powder and NdFeB hydrogen-decomposed powder were uniformly mixed in a mass ratio of 2:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-decomposed powder and sintered NdFeB hydrogen-decomposed powder after jet milling was 5 μm; the sintered NdFeB magnetic powder and rare earth alloy powder after jet milling were oriented and formed into a green compact, and then sintered at 1050°C for 10 hours to obtain an NdFeB substrate; a heavy rare earth diffusion source was subjected to grain boundary diffusion treatment perpendicular to the easy magnetization direction of the NdFeB substrate by magnetron sputtering. The thickness of the heavy rare earth Dy diffusion direction was shown in Table 8, and the heavy rare earth Dy diffusion amount was 0.5%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 10 h and at 510°C for 5 h.
[0113] Table 8
[0114] Example 42
[0115] The sintered NdFeB magnetic powder (composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 After orientation molding, the compact was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth (Tb) diffusion source was diffused parallel to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness in the direction of the heavy rare earth (Tb) diffusion was 6 mm, and the Tb diffusion content was 1%. The NdFeB magnet was then heat treated at 925°C for 14 hours and at 510°C for 3 hours.
[0116] Example 43
[0117] The sintered NdFeB magnetic powder (composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95After orientation molding, the compact was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth (Tb) diffusion source was diffused perpendicular to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness was 8 mm and the Tb diffusion content was 1%. The NdFeB magnet was then heat treated at 925°C for 40 hours and then at 510°C for 3 hours.
[0118] Example 44
[0119] The sintered NdFeB magnetic powder (composition of Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95 After orientation molding, the compact was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth (Tb) diffusion source was diffused perpendicular to the easy magnetization direction of the NdFeB substrate using magnetron sputtering. The Tb diffusion thickness in the direction of diffusion was 10 mm, and the Tb diffusion content was 1%. The NdFeB magnet was then heat treated at 925°C for 40 hours and at 510°C for 3 hours.
[0120] Table 9
[0121] Comparing Figure 1(a)-(d), we can find that the introduction of R x M 100-x After alloying, the difference in the grain boundary phase content in different directions of the substrate is reduced, which effectively improves the anisotropy of the grain boundary phase distribution of the substrate and forms a continuous and narrow grain boundary inside the substrate. The electron probe results (Figure 2) show that the Tb element has a great influence on the growth of the R x M 100-x The alloy has a deeper diffusion depth in the matrix, the accumulation of heavy rare earth on the surface is significantly reduced, and the concentration gradient inside the magnet is slowed down. x M 100-x The alloyed NdFeB diffused magnets exhibited even better squareness. For a 10 mm thick substrate, the squareness of the magnets after Tb diffusion perpendicular to the easy magnetization direction still reached 0.92, significantly better than the 0.77 in Example 83.
[0122] By comparing the magnetic performance data of the embodiment and the comparative example, it can be seen that by introducing R x M 100-xBy regulating the distribution morphology and content of the grain boundary phase in different directions of the substrate, the squareness of the diffusion magnet is effectively improved, the accumulation of Tb elements on the surface of the magnet is reduced, and the utilization rate of heavy rare earths is effectively improved.
[0123] Examples 45-47
[0124] The elements Nd and Al were mixed in a mass ratio of Nd:Al of 87:13, and the mixed raw materials were placed in an arc melting furnace and melted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-decomposed for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-decomposed powder was uniformly mixed with NdFeB hydrogen-decomposed powder having the composition shown in Table 10 in a mass ratio of 1.5:100 and then jet-milled. The average particle size of the rare earth alloy hydrogen-decomposed powder and sintered NdFeB hydrogen-decomposed powder after jet milling was 4 μm. The sintered NdFeB magnetic powder after jet milling and the rare earth alloy powder were oriented and formed into a green compact, which was sintered at 1065°C for 6 hours to obtain an NdFeB substrate. A heavy rare earth diffusion source was subjected to grain boundary diffusion treatment parallel to the easy magnetization direction of the NdFeB substrate by magnetron sputtering. The thickness of the heavy rare earth Tb diffusion direction was 6 mm, and the heavy rare earth Tb diffusion amount was 1%. High performance NdFeB magnets with excellent squareness were obtained by heat treatment at 925°C for 14 hours and at 510°C for 3 hours.
[0125] Table 10
[0126] Examples 48-49
[0127] The elements Nd and Al were mixed in a mass ratio of 87:13. The mixed raw materials were placed in an arc melting furnace and smelted under an argon atmosphere to obtain a rare earth alloy ingot. The rare earth alloy ingot was hydrogen-broken for 7 hours at a temperature of 300°C and a hydrogen pressure of 0.10 MPa. The rare earth alloy hydrogen-broken powder was mixed with a Pr 6.95 Nd 22.14 Tb 0.12 Fe 68.95 Co 0.5 Ga 0.13 Cu 0.09 Al 0.06 Zr 0.11 B 0.95The NdFeB hydrogen-crushed powders were mixed uniformly according to the mass ratios specified in Table 11 and then jet-milled. The average particle size of the rare earth alloy hydrogen-crushed powder and sintered NdFeB hydrogen-crushed powder after jet milling was 4 μm. The jet-milled sintered NdFeB magnetic powder and rare earth alloy powder were oriented and compacted, and then sintered at 1065°C for 6 hours to produce an NdFeB substrate. A heavy rare earth diffusion source was diffused parallel to the easy magnetization direction of the NdFeB substrate via magnetron sputtering. The heavy rare earth Tb diffusion thickness in the diffusion direction was 6 mm, and the heavy rare earth Tb diffusion content was 1%. Heat treatment was then performed at 925°C for 14 hours and at 510°C for 3 hours, resulting in a high-performance NdFeB magnet with excellent squareness.
[0128] Table 11
[0129] The average particle size and particle size dispersion of the powder compositions obtained in Examples 1-49 were measured to obtain the measurement results shown in Table 12. The difference in the crystal interface area fraction parallel to the easy magnetization direction and perpendicular to the easy magnetization direction, the average particle size of the rare earth-rich phase particles, the proportion of rare earth-rich phase particles with a particle size greater than 3 μm to the total rare earth-rich phase particles, the grain boundary width, and the grain boundary length of the substrates obtained in Examples 1-49 were measured to obtain the measurement results shown in Tables 13-14.
[0130] Table 12
[0131] Table 13
[0132] Table 14
[0133] The above embodiments are intended only to illustrate the technical concepts and features of the present disclosure. Their purpose is to enable those skilled in the art to understand the contents of the present disclosure and implement them accordingly. They are not intended to limit the scope of protection of the present disclosure. Any equivalent changes or modifications made in accordance with the spirit of the present disclosure shall be included in the scope of protection of the present disclosure.
Claims
1. A NdFeB substrate, the substrate being in a sintered state, wherein the crystal interface area fraction of the substrate parallel to the easy magnetization direction and perpendicular to the easy magnetization direction is less than 2%.
2. The NdFeB substrate of claim 1, comprising a bulk agglomerated rare earth-rich phase.
3. The NdFeB substrate of claim 2, wherein the average particle size of the rare earth-rich phase particles is less than 2.4 microns.
4. The NdFeB substrate of claim 2, wherein the proportion of rare earth-rich phase particles having a particle size greater than 3 microns to all the rare earth-rich phase particles is less than 20%. 5 . The NdFeB substrate of claim 1 , comprising a grain boundary, wherein the width of the grain boundary is less than 0.5 μm, and the length of the grain boundary is 0.5 to 6 μm.
6. The NdFeB substrate according to claim 1, wherein the substrate is obtained by sintering a powder composition obtained by mixing a raw material NdFeB alloy powder with an alloy powder composed of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R, and 0 <x≤90。 7. A method for preparing a NdFeB magnet, the method comprising subjecting a NdFeB substrate to grain boundary diffusion treatment to obtain the NdFeB magnet, wherein the NdFeB substrate is in a sintered state, and the crystal interface area fraction of the substrate parallel to the easy magnetization direction and perpendicular to the easy magnetization direction is less than 2%.
8. The method for preparing a NdFeB magnet according to claim 7, wherein the heavy rare earth is diffused 8 mm along a direction perpendicular to the easy magnetization direction of the substrate, so that the squareness of the obtained NdFeB magnet is greater than or equal to 0.
85.
9. The method for preparing a NdFeB magnet according to claim 7, wherein the heavy rare earth is diffused along a direction perpendicular to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 8 mm.
10. The method for preparing a NdFeB magnet according to claim 7, wherein the heavy rare earth is diffused in a direction parallel to the easy magnetization direction of the substrate, and the diffusion depth is greater than or equal to 8 mm.
11. The method for preparing a NdFeB magnet according to any one of claims 8 to 10, wherein the heavy rare earth is one or both of Dy and Tb.
12. The method for preparing a NdFeB magnet according to claim 7, wherein the NdFeB substrate is obtained by sintering a powder composition obtained by mixing a raw NdFeB alloy powder with an alloy powder consisting of R and M, wherein the mass ratio of R to M is x:(100-x), R is one or more of Nd and Pr, M is one or a combination of two or more of Cu, Al, Ga, and Zn, x is the mass fraction of R, and 0 <x≤90。
Citation Information
Patent Citations
R-Fe-B microcrystalline high-density magnet and process for production thereof
CN101379574A
Sintered neodymium-iron-boron magnet and preparation method thereof
CN105702403A
Neodymium iron boron permanent magnet material and preparation method thereof
CN108074693A
R-fe-b sintered magnet and production method therefor
CN109997203A
Neodymium iron boron base material
CN116453792A