Structure manufacturing method and structure

The method of using a conductive composition with small metal nanoparticles on non-flat surfaces addresses the issues of conductivity loss and discharge instability by forming a stable and conductive layer through deposition and sintering, ensuring consistent performance even on deformed substrates.

WO2024237008A1PCT designated stage expired Publication Date: 2024-11-21DAICEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015454
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-04-18
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional methods for forming conductive layers on non-flat surfaces face challenges such as decreased conductivity due to deformation of the conductive layer when the base material is processed, and issues with nozzle clogging during continuous dispensing of conductive paste, leading to instability in the discharge process.

Method used

A method involving the use of a conductive composition with metal nanoparticles of less than 50 nm average particle diameter, applied to a non-flat surface through a deposition step, followed by sintering to form a conductive layer, which ensures stability during continuous discharge and maintains excellent conductivity.

Benefits of technology

The method effectively forms a conductive layer on non-flat surfaces with enhanced stability and conductivity, preventing degradation during deformation of the base material and ensuring consistent discharge, while minimizing nozzle clogging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015454_21112024_PF_FP_ABST
    Figure JP2024015454_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a structure manufacturing method, with which it is possible to form a conductive layer on a base material that has a non-flat surface and to achieve excellent stability during continuous ejection. Also provided is a structure which is provided with a conductive layer having excellent conductivity on a base material that has a non-flat surface. This manufacturing method is for manufacturing a structure 1 comprising: a base material 2 that has non-flat surfaces 2a-2d; and a conductive layer 3 that is formed on the non-flat surfaces 2a-2d of the base material 2. The manufacturing method comprises an adhesion step for forming a metal film by having a conductive composition adhered to the non-flat surface 2a of the base material 2, the conductive composition containing metal nanoparticles that have an average particle diameter of less than 50 nm with the content ratio of the metal nanoparticles being 1-66% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a structure and the structure

[0001] The present disclosure relates to a method for manufacturing a structure and the structure. The present disclosure relates to a structure including a conductive layer formed on a non-flat surface of a substrate, and a method for manufacturing the structure. This application claims priority from Japanese Patent Application No. 2023-080191, filed in Japan on May 15, 2023, the contents of which are incorporated herein by reference.

[0002] Metal nanoparticles, such as silver nanoparticles, can be fired even at low temperatures. Taking advantage of this property, metal compositions containing metal nanoparticles are used to form metal coating patterns, such as electrodes and conductive circuit patterns, on substrates in the manufacture of various electronic devices. The metal composition contains metal particles and an organic solvent for dispersing the metal particles. The metal nanoparticles have an average primary particle size of several nanometers to several tens of nanometers. The metal composition is applied to a substrate to form a pattern, and then fired to volatilize the organic solvent in the metal composition while sintering and fusing the metal nanoparticles to form a conductive layer, such as an electrode, conductor wiring, or conductive circuit pattern.

[0003] Known methods for producing a structure comprising a conductive layer such as conductor wiring on a substrate having an uneven surface include a method in which a conductive layer is formed on a flat substrate and then the substrate is processed, such as by bending, to form an uneven surface (see Patent Document 1), and a method in which a conductive layer is formed by printing, by dispense printing, a conductive paste containing metal particles having an average particle size of 0.05 to 5 μm on the uneven surface of a substrate on which an uneven surface has already been formed (see Patent Documents 2 and 3).

[0004] JP 2020-123633 A JP 2017-19271 A International Publication No. 2016 / 039327

[0005] However, when a non-flat surface is formed by forming conductor wiring on a flat substrate and then bending or otherwise processing it, the conductive layer also deforms along with the deformation of the substrate, which can cause the conductivity of the conductive layer to deteriorate compared to before processing, resulting in a loss of conductivity. Furthermore, in conventional methods of printing a conductor paste using metal particles with an average particle size of 0.05 to 5 μm onto a non-flat surface by dispense printing, there was a problem that when the paste was continuously dispensed using a dispenser, the nozzle of the dispenser would clog, making it difficult to stabilize the weight of the dispensed paste.

[0006] Therefore, an object of the present disclosure is to provide a method for manufacturing a structure that can form a conductive layer on a substrate having an uneven surface and that has excellent stability during continuous discharge. Another object of the present disclosure is to provide a structure that includes a conductive layer with excellent conductivity on a substrate having an uneven surface.

[0007] As a result of intensive research to solve the above problems, the inventors of the present disclosure have found that a conductive layer can be formed on a substrate having an uneven surface and has excellent stability during continuous discharge by including a step of forming a metal film by adhering a specific conductive composition containing metal nanoparticles with an average particle size of less than 50 nm to the uneven surface of the substrate. The present disclosure relates to a product completed based on these findings.

[0008] That is, the present disclosure provides a method for manufacturing a structure including a substrate having an uneven surface and a conductive layer formed on the uneven surface of the substrate, the method comprising an attachment step of attaching, to the uneven surface of the substrate, a conductive composition containing metal nanoparticles having an average particle size of less than 50 nm, the metal nanoparticles being present in an amount of 1 to 66 mass %, to form a metal film.

[0009] The manufacturing method preferably includes, after the deposition step, a firing step of sintering the metal film to form the conductive layer.

[0010] Preferably, the deposition is printing, which does not include screen printing.

[0011] Preferably, the metal nanoparticles comprise silver and / or copper.

[0012] The non-flat surface preferably includes at least a curved surface, a convex surface, or a concave surface.

[0013] The content of metal microparticles having a particle size of 1 μm or more in the conductive composition is preferably less than 1 per 100 total particles of the metal nanoparticles.

[0014] The present disclosure also provides a structure comprising: a substrate having an uneven surface; and a conductive layer formed on the uneven surface of the substrate, wherein at least a portion of the conductive layer has a porosity of 0.01 to 50%.

[0015] The conductive layer preferably has a volume resistivity of 1000 μΩ·cm or less.

[0016] The thickness of the conductive layer is preferably 0.05 to 1000 μm.

[0017] The non-flat surface preferably includes at least a curved surface, a convex surface, or a concave surface.

[0018] According to the method for manufacturing a structure of the present disclosure, a conductive layer can be formed on a substrate having an uneven surface, and the method has excellent stability during continuous discharge. Furthermore, according to the structure of the present disclosure, a structure can be provided which includes a conductive layer having excellent conductivity on a substrate having an uneven surface.

[0019] 1A-1C show partial cross-sectional views of a structure according to one embodiment of the present disclosure, FIG. 1B show partial cross-sectional views of a structure according to another embodiment of the present disclosure, FIG. 1C show partial cross-sectional views of a structure according to yet another embodiment of the present disclosure, and FIG. 1D show partial cross-sectional views of a structure according to yet another embodiment of the present disclosure.

[0020] [Method for manufacturing a structure] The method for manufacturing a structure of the present disclosure is a method for manufacturing a structure including a substrate having an uneven surface and a conductive layer formed on the uneven surface of the substrate. The method includes at least a step (adhering step) of forming a metal film by adhering a conductive composition containing metal nanoparticles having an average particle size of less than 50 nm to the uneven surface of the substrate. The method may further include a step (firing step) of sintering the metal film after the adhering step to form the conductive layer.

[0021] Examples of the non-flat surface of the substrate include curved surfaces, concave surfaces, convex surfaces, and surfaces comprising two or more of these (for example, uneven surfaces). Examples of structures having a curved surface include structures having curved portions, such as a shape having at least a portion of a cylindrical body, a structure having at least a portion of a sphere, and a shape having at least a portion of a tile-like shape. In addition, for example, when a conductive composition is continuously applied from the first surface of a sheet-like substrate having flat first and second surfaces via the side to the second surface, the application track (printing track) continuously passes through a first region and a second region that is not on the same plane as the first region. This specification also includes examples of microscopically uneven surfaces (for example, an arithmetic mean roughness Ra of less than 0.1 mm), such as a surface roughened by pre-treating the substrate or a surface on which minute irregularities are formed. These do not fall under the category of "non-flat surface," and whether a surface is non-flat is determined by macroscopically viewing the surface.

[0022] The structure having a concave, convex, or uneven surface includes a structure having at least a portion of a step, a shape having at least a portion of a ridge shape, a shape having at least a portion of a groove shape, a structure having a combination of two or more of these, etc. Furthermore, the structure having a convex surface includes, for example, a structure in which two or more flat surfaces are joined together and share one side or one vertex (for example, the corner of a prism such as a rectangular parallelepiped).

[0023] The concave structure may be a hollow portion such as a groove. The cross-sectional shape of the hollow portion is not particularly limited, and may be a polygon such as a triangle or a square, or a circle. From the viewpoint of ease of attachment, the hollow portion preferably has an opening of 1 cm or more.

[0024] When the non-flat surface has an uneven surface, the maximum unevenness difference may be 0.1 mm or more, 0.3 mm or more, or 0.5 mm or more. The maximum unevenness difference is the maximum difference between adjacent convex and concave portions. According to the manufacturing method, when the maximum unevenness difference is large, the conductive composition can be more uniformly applied to the uneven surface.

[0025] When the non-flat surface has a curved surface, the radius of curvature may be 100 mm or less, 80 mm or less, 60 mm or less, or 10 mm or less. The radius of curvature may be, for example, 0.1 mm or more, 1 mm or more, or 5 mm or more. The radius of curvature may be the radius when the curved surface is convex or concave. Furthermore, the side on which the conductive layer is provided may be the inner side (i.e., the side of the center point of a circle whose radius is the radius of curvature) or the outer side when the curved surface of the substrate having the non-flat surface is an arc. The larger the radius of curvature, the closer the surface becomes to flatness, allowing the conductive composition to be more uniformly applied. Furthermore, according to the above manufacturing method, the conductive composition can be more uniformly applied to the curved surface, even when the radius of curvature is small, and also on the outer side of the curved surface. Furthermore, when the substrate is cylindrical, columnar, conical, or frustum-shaped, the radius (in the case of a cylinder, column, cone, truncated cone, etc.) or the radius of the circumscribed circle of the cross section (in the case of a rectangular cylinder, column, pyramid, truncated pyramid, etc.) is preferably within the above range. The larger the radius and the radius of the circumscribed circle, the closer to flatness the substrate becomes, allowing the conductive composition to be applied more uniformly. Furthermore, according to the above manufacturing method, the conductive composition can be applied more uniformly even when the radius and the circumscribed circle are small.

[0026] When the non-flat surface has a convex surface, the angle of the convex portion is less than 180°, and may be 150° or less, or 120° or less. The angle of the convex portion is, for example, 1° or more, preferably 30° or more, and more preferably 50° or more.

[0027] The angle (tilt angle) of the slope connecting the convex and concave portions of the uneven surface with respect to the horizontal plane (if the angle changes gradually, the angle at the midpoint of the cross section of the slope) is preferably less than 90° on the acute angle side, more preferably 70° or less, and even more preferably 40° or less. If the tilt angle is less than 90°, the conductive composition can be more uniformly applied to the non-flat surface by the manufacturing method.

[0028] The distance from the apex of any convex portion to the apex of the convex portion adjacent to that convex portion (the distance between adjacent convex portions) is, for example, 0.1 mm or more, preferably 0.3 mm or more, more preferably 0.5 mm or more, and even more preferably 1 mm or more. When the distance between convex portions is 0.01 mm or more, the conductive composition can be more uniformly applied to the non-flat surface by the above-mentioned manufacturing method.

[0029] Specific examples of the non-flat surface include those having at least a portion thereof a structure such as the outer surface of a cylinder, rectangular prism, cone, pyramid, truncated cone, sphere, or ellipsoid, the inner or outer surface of a cylinder, rectangular tube, or ring, the inner or outer surface of a bellows, the convex or concave surface of a spherical crown, the inner or outer surface of a tile-shaped surface, the inner or outer surface of an octopus pot-shaped surface, a stepped shape, or the inner or outer surface of another polyhedron.

[0030] 1 to 4 show embodiments of structures obtained by the method for manufacturing a structure of the present disclosure. The structure 1 shown in Fig. 1 comprises a substrate 2 having a non-flat surface 2a and a conductive layer 3 formed on the non-flat surface 2a of the substrate 2. In the structure 1 shown in Fig. 1, the non-flat surface 2a is an uneven surface, D1 represents the difference in unevenness, D2 represents the distance between the convex portions, and θ represents the tilt angle.

[0031] The structure 1 shown in Figure 2 includes a substrate 2 having an uneven surface 2b and a conductive layer 3 formed on the uneven surface 2b of the substrate 2. In the structure 1 shown in Figure 2, the uneven surface 2b is an uneven surface with convex portions formed by hemispherical curved surfaces and concave portions formed by the planes between the hemispheres. D1 indicates the difference in unevenness and is the distance from the apex of the hemispherical convex portion to the concave portion. D2 indicates the distance between the convex portions and is the distance between the apexes of the hemispheres. θ indicates the inclination angle and is the angle formed by the horizontal plane and the midpoint of the inclination connecting the apex of the convex portion and the concave portion.

[0032] The structure 1 shown in Fig. 3 includes a substrate 2 having an uneven surface 2c and a conductive layer 3 formed on the uneven surface 2c of the substrate 2. In the structure 1 shown in Fig. 3, the substrate 2 is cylindrical, and the uneven surface 2c is a curved surface that is the outer circumferential surface of the cylinder. r is the radius of the outer circumferential cross section of the cylindrical substrate, and is the radius of curvature of the uneven surface 2c.

[0033] The structure 1 shown in Fig. 4 includes a substrate 2 having an uneven surface 2d, and a conductive layer 3 formed on the uneven surface 2d of the substrate 2. In the structure 1 shown in Fig. 4, the uneven surface 2d is an uneven surface, D1 represents the unevenness difference, D2 represents the distance between the convex portions, and θ represents the tilt angle.

[0034] According to the manufacturing method, the conductive composition can be evenly applied to the entire surface of the non-flat surface (e.g., the concave, inclined, and convex portions of the uneven portion), but it may also be applied in a spotted or continuous manner to one or more of the concave, inclined, and convex portions, for example, only to the concave portions or only to the convex portions.

[0035] (Substrate) The substrate (substrate) may be any known or commonly used material for providing the metal layer. The substrate may be a conductive substrate, a non-conductive substrate, or a dielectric material. The substrate may be a single layer or a multi-layer structure in which multiple layers are laminated.

[0036] Examples of materials for forming the non-conductive substrate include resins, glass, ceramics, wood, paper, etc. Examples of the resin include heat-resistant plastics such as polyimide resins, polycarbonate resins, isocyanate resins, melamine resins, and glass epoxy resins, as well as polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene and polypropylene, acrylic resins, epoxy resins, phenolic resins, and polyamide resins, as well as resins with low heat resistance such as polychlorinated biphenyl (PCB), liquid crystal polymers (LCP), vinyl chloride, molded resins, and epoxy resins, and combinations thereof may also be used.

[0037] Examples of the conductive substrate include metal substrates such as metal foils and metal plates formed from metals (copper, iron, alloys thereof, etc.); carbon substrates such as carbon cloth, carbon paper, and graphite; composite substrates such as conductive particle-containing films, conductive fiber-containing films, metal mesh films, metal-plated films, and optical laminates having a transparent conductive layer; resin substrates such as conductive polymer films; metal wire-containing films; and metal film laminates (printed circuit boards, etc.) having a metal (silver, copper, etc.) film on a part or all of a non-conductive substrate, and combinations of these may also be used.

[0038] Examples of the substrate include semiconductor elements such as IGBTs, diodes, Schottky barrier diodes, MOS-FETs, thyristors, logic circuits, sensors, analog integrated circuits, LEDs, semiconductor lasers, and oscillators; lead frames, metal plate-attached ceramic substrates (for example, DBC), piezoelectric materials (for example, inorganic materials such as quartz, zinc oxide, and lead zirconate titanate, and organic materials such as polylactic acid), transparent conductive films, semiconductor packages, and LED packages; power supply members such as copper ribbons, metal blocks, and terminals; heat sinks; water-cooled plates; lenses for eyeglasses and sunglasses; glass (automotive glass such as windshields, side windows, and rear windows of automobiles); sensor covers; thermal transfer rollers; printed circuit boards; vias in printed circuit boards; displays of personal computers, televisions, and the like; convex mirrors; traffic lights; smartphones; wearable devices such as watches and earphones; writing implements; glass slides; and office automation equipment such as mice.

[0039] (Conductive Composition) The conductive composition can take various forms without any particular limitation. For example, a conductive composition called a metal ink can be prepared by dispersing metal nanoparticles in a suspension state in an appropriate solvent (dispersion medium, particularly an organic solvent). Alternatively, a conductive composition called a metal paste can be prepared by dispersing metal nanoparticles in a kneaded state in a solvent. Only one type of metal nanoparticle can be used, or two or more types (e.g., metal nanoparticles having different constituent metals or metal nanoparticles with different average particle sizes) can be used.

[0040] The conductive composition contains metal nanoparticles. The average particle size of the metal nanoparticles is less than 50 nm, preferably 0.5 nm or more but less than 50 nm, more preferably 1 to 45 nm, and even more preferably 1 to 40 nm. The average particle size is the size excluding the protective agent that coats the surface (i.e., the size of the metal nanoparticles themselves). The average particle size is determined as the number-average particle size based on particle sizes determined by observation with a transmission electron microscope (TEM). Only one type of metal nanoparticle may be used, or two or more types may be used. When two or more types of metal nanoparticles are contained, the average particle size refers to the average particle size of all the metal nanoparticles.

[0041] In one embodiment, the average particle size of the metal nanoparticles is preferably less than 40 nm, more preferably 30 nm or less, and even more preferably 20 nm or less. In this case, excellent conductivity is achieved when a conductive layer having a thickness of 1 μm or less is formed. In addition, in this embodiment, the porosity of the formed conductive layer may be approximately 15 to 25%.

[0042] In another embodiment, the average particle size of the metal nanoparticles is preferably 40 nm or more but less than 50 nm. In this case, when a conductive layer having a thickness of 1 μm or more is formed, the conductive layer has excellent conductivity. In this embodiment, the porosity of the formed conductive layer may be approximately 0.01 to 10%.

[0043] Examples of metals constituting metal nanoparticles include conductive metals, such as gold, silver, copper, nickel, aluminum, rhodium, cobalt, ruthenium, platinum, palladium, chromium, indium, etc. Among these, silver particles (i.e., silver nanoparticles) or copper particles (i.e., copper nanoparticles) are preferred as the metal nanoparticles, since they can be fused to each other at a temperature of about 100°C and form connecting members for electronic components and the like that are conductive even on general-purpose plastic substrates with low heat resistance.

[0044] The shape of the metal nanoparticles is not particularly limited, and examples thereof include spherical (including spherical and elliptical), flake (scale-like), dendritic, and lumpy shapes. Of these, spherical shapes are preferred.

[0045] Furthermore, surface-modified metal particles having a configuration in which the surfaces of metal nanoparticles are coated with an organic protective agent are preferred. That is, the metal nanoparticles are preferably surface-modified metal nanoparticles. Surface-modified metal nanoparticles ensure spacing between metal nanoparticles, suppress aggregation, and have excellent dispersibility in solvents. The metal constituting the metal nanoparticles is appropriately selected depending on the constituent components of the metal layer.

[0046] The organic protective agent is not particularly limited, and examples thereof include known or commonly used organic protective agents used as protective agents (stabilizers) for metal particles. Examples of the organic protective agent include organic protective agents having functional groups such as carboxyl groups, hydroxyl groups, carbonyl groups, amide groups, ether groups, amino groups, sulfo groups, sulfonyl groups, sulfinic acid groups, sulfenic acid groups, mercapto groups, phosphate groups, and phosphite groups. Among the functional groups, carboxyl groups, hydroxyl groups, amino groups, sulfo groups, and mercapto groups are preferred, and amino groups are more preferred. The organic protective agents may be used alone or in combination of two or more.

[0047] The content of the metal nanoparticles in the conductive composition is 1 to 66 mass %, preferably 10 to 65 mass %, and more preferably 40 to 64 mass %, relative to 100 mass % of the total amount of the conductive composition.

[0048] As the solvent, any known or conventional solvent used for dispersing metal particles can be used, and examples thereof include aliphatic hydrocarbons such as pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, and tetradecane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; aromatic hydrocarbons such as toluene, xylene, and mesitylene; alcohols such as methanol, ethanol, propanol, n-butanol, n-pentanol, n-hexanol, n-heptanol, n-octanol, n-nonanol, n-decanol, and menthol; diethylene glycol dibutyl ether, diethylene glycol methyl-n-butyl ether, and diethylene glycol-n-butyl ether acetate. Examples of suitable solvents include water and organic solvents such as ethers, including glycol ethers such as ethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl isopentyl ether, dipropylene glycol monobutyl ether, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl n-butyl ether, dipropylene glycol methyl cyclopentyl ether, triethylene glycol dimethyl ether, triethylene glycol methyl n-butyl ether, tripropylene glycol methyl n-propyl ether, tripropylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether. Examples of suitable solvents include terpene-based solvents such as terpineol and dihydroterpineol. The terpene-based solvents are preferably incorporated into metal pastes. The type and amount of the solvent can be determined appropriately depending on the concentration and viscosity of the desired conductive composition (metal ink, metal paste). One or more of the solvents may be used. Among these, alcohols, ethers, hydrocarbons, and terpene-based solvents are preferred.

[0049] The content of the solvent (particularly the organic solvent) in the conductive composition is preferably 0.5 to 99 mass %, more preferably 2 to 80 mass %, and even more preferably 5 to 60 mass %, relative to 100 mass % of the total amount of the conductive composition. When the content is within the above range, the dispersibility of the metal nanoparticles is superior.

[0050] The total content of the metal components (metal nanoparticles, as well as metal resinates and metal nanowires described below) and the solvent in the conductive composition is preferably 1.5% by mass or more, more preferably 50% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, relative to 100% by mass of the total amount of the conductive composition.

[0051] The conductive composition may contain other components in addition to the metal nanoparticles and the organic solvent. The conductive composition may contain a binder resin, for example, to adjust the viscosity of the conductive composition. Only one type of binder resin may be used, or two or more types may be used. Examples of the binder resin include known or commonly used binder resins that are incorporated into conductive compositions, such as vinyl chloride-vinyl acetate copolymers, polyvinyl butyral resins, polyester resins, acrylic resins, and cellulose resins (e.g., ethyl cellulose). The content of the binder resin in the conductive composition is, for example, 10% by mass or less. From the viewpoint of excellent conductivity of the metal layer, the content is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0.01% by mass or less.

[0052] Examples of the other components include conductive particles other than metal nanoparticles (e.g., metal nanowires, metal resinates, etc.), additives such as dispersants, surface energy adjusters, plasticizers, leveling agents, antifoaming agents, and adhesion promoters. Only one of the other components may be used, or two or more of them may be used.

[0053] The conductive composition preferably does not substantially contain metal particles (metal microparticles) having a particle diameter of 1 μm or more. The content of the metal microparticles in the conductive composition is preferably less than 1, more preferably less than 0.5, even more preferably less than 0.1, and particularly preferably less than 0.01 per 100 of the total amount of the metal nanoparticles. The presence or absence of the particle diameter of the metal microparticles and the content of the metal microparticles can be confirmed by the above-mentioned transmission electron microscope (TEM) observation.

[0054] The shear rate of the conductive composition is 10 s -1 The viscosity at is preferably 1 to 70,000 mPa, more preferably 5 to 50,000 mPa.

[0055] The conductive composition is applied to the substrate having the uneven surface via at least the uneven surface. The substrate may include a receiving layer on the uneven surface side. Examples of the receiving layer include coating layers such as a primer layer, an easy-adhesion treatment layer, and a hard coat layer. Among these, a primer layer is preferred. The method for producing a structure of the present disclosure may include a step of forming the receiving layer on the substrate. The receiving layer can be formed, for example, by applying and curing a composition layer containing a binder such as a curable resin or a thermoplastic resin. The receiving layer can be formed, for example, by kneading the binder using a known or conventional kneading method (such as melt kneading), forming a sheet or film, and then attaching it to the substrate, or by dissolving the binder in an organic solvent, applying it to the substrate to form a coating film, and then drying and curing it.

[0056] The method for applying the conductive composition in the step of forming a metal film (adhesion step) is not particularly limited, and any known or conventional application method can be used. Examples include spin coating, inkjet printing, screen printing, spray printing, dispense printing, relief printing (flexographic printing), dye-sublimation printing, offset printing, laser printer printing (toner printing), intaglio printing (gravure printing), contact printing, microcontact printing, ultra-precise deposition (UPD), electrohydrodynamic printing (EHD printing), laser-induced forward transfer (LIFT), and aerosol jet printing. Only one of the above application methods may be used, or two or more may be used in combination. Among these, printing is preferred. From the viewpoints of ease of printing and excellent stability during continuous discharge due to the use of the conductive composition, printing that does not include screen printing is preferred. Dispense printing, inkjet printing, and spray printing are more preferred, and dispense printing is even more preferred.

[0057] In the step of sintering the metal film to form the conductive layer (firing step), the metal composition constituting the metal film obtained through the deposition step is fired. Through the firing step, the solvent in the metal composition volatilizes (evaporates) and the metal nanoparticles are sintered together to form a metal layer.

[0058] The baking method includes thermal baking (IH, etc.), light baking (UV irradiation, etc.), reduced pressure baking, etc. The baking methods may be used alone or in combination of two or more.

[0059] The temperature (baking temperature) during the baking can be, for example, 900°C or less, preferably 500°C or less, more preferably 200°C or less, even more preferably room temperature (e.g., 25°C) to 150°C, and particularly preferably room temperature (e.g., 25°C) to 120°C. Baking temperatures of 200°C or less (particularly 180°C or less) can suppress thermal deformation even when the substrate is made of a material that is prone to thermal deformation, such as plastic. In particular, when it is desired to complete the baking of metal by short-term baking, it is recommended to perform the baking at, for example, 60 to 200°C, preferably 70 to 180°C, more preferably 80 to 150°C, and even more preferably 90 to 120°C. The baking time can be appropriately determined taking into account the type of conductive composition, the amount of adhesion, the baking temperature, etc., and is, for example, within several hours (e.g., within 40 seconds to 33 hours), preferably within 1 hour, more preferably within 50 minutes, even more preferably 10 to 40 minutes, and particularly preferably 15 to 30 minutes.

[0060] In the method for manufacturing a structure of the present disclosure, the combination of the deposition step and the firing step may be performed only once, or may be repeated two or more times. By repeating the combination of the deposition step and the firing step two or more times, a thick metal layer can be formed. Furthermore, when the combination is repeated two or more times, only one type of conductive composition may be used (i.e., the same conductive composition may be used), or two or more types may be used.

[0061] Furthermore, in the method for manufacturing a structure of the present disclosure, the baking step may be performed after the above-mentioned deposition step is performed multiple times. For example, it is possible to use conductive compositions with different compositions suitable for each shape, such as thin lines, thick lines, and solid paint. In such cases, the deposition step can be performed by changing the printing method and type of ink according to the printing location and printing pattern, and multiple metal films can be baked at once in a single baking step to manufacture a structure. The conductive compositions used in the multiple deposition steps may be only one type (i.e., the same conductive composition) or two or more types (i.e., different conductive compositions).

[0062] [Structure] The above manufacturing method provides a structure comprising the substrate and the conductive layer formed on the non-flat surface of the substrate, wherein the porosity of at least a portion of the conductive layer is 0.01 to 50%.

[0063] (Conductive Layer) The conductive layer is a layer composed of the conductive composition. The conductive layer is a layer having electrical conductivity and may contain components other than the metals composed of the conductive composition.

[0064] The conductive layer has a porosity of 0.01 to 50%, preferably 0.1 to 40%, and more preferably 1 to 30%, when measured by taking out a portion of the conductive layer. Having the porosity within this range ensures excellent conductivity even when the conductive layer is formed on an uneven surface. In one embodiment, the porosity may be 15 to 25%. In another embodiment, the porosity may be 0.01 to 10%, or 0.05 to 5%.

[0065] The porosity can be calculated by taking out a part of the conductive layer, exposing the cross section, observing the cross section of the conductive layer using a scanning electron microscope, analyzing the obtained cross-sectional image, and calculating the metal occupancy rate using the following formula: porosity [%] = 100 - occupancy rate [%]

[0066] A conductive layer containing voids can be produced, for example, by using a conductive composition containing the metal nanoparticles, applying the conductive composition, volatilizing (evaporating) the solvent, and sintering the remaining metal nanoparticles. More specifically, it can be produced by the above-mentioned manufacturing method. In this case, the metal nanoparticles are fused together by melting the surfaces of the metal nanoparticles to form a conductive layer, and at the same time, the gaps between the metal nanoparticles are not completely filled, resulting in the presence of voids in the conductive layer. The porosity in the conductive layer can be adjusted by appropriately selecting the particle size of the metal nanoparticles, the type of metal, etc.

[0067] The metal content in the conductive layer is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, relative to 100% by mass of the total amount of the conductive layer.

[0068] The thickness of the conductive layer is preferably 0.05 to 1000 μm, more preferably 0.1 to 500 μm, even more preferably 0.2 to 100 μm, and particularly preferably 0.3 to 50 μm. A thickness of 0.05 μm or more provides sufficient thickness and excellent conductivity. Furthermore, the above manufacturing method makes it possible to uniformly produce a conductive layer having a thickness of 1000 μm or less. The thickness of the conductive layer is selected appropriately depending on the deposition method, but is preferably 2 μm or less.

[0069] The conductive layer can be used as conductor wiring, an electrode, an electromagnetic wave shielding layer, a design layer, etc. The width of the conductive layer is not particularly limited, and may be, for example, 3 mm or less (e.g., 0.01 to 3 mm), 1 mm or less (e.g., 0.05 to 1 mm), 500 μm or less, or 400 μm or less. When the width of the conductive layer is 3 mm or less, it can be preferably used as conductor wiring.

[0070] The volume resistivity of the conductive layer is, for example, 1000 μΩ cm or less, preferably 500 μΩ cm or less, more preferably 100 μΩ cm or less, even more preferably 30 μΩ cm or less, and particularly preferably 10 μΩ cm or less. According to the above-mentioned production method, a conductive layer having excellent conductivity can be formed, and the above-mentioned volume resistivity value is sufficiently low, so that the conductive layer can be preferably used in devices that require only low voltage (for example, in-vehicle heating elements and antennas).

[0071] The voltage that the conductive layer can handle is preferably 10,000 V or less, more preferably 1,000 V or less, and even more preferably 100 V or less. There is no lower limit to the voltage that can be handled, but it may be, for example, 0.0000001 V or more, 0.000001 V or more, or 0.00001 V or more. When the voltage is 10,000 V or less, the structure can be preferably used in low-voltage applications. The conductive layer is considered to be "handled" if it does not break when a certain voltage is applied to it.

[0072] The above structure can be applied to, for example, electrical and electronic devices such as electromagnetic wave control materials, circuit boards, antennas, heat sinks, liquid crystal displays, organic EL displays, field emission displays (FEDs), IC cards, IC tags, solar cells, LED elements, piezoelectric elements, heaters, organic transistors, condensers (capacitors), electronic paper, flexible batteries, flexible sensors, membrane switches, touch panels, and electromagnetic wave shields.

[0073] According to the above-described method for manufacturing a structure, a conductive layer can be formed on a substrate having an uneven surface, and the stability during continuous discharge is excellent. When the substrate is deformed after the conductive layer is formed, the conductivity of the conductive layer must be maintained, which imposes constraints on the deformation process. However, according to the above-described manufacturing method, as described above, the conductive layer can be formed by directly adhering it to a substrate having a pre-deformed uneven surface. Therefore, there is no need to deform the substrate after forming the conductive layer, and there are no process constraints, and the conductive layer can be formed on substrates of various shapes. Furthermore, according to the structure of the present disclosure, a structure can be provided which has a conductive layer with excellent conductivity on a substrate having an uneven surface.

[0074] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Each configuration and combination thereof in each embodiment is an example, and addition, omission, substitution, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. Furthermore, each invention according to this disclosure is not limited by the embodiments or the following examples, but is limited only by the scope of the claims.

[0075] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.

[0076] The conductive compositions used in the examples and comparative examples are as follows: Ink 1: Silver nanoparticle ink (number average particle diameter of silver nanoparticles: 44.7 nm, silver concentration: 63 mass %, non-aqueous solvent, shear rate: 10 s -1 Ink 2: Silver nanoparticle ink (number average particle diameter of silver nanoparticles 14.5 nm, silver concentration 50 mass %, hydrocarbon / alcohol solvent, shear rate 10 s -1 Ink 3: Silver nanoparticle ink (number average particle diameter of silver nanoparticles: 44.7 nm, silver concentration: 67% by mass, non-aqueous solvent, shear rate: 10 s -1 Ink 4: Silver microparticle ink (number average particle diameter of silver microparticles: 1 μm, silver concentration: 92% by mass, non-aqueous solvent)

[0077] (Average Particle Diameter of Silver Particles) The number-average particle diameter of silver particles in the inks used in the following Examples and Comparative Examples was measured by the following method. The number-average particle diameter of silver particles was measured by dropping ink onto a copper mesh and observing it using a transmission electron microscope (trade name "JEM-1200EXII", manufactured by JEOL Ltd.) in a standard manner. 300 silver particles were randomly selected from the obtained image, and the particle diameter of each was measured. The average value of these measurements was calculated as the average primary particle diameter.

[0078] Example 1 Ink 1 was applied to the uneven surface of an iron substrate (maximum unevenness difference: 10 mm, D1: 6 mm, D2: 60 mm, θ: 60°, circumscribed circle radius: 30 cm) having the uneven shape shown in FIG. 1 using a jet dispensing device (nozzle diameter: 50 μm) to prepare a silver film, and the film was dried by heating in an oven at 120° C. for 30 minutes to form a silver layer (conductive layer) with a line width of approximately 200 μm and a thickness of approximately 8 μm, thereby preparing a structure.

[0079] Example 2 A structure was produced in the same manner as in Example 1, except that a silver layer was formed on the uneven surface of a PET substrate having the uneven shape shown in FIG. 2 (maximum unevenness difference: 10 mm, D1: 5 mm, D2: 15 mm, θ: 25°, radius of curvature of each hemispherical convex portion: 5 mm, radius of circumscribed circle: 15 cm).

[0080] Example 3 A structure was produced in the same manner as in Example 1, except that a silver layer was formed on the uneven surface of a printed circuit board (having a mold resin and a glass epoxy base material) having the uneven shape shown in FIG. 4 (maximum unevenness difference: 3 mm, D1: 1 mm, D2: 20 mm, θ: 90°, circumscribed circle radius: 10 cm) as the substrate.

[0081] Example 4 Ink 2 was printed using an inkjet printing device on the surface of the curved portion (outer periphery of the curved surface) of a PC sunglasses lens (radius of curvature: 50 mm, maximum unevenness difference: 3 mm, radius of circumscribed circle: 15 cm) to produce a silver film, and the silver layer was heated and dried in an oven at 120°C for 30 minutes to form a silver layer with a line width of approximately 30 μm and a thickness of approximately 0.3 μm, and a structure was produced.

[0082] Example 5 Ink 2 was printed on the outer peripheral surface of a cylindrical PET substrate (cross-sectional radius: 50 mm, circumscribed circle radius: 40 cm) as shown in FIG. 3 using an inkjet printing device to prepare a silver film, and the silver film was dried by heating in an oven at 120°C for 30 minutes to form a silver layer with a line width of about 30 μm and a thickness of about 0.3 μm, thereby preparing a structure.

[0083] Example 6 A structure was produced in the same manner as in Example 4, except that the line width of the silver layer was about 100 μm and the thickness was about 3 μm.

[0084] Example 7 A structure was produced in the same manner as in Example 1, except that an air-type dispensing device (nozzle diameter: 100 μm) was used instead of the jet dispensing device (nozzle diameter: 50 μm).

[0085] Example 8 Ink 2 was applied to the uneven surface of a printed circuit board (having a mold resin and a glass epoxy base material) having the uneven shape shown in FIG. 4 (maximum unevenness difference: 3 mm, D1: 1 mm, D2: 20 mm, θ: 90°, circumscribed circle radius: 10 cm) using a spray application device to prepare a silver film, and the silver layer (conductive layer) having a thickness of approximately 0.5 μm was formed by heating and drying in an oven at 120° C. for 30 minutes, thereby preparing a structure.

[0086] Reference Example 1 Ink 2 was printed on the surface of a PET substrate that did not have an uneven surface using an inkjet printing device to prepare a silver film, and the silver film was then dried by heating in an oven at 120°C for 30 minutes to form a silver layer (conductive layer) with a line width of approximately 30 μm and a thickness of approximately 0.3 μm, and a structure was prepared.

[0087] Reference Example 2 Ink 1 was applied to the surface of a PET substrate that did not have a rough surface using an air-type dispensing device (nozzle diameter 100 μm) to prepare a silver film, and the film was dried by heating in an oven at 120° C. for 30 minutes to form a silver layer (conductive layer) with a line width of approximately 200 μm and a thickness of approximately 8 μm, thereby preparing a structure.

[0088] Reference Example 3 Ink 1 was applied to the surface of a PET substrate that did not have an uneven surface using a jet dispensing device (nozzle diameter: 50 μm) to prepare a silver film, and the film was dried by heating in an oven at 120° C. for 30 minutes to form a silver layer (conductive layer) with a line width of approximately 200 μm and a thickness of approximately 8 μm, thereby preparing a structure.

[0089] Comparative Example 1 When an attempt was made to apply Ink 4 to a PET substrate having no uneven surface using a jet dispenser (nozzle diameter 50 μm), the ink could not be ejected at all.

[0090] Comparative Example 2 Ink 4 was applied to a PET substrate having no uneven surface using an air-type dispensing device (nozzle diameter 150 μm) to prepare a silver film, and the film was dried by heating in an oven at 120° C. for 30 minutes to form a silver layer with a line width of approximately 300 μm and a thickness of approximately 14 μm, thereby preparing a structure.

[0091] Comparative Example 3 When an attempt was made to print Ink 4 on a PET substrate that did not have an uneven surface using an inkjet printing device, the ink could not be ejected at all.

[0092] Comparative Example 4 When an attempt was made to print Ink 3 using a screen printing device on the uneven surface of a printed circuit board (having a mold resin and a glass epoxy base material) having the uneven shape shown in Figure 4 (maximum unevenness difference: 3 mm, D1: 1 mm, D2: 20 mm, θ: 90°, circumscribed circle radius: 10 cm), printing was only possible on the largest convex parts of the base material surface, and not on the concave parts. The printed parts were heated and dried in an oven at 120°C for 30 minutes, and a silver layer with a line width of approximately 100 µm and a thickness of approximately 4 µm was formed.

[0093] Comparative Example 5 When an attempt was made to print Ink 3 using a screen printing device on the curved portion (outer periphery of the curved surface) of a PC sunglasses lens (radius of curvature: 50 mm, maximum unevenness difference: 3 mm, radius of circumscribed circle: 15 cm), printing was only possible in an area about 10 mm radius from the apex of the substrate, with no printing outside of that. The printed portion was heated and dried in an oven at 120°C for 30 minutes, forming a silver layer with a line width of about 100 μm and a thickness of about 4 μm.

[0094] <Evaluation> The structures obtained in the examples and comparative examples were evaluated as follows, and the results are shown in the table.

[0095] (1) Continuous Discharge Stability Continuous discharge stability during the preparation of structures in Examples and Comparative Examples was evaluated according to the following criteria. [Evaluation Criteria] ◎ Stable continuous discharge possible for 8 hours or more ○ Stable continuous discharge possible for about 30 minutes × Stable continuous discharge not possible for about 30 minutes

[0096] (2) Porosity The structures obtained in the examples and comparative examples were cut and the cross section was polished using a milling machine (trade name "ArBlade5000", manufactured by Hitachi, Ltd.). Next, the cross section was observed using a scanning electron microscope (trade name "JEOL JSM-F100", manufactured by JEOL Ltd.) by adjusting the magnification, and the porosity of the conductive layer was calculated.

[0097] (3) Volume Resistivity For the structures obtained in the Examples and Comparative Examples, the electrical resistance per cm of the conductive layer length was measured using a digital multimeter (product name "VOAC7602", manufactured by Iwasaki Electric Co., Ltd.). Next, the cross-sectional area of ​​the conductive layer was measured using a step gauge (product name "ET4000A", manufactured by Kosaka Laboratory Co., Ltd.). The volume resistivity was calculated by multiplying the electrical resistance value by the cross-sectional area value.

[0098]

[0099]

[0100] As shown in Tables 1 and 2, the examples demonstrated excellent ink continuous ejection stability, and the volume resistivity of the conductive layer formed on the non-flat surface was comparable to that of the reference example, which used the corresponding printing method, and was therefore evaluated as having excellent conductivity. In Examples 3 and 8, ink adhesion and conductive layer formation were possible only on the convex portions. In Example 6, a conductive layer could be formed on the non-flat surface, but the volume resistivity was higher than in the other examples, so porosity measurement was not performed. On the other hand, when using ink containing silver nanoparticles with a number-average particle diameter of 50 μm or more, stable continuous ejection was not possible (Comparative Examples 1 to 3). In Comparative Example 2, clogging occurred approximately 10 minutes after the start of ejection, and the volume resistivity of the formed conductive layer was also high. Furthermore, when attempting to form a conductive layer on a non-flat surface by screen printing (Comparative Examples 4 and 5), the screen plate is pressed firmly with a squeegee. However, pressing the squeegee too hard can deform the substrate itself or damage the screen plate, limiting the areas that can be printed.

[0101] Variations of the invention according to the present disclosure are described below. [Appendix 1] A method for producing a structure including a substrate having an uneven surface and a conductive layer formed on the uneven surface of the substrate, the method comprising: an attachment step of attaching a conductive composition containing metal nanoparticles having an average particle size of less than 50 nm to the uneven surface of the substrate to form a metal film, the conductive composition containing the metal nanoparticles in an amount of 1 to 66 mass %. [Appendix 2] A method for producing a structure according to Appendix 1, the method comprising, after the attachment step, a firing step of sintering the metal film to form the conductive layer. [Appendix 3] A method for producing a structure according to Appendix 1 or 2, the attachment being by printing, not screen printing. [Appendix 4] A method for producing a structure according to any one of Appendices 1 to 3, wherein the metal nanoparticles include silver and / or copper. [Appendix 5] A method for producing a structure according to any one of Appendices 1 to 4, wherein the uneven surface includes at least a curved, convex, or concave surface. [Appendix 6] The method for producing a structure according to any one of Appendices 1 to 5, wherein the content of metal microparticles with a particle diameter of 1 μm or more in the conductive composition is less than 1 per 100 total particles of the metal nanoparticles. [Appendix 7] A structure comprising a substrate having an uneven surface and a conductive layer formed on the uneven surface of the substrate, wherein the porosity of at least a portion of the conductive layer is 0.01 to 50%. [Appendix 8] The structure according to Appendices 7, wherein the conductive layer has a volume resistivity of 1000 μΩ cm or less. [Appendix 9] The structure according to Appendices 7 or 8, wherein the conductive layer has a thickness of 0.05 to 1000 μm. [Appendix 10] The structure according to any one of Appendices 7 to 9, wherein the uneven surface includes at least a curved surface, a convex surface, or a concave surface.

[0102] 1 Structure 2 Base material 2a to 2d Non-flat surface 3 Conductive layer

Claims

1. A method for producing a structure comprising a substrate having an uneven surface and a conductive layer formed on the uneven surface of the substrate, the method comprising a step of adhering a conductive composition to the uneven surface of the substrate, the conductive composition containing metal nanoparticles having an average particle size of less than 50 nm, the metal nanoparticles being present in an amount of 1 to 66 mass %, to form a metal film.

2. The method for producing the structure according to claim 1, further comprising a firing step of sintering the metal film to form the conductive layer after the deposition step.

3. The method for producing the structure according to claim 1 or 2, wherein said deposition is printing that does not include screen printing.

4. The method for producing a structure according to claim 1 or 2, wherein the metal nanoparticles contain silver and / or copper.

5. The method for producing a structure according to claim 1 or 2, wherein the non-flat surface includes at least a curved surface, a convex surface, or a concave surface.

6. The method for producing a structure described in claim 1 or 2, wherein the content of metal microparticles having a particle diameter of 1 μm or more in the conductive composition is less than 1 per 100 total particles of the metal nanoparticles.

7. A structure comprising a substrate having an uneven surface and a conductive layer formed on the uneven surface of the substrate, wherein the porosity of at least a portion of the conductive layer is 0.01 to 50%.

8. The structure according to claim 7, wherein the volume resistivity of said conductive layer is 1000 μΩ·cm or less.

9. The structure according to claim 7 or 8, wherein the conductive layer has a thickness of 0.05 to 1000 μm.

10. The structure according to claim 7 or 8, wherein the non-flat surface includes at least a curved surface, a convex surface, or a concave surface.

Citation Information

Patent Citations

  • Laminated body and electronic equipment

    JP2016005909A

  • Laminated structure and printing method

    JP2019160995A

  • Method for manufacturing dispersion

    JP2019178059A

  • Metal-resin bonded product

    JP2019181711A

  • Conductive composition for molded film, molded film and production method of the same, and molded article and production method of the same