Aluminum alloy having good resistance to hydrogen embrittlement and hydrogen-transport pipe comprising same
A specifically composed and structured aluminum alloy with controlled precipitated phases addresses the need for a lightweight, cost-effective, non-heat treatable material with superior hydrogen embrittlement and corrosion resistance, suitable for hydrogen transport applications.
Patent Information
- Application Number
- PCT/KR2023/009115
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2023-06-29
- Publication Date
- 2024-11-28
AI Technical Summary
There is a need for a lightweight, inexpensive, non-heat treatable aluminum alloy with excellent hydrogen embrittlement resistance, mechanical properties, and corrosion resistance, as existing materials like stainless steel are costly and require heat treatment, while current alternatives like A6063 have limitations in strength and corrosion resistance.
An aluminum alloy with a specific composition and microstructure, including a precipitated phase distribution of AlMn6, containing 0.05-0.3% Fe, 0.05-0.2% Cu, 0.5-1.1% Mn, and 0.05% Mg, and a controlled distribution of precipitated phases to enhance hydrogen embrittlement resistance and corrosion resistance, without the need for heat treatment.
The alloy achieves a tensile strength/yield strength ratio greater than 1.07, elongation of 12% or more, and corrosion resistance exceeding 1000 hours in SWAAT tests, while maintaining hydrogen embrittlement resistance comparable to heat-treated alloys, making it suitable for hydrogen transport pipes.
Smart Images

Figure KR2023009115_28112024_PF_FP_ABST
Abstract
Description
Aluminum alloy with excellent hydrogen embrittlement resistance and hydrogen transport pipe containing the same
[0001] The present invention relates to an aluminum alloy with excellent hydrogen embrittlement resistance. Specifically, the invention relates to an aluminum alloy that is lightweight and exhibits excellent properties, including hydrogen embrittlement resistance, mechanical properties, and corrosion resistance, despite being inexpensive and non-heat-treatable.
[0002] Hydrogen embrittlement, a phenomenon in which hydrogen is absorbed into a metal, weakening its mechanical properties and making it brittle, is an unavoidable and fatal defect in metal products and components. Therefore, when designing parts or components that come into direct contact with hydrogen gas, it is advisable to avoid metals or materials prone to hydrogen embrittlement.
[0003] However, in the case of products such as hydrogen transport pipes, where metal materials must be selected due to the simultaneous requirements for appropriate processability, bendability, pressure strength, and corrosion resistance, a technical requirement to suppress hydrogen embrittlement arises.
[0004] Meanwhile, the most renowned metal material for its excellent hydrogen embrittlement resistance is stainless steel (STS). Stainless steel (STS) is the metal with the most user-verified hydrogen embrittlement resistance. Its superior mechanical properties and corrosion resistance make it highly valuable for use in piping.
[0005] However, stainless steel (STS) is relatively expensive and its use is limited in products requiring lightweight construction. To address these issues, aluminum alloy A6063 has recently been adopted. While aluminum alloy A6063 has lower strength and corrosion resistance than stainless steel (STS), its superior specific strength has made it a popular complementary or alternative to stainless steel (STS).
[0006] However, aluminum alloy A6063 is a heat-treatable alloy, meaning that it requires appropriate aging heat treatment to achieve the desired strength, and therefore is disadvantageous in terms of price and quality control compared to non-heat-treatable aluminum alloys.
[0007] In addition, when aluminum alloy A6063 is manufactured without solution heat treatment in the T5 condition (artificial age hardening after cooling from high-temperature processing) or T6 condition (artificial age hardening after solution heat treatment), the internal structure of the metal may not be properly controlled, and the intended hydrogen embrittlement resistance may not be achieved.
[0008] Therefore, there is an urgent need for a lightweight aluminum alloy that is inexpensive, non-heat-treatable, and has excellent properties such as hydrogen embrittlement resistance, mechanical properties, and corrosion resistance.
[0009] The purpose of the present invention is to provide an aluminum alloy that is lightweight and has excellent properties such as hydrogen embrittlement resistance, mechanical properties, and corrosion resistance despite being a non-heat-treatable type and inexpensive.
[0010] In order to solve the above problem, the present invention,
[0011] As an aluminum alloy, the area in any cross section is 1 ㎛ 2 When an imaginary rectangle of 10㎛×50㎛ in size is formed at an arbitrary angle on the cross-section with an arbitrary precipitate phase as the center, the area of the precipitate phase included in the rectangle is 0.8㎛. 2 An aluminum alloy is provided having a precipitation phase distribution in which the number of ideal precipitation phases is less than 10.
[0012] Here, an aluminum alloy is provided, characterized in that the precipitate phase includes a precipitate phase of AlMn6.
[0013] In addition, the aluminum alloy is characterized in that it contains alloying elements of 0.05 to 0.3 wt% of iron (Fe), 0.05 to 0.2 wt% of copper (Cu), 0.5 to 1.1 wt% of manganese (Mn), and 0.05 to 0.3 wt% of magnesium (Mg) based on the total weight of the aluminum alloy, and the remaining balance contains aluminum and inevitable impurities.
[0014] Furthermore, an aluminum alloy is provided, characterized in that the aluminum alloy, which is hydrogen-injected and sealed through an SSRT test according to standard ISO 16573, has a tensile strength / yield strength ratio (TS / YS) of 1.07 or more, an elongation of 12% or more, and a shrinkage ratio at break (RRA) of 0.9 or more compared to an aluminum alloy that is not hydrogen-injected and sealed.
[0015] In addition, an aluminum alloy is provided, characterized by having a tensile strength of 10 MPa or more, an elongation of 15% or more, and a corrosion resistance of SWAAT of 1000 hours or more.
[0016] Meanwhile, a hydrogen transport pipe including the above aluminum alloy is provided.
[0017] The aluminum alloy according to the present invention exhibits excellent properties such as hydrogen embrittlement resistance, mechanical properties, and corrosion resistance despite being a non-heat-treatable lightweight aluminum alloy by precisely controlling the pores, tempering, and precipitation phase distribution.
[0018] Figure 1 is an electron microscope photograph of the aluminum alloy of Example 1.
[0019] Figure 2 is an electron microscope photograph of the aluminum alloy of Comparative Example 2.
[0020] Figure 3 is an electron microscope photograph of the aluminum alloy of Comparative Example 4.
[0021] Figure 4 is an electron microscope photograph of the aluminum alloy of Comparative Example 7.
[0022] Hereinafter, preferred embodiments of the present invention will be described in detail. However, the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosure is thorough and complete, and to sufficiently convey the spirit of the present invention to those skilled in the art.
[0023] The exact mechanism of hydrogen embrittlement of aluminum has not yet been elucidated, but several theories and models have been proposed. Representative theories of aluminum hydrogen embrittlement include HELP (Hydrogen Enhanced Local Plasticity), HEDE (Hydrogen Enganced Decohesion), and AIDE (Adsorption Induced Disloaction Emission).
[0024] According to these theories, although the details of the hydrogen embrittlement process are different, they all have in common that hydrogen propagates and diffuses from the weakest part or the part with a structural defect in the material, and when this defect grows beyond a certain size, the bonds of atoms are broken or weakened in a chain reaction, causing embrittlement.
[0025] Here, structural defects of the material are understood to include structural defects such as pores, atomic-level defects of alloy materials such as precipitates that are elements other than aluminum or aggregations thereof, and microscopic material defects such as the size or distribution of grain boundaries and even the density of dislocations.
[0026] In this situation, the inventors of the present invention evaluated hydrogen embrittlement resistance using test pieces and products manufactured from aluminum alloys under various conditions and found that the sensitivity to hydrogen embrittlement is determined in the following order.
[0027] Hydrogen embrittlement susceptibility: Pores and vacancies > Type / distribution / size of precipitates > Grain boundary size / distribution > Degree of plastic processing
[0028] Since the presence of the above pores and vacancies indicates a defective product, they are specific characteristics rather than controllable characteristics of good products. Therefore, the most important factors for hydrogen embrittlement resistance design are the type, distribution, and size of precipitates contained in the alloy. This is because, as expected, precipitates have a different crystal structure from aluminum crystals, making it easy for small-sized hydrogen to enter and diffuse into the gaps between the crystals.
[0029] Specifically, the aluminum alloy having excellent hydrogen embrittlement resistance according to the present invention is based on the aluminum (Al)-manganese (Mn) system. The aluminum (Al)-manganese (Mn) system alloy has AlMn6 as a representative precipitation phase, and the inventors of the present invention have found that an alloy having an AlMn6 precipitation phase has superior hydrogen embrittlement resistance compared to an aluminum alloy (A7075) having a MgZn2 precipitation phase, and has hydrogen embrittlement resistance at the same level as an aluminum alloy (A6061, A6063) having a Mg2Si precipitation phase.
[0030] However, aluminum alloys (A6061, A6063) having a Mg2Si precipitation phase are heat-treatable alloys, that is, alloys that require appropriate aging heat treatment to achieve the desired strength, and therefore are disadvantageous in terms of price and quality control compared to non-heat-treatable aluminum alloys according to the present invention.
[0031] The aluminum alloy having excellent hydrogen embrittlement resistance according to the present invention may contain alloying elements of 0.05 to 0.3 wt% of iron (Fe), 0.05 to 0.2 wt% of copper (Cu), 0.5 to 1.1 wt% of manganese (Mn), and 0.05 to 0.3 wt% of magnesium (Mg) based on the total weight thereof, and the remaining portion may be aluminum and unavoidable impurities.
[0032] Here, among the alloying elements, iron (Fe) and copper (Cu) can further improve the corrosion resistance and strength of the aluminum alloy. When the content of each of iron (Fe) and copper (Cu) is less than 0.05 wt%, the corrosion resistance and strength of the aluminum alloy may be reduced, whereas when the content of iron (Fe) exceeds 0.3 wt%, the hydrogen embrittlement resistance of the aluminum alloy may be reduced, and when the content of copper (Cu) exceeds 0.2 wt%, the hydrogen embrittlement resistance and elongation of the aluminum alloy may be reduced.
[0033] In addition, among the alloying elements, manganese (Mn) increases the recrystallization temperature of the aluminum alloy and suppresses grain growth by forming an aluminum (Al)-manganese (Mn) precipitation phase that is incorporated into the aluminum alloy during casting, thereby suppressing recrystallization during homogenization heat treatment, preventing stress concentration due to deformation processing during extrusion and hot working processes, and increasing resistance to deformation, thereby improving elongation and workability.
[0034] Furthermore, when the manganese (Mn) content is less than 0.5 wt%, it is difficult to secure the strength and corrosion resistance of the aluminum alloy, whereas when it exceeds 1.1 wt%, there is a problem of reduced hydrogen embrittlement resistance.
[0035] In addition, among the alloying elements, magnesium (Mg) further improves the corrosion resistance, elongation, etc. of the aluminum alloy, and when the content of magnesium (Mg) is less than 0.05 wt%, it is difficult to secure the corrosion resistance of the aluminum alloy, whereas when it exceeds 0.3 wt%, the corrosion resistance, elongation, hydrogen embrittlement resistance, etc. of the aluminum alloy may be reduced.
[0036] Even if the aluminum alloy according to the present invention, which exhibits excellent hydrogen embrittlement resistance, satisfies the composition described above, if the pores, tempering, and precipitation distribution of the material are not appropriate, the hydrogen embrittlement resistance may be significantly reduced. In particular, precipitation distribution control can be achieved through various methods, such as heat treatment or plastic processing of the aluminum alloy. These processes can be adjusted to a limited extent depending on the characteristics of the product to be manufactured, and thus can be appropriately selected and implemented by a skilled artisan.
[0037] For example, in order to control the distribution of the precipitate, for example, the precipitate of a billet or rod in a cast state is spheroidized, but a homogenization heat treatment is performed within an appropriate range so that it does not coarsen, and the extrusion ratio, that is, the ratio of the cross-sectional areas before and after extrusion, can be adjusted to 3:1 to 30:1 so that the spheroidized precipitate can be distributed in an appropriate size and range. If the extrusion ratio is less than 3:1, some of the cast structure may remain, making the distribution of the precipitate uneven, and if the extrusion ratio is more than 30:1, the precipitate is likely to be aligned in the extrusion direction and used as a diffusion path for hydrogen.
[0038] The present inventors have discovered that the diffusion of hydrogen that causes hydrogen embrittlement of aluminum alloys is centered on the interface between aluminum and precipitate phases, and thus, the greater the distance between the interfaces of precipitate phases, the more hydrogen embrittlement can be delayed. In addition, considering that the more fine precipitate phases are distributed, the more advantageous it is for dispersion strengthening of aluminum alloys, the more the area of the precipitate phase is distributed. In the aluminum alloy with excellent hydrogen embrittlement resistance according to the present invention, the area of the precipitate phase is 1 ㎛ in any cross section. 2 When an imaginary rectangle of 10㎛×50㎛ in size is formed at an arbitrary angle on the cross-section with an arbitrary precipitate phase as the center, the area of the precipitate phase included in the rectangle is 0.8㎛. 2 The number of ideal precipitates was adjusted to less than 10. Here, precipitates that contact the outer line of the virtual rectangle are considered to be precipitates included within the rectangle.
[0039] Here, the area of the precipitate included within the above rectangle is 0.8 ㎛ 2 If the number of abnormal precipitates is more than 10, hydrogen embrittlement of the aluminum alloy may be serious.
[0040] Meanwhile, the area of precipitates can be determined by measuring the area of precipitates using an analysis program in photographs of aluminum alloy samples taken with an electron microscope or optical microscope. Examples of such analysis programs include NIS Elements, an analysis program for Nikon optical microscopes, but any image analysis program capable of scale correction can also be used.
[0041]
[0042] [Example]
[0043]
[0044] 1. Manufacturing example
[0045]
[0046] An aluminum rod (Φ12.5) containing the alloy components described in Table 1 below was manufactured through continuous casting and rolling, and then a homogenization heat treatment was performed by maintaining the rod at 320 to 480°C for 6 to 48 hours and then air-cooling. An aluminum tube (Φ12.5, t0.51) was manufactured through confirm extrusion, and a tube (Φ9.8, t0.50) was processed through drawing, thereby manufacturing a sample having the precipitation phase distribution described in Table 1 below.
[0047] Here, the distribution of precipitates was evaluated by obtaining a cross-section of 1 cm × 1 cm in a random direction from each sample, mechanically polishing it using a diamond suspension with a particle diameter of 1 ㎛ or less as an abrasive, and taking a photograph magnified 1000 times using an electron microscope, and the area was 1 ㎛. 2 When an imaginary rectangle of 10㎛×50㎛ in size is formed at an arbitrary angle on the cross-section with an arbitrary precipitate phase as the center, the area of the precipitate phase included in the rectangle is 0.8㎛.2 It refers to the number of abnormal precipitates.
[0048]
[0049]
[0050] 2. Physical property evaluation
[0051]
[0052] 1) Tensile strength and elongation evaluation
[0053] Tensile strength and elongation were measured for each sample of the examples and comparative examples at a standard distance of 40 mm and a strain rate of 1 mm / s in accordance with ASTM E8. The tensile strength must be 10 MPa or more and the elongation must be 15% or more.
[0054] 2) Corrosion resistance evaluation
[0055] The SWAAT test was performed on each sample of the examples and comparative examples according to the standard ASTM G85. Specifically, an aqueous solution of glacial acetic acid (10G / 1L) and NaCl (4.2 wt%) was sprayed on the sample surface at 1 to 2 mL / Hr at 49°C, and a cycle of spraying for 30 minutes and then maintaining for 90 minutes was performed. After 1000 hours of SWAAT, there should be no formation of pitting in the sample. Here, the presence of pitting in the sample is judged based on whether air bubbles are generated when air pressure is applied inside the tube sample while the sample is immersed in a water bath.
[0056] OK: Pass, NG: Bad
[0057] 3) Hydrogen embrittlement evaluation
[0058] SSRT tests were performed on each sample of the examples and comparative examples in accordance with the standard ISO 16573.
[0059] Specifically, two samples each of the examples and comparative examples were prepared, and one was prepared at a current density of 20 A / m in an electrolyte of NaCl (30 g / L) + NH4SCN (3 g / L). 2By maintaining it for 24 hours, hydrogen is artificially injected into the inside of the sample and sealed with zinc plating to prevent hydrogen from escaping, and the remaining one is used as a reference sample without hydrogen injection.
[0060] Next, for the hydrogen-injected and sealed samples, the standard distance was 40 mm, and the strain rate was 2×10 -5 Tensile strength, yield strength and elongation are measured in mm / s, and the ratio of tensile strength / yield strength (TS / YS) must be 1.07 or more, and the elongation must be 12% or more.
[0061] Additionally, the shrinkage ratio (RRA) of the fracture surface of the hydrogen-injected and sealed sample compared to the reference sample must be 0.9 or more.
[0062] If the hydrogen embrittlement resistance is OK overall, it is a pass, and if it is NG, it is a failure.
[0063]
[0064] The results of the above property evaluation are shown in Table 2 below and Figures 1 to 4.
[0065]
[0066]
[0067]
[0068] As shown in Tables 1 and 2 and FIG. 1, the aluminum alloys of Examples 1 to 3 having appropriate alloying elements and precipitate distributions were confirmed to have excellent room temperature mechanical properties, corrosion resistance, and hydrogen embrittlement resistance. On the other hand, the aluminum alloy of Comparative Example 1 had insufficient corrosion resistance because the content of manganese (Mn) among the alloying elements was below the standard, and the aluminum alloy of Comparative Example 2 had significantly reduced hydrogen embrittlement resistance because the content of manganese (Mn) among the alloying elements exceeded the standard and the precipitate phase distribution (FIG. 2) did not meet the standard.
[0069] In addition, the aluminum alloy of Comparative Example 3 did not contain copper (Cu) and magnesium (Mg) among the alloying elements, so the corrosion resistance was insufficient, and the aluminum alloy of Comparative Example 4 had an iron (Fe) content among the alloying elements exceeding the standard and a precipitation phase distribution (Fig. 3) that did not meet the standard, so the hydrogen embrittlement resistance was greatly reduced.
[0070] In addition, the aluminum alloy of Comparative Example 5 had a content of copper (Cu) among alloy elements exceeding the standard and a distribution of precipitation phases not satisfying the standard, resulting in a significant reduction in hydrogen embrittlement resistance, and the aluminum alloy of Comparative Example 6 had a content of magnesium (Mg) among alloy elements exceeding the standard, resulting in a significant reduction in room temperature elongation and hydrogen embrittlement resistance.
[0071] In addition, the aluminum alloy of Comparative Example 7 had an appropriate alloying element content, but the extrusion ratio exceeded 30:1, so the precipitation phase distribution (see Fig. 4) did not meet the standard, and thus the hydrogen embrittlement resistance was significantly reduced.
[0072] While this specification has described preferred embodiments of the present invention, those skilled in the art will appreciate that various modifications and variations can be made to the present invention without departing from the spirit and scope of the invention as defined in the claims below. Therefore, any modified implementation that fundamentally includes elements of the claims of the present invention should be considered within the technical scope of the present invention.
Claims
1. As an aluminum alloy, Area of 1 ㎛ in any cross-section 2 When an imaginary rectangle of 10㎛×50㎛ in size is formed at an arbitrary angle on the cross-section with an arbitrary precipitate phase as the center, the area of the precipitate phase included in the rectangle is 0.8㎛. 2 An aluminum alloy having a precipitation phase distribution in which the number of abnormal precipitation phases is less than 10.
2. In paragraph 1, An aluminum alloy, characterized in that the above precipitate phase includes a precipitate phase of AlMn6.
3. In paragraph 2, An aluminum alloy characterized in that the aluminum alloy comprises alloying elements of 0.05 to 0.3 wt% of iron (Fe), 0.05 to 0.2 wt% of copper (Cu), 0.5 to 1.1 wt% of manganese (Mn), and 0.05 to 0.3 wt% of magnesium (Mg), based on the total weight of the aluminum alloy, and the remaining balance comprises aluminum and unavoidable impurities.
4. In any one of paragraphs 1 to 3, An aluminum alloy characterized by a tensile strength / yield strength ratio (TS / YS) of 1.07 or more, an elongation of 12% or more, and a shrinkage ratio at break (RRA) of 0.9 or more compared to an aluminum alloy that has not been hydrogen-injected and sealed, as determined by an SSRT test according to standard ISO 16573.
5. In any one of paragraphs 1 to 3, An aluminum alloy characterized by a tensile strength of 10 MPa or more, an elongation of 15% or more, and a corrosion resistance of SWAAT 1000 hours or more.
6. A hydrogen transport pipe comprising an aluminum alloy according to any one of claims 1 to 3.
Citation Information
Patent Citations
Aluminum alloy blank for magnetic disk and aluminum alloy substrate for magnetic disk
CN113544304A
High-strength aluminum alloy plate for printing plate
JP1985063340A
Method for producing aluminum alloy thick plate, and aluminum alloy thick plate
JP2007308766A
Al-Mg BASED ALLOY FOR HIGH PRESSURE HYDROGEN GAS VESSEL
JP2014009398A