Plated steel and manufacturing method therefor

The use of a plating bath with controlled aluminum, magnesium, and zinc compositions and cooling rates forms a multilayer primary Zn phase structure, addressing corrosion and crack resistance issues in plated steel, resulting in enhanced performance and processing quality.

WO2024248366A1PCT designated stage expired Publication Date: 2024-12-05HYUNDAE STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006554
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-14
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing plated steel products face challenges in achieving high corrosion resistance and crack resistance due to the inefficiencies of zinc sacrificial anode properties and magnesium oxidation, which affect the quality and processing difficulties of the plating layer.

Method used

A method involving a plating bath with aluminum (Al), magnesium (Mg), and zinc (Zn) is used, with specific weight ratios and cooling rates to form a primary Zn phase structure with a multilayer configuration, enhancing corrosion resistance and crack resistance.

Benefits of technology

The method results in a plated steel material with improved corrosion resistance and crack resistance, as demonstrated by extended red rust generation times and excellent processing quality, while minimizing operational complexities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006554_05122024_PF_FP_ABST
    Figure KR2024006554_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Plated steel of the present invention comprises a base iron and a plating layer, which is formed on the base iron and comprises 1-3 wt% of aluminum (Al), 1-2 wt% of magnesium (Mg) and the balance of zinc (Zn) and other inevitable impurities, wherein the weight ratio of aluminum and magnesium in the plating layer is 1.2 or greater, the plating layer comprises a primary Zn phase structure and a eutectic phase structure, the primary Zn phase structure has a multilayer structure in the height direction of the plating layer, the area fraction of the primary Zn phase structure having a multilayer structure in the plating layer is 30% or higher, and the thickness of the plating layer is 15-50 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Galvanized steel and its manufacturing method

[0001] The present invention relates to a plated steel and a method for manufacturing the same, and more particularly, to a plated steel having excellent corrosion resistance in a processed part and a method for manufacturing the same.

[0002] Conventional hot-dip galvanized steel has excellent self-sacrificing properties, and is widely used in construction materials and home appliances. When hot-dip galvanized steel is exposed to a corrosive environment, zinc (Zn) acts as a sacrificial anode on the exposed iron portion, causing zinc loss from the plating layer. This sacrificial anode action of zinc plays an excellent role in suppressing rust of the base iron in a corrosive environment, but has the problem of somewhat low sacrificial anode efficiency. To solve this problem, recently in Japan and Europe, high-corrosion-resistant plating products are being produced by adding magnesium (Mg) to the zinc (Zn) plating bath. This creates dense corrosion products in corrosive environments and improves sacrificial anode efficiency, thereby exhibiting excellent corrosion resistance.

[0003] However, the plating bath process in which magnesium (Mg) is added to zinc (Zn) has a problem in that as the magnesium (Mg) content increases, it reacts with oxygen in the air to form oxides, which lowers the surface quality. To solve this problem, an inert gas (nitrogen) is used in the wiping process to control the plating amount. In addition, an oxidation-free chamber is used to minimize contact with oxygen in the wiping process area. While high-corrosion-resistant plating steel has the advantage of improving corrosion resistance as the magnesium (Mg) content increases, it has the disadvantage of increasing additional processes due to magnesium (Mg) oxidation and making operation difficult due to the oxides.

[0004] To minimize these problems, magnesium (Mg) can be added with a low content, but the primary Zn phase formed during solidification of the plating layer is formed in a relatively coarse shape, and the area where the coarse primary Zn phase is formed in a corrosive environment develops into an area with poor corrosion resistance. In addition, when the magnesium (Mg) content is low, the amount of eutectic phase containing magnesium (Mg) produced decreases, making it difficult to exhibit high corrosion resistance. On the other hand, the eutectic phase containing magnesium (Mg) has high hardness, which acts as a starting point for cracks in the plating layer during processing, and the base iron exposed by the cracks causes a rapid decrease in corrosion resistance in a corrosive environment.

[0005] Related prior art includes Japanese Patent Publication No. 2005-105367.

[0006] The technical problem to be achieved by the present invention is to provide a highly corrosion-resistant plated steel having excellent corrosion resistance and crack resistance in a processed part, and a method for manufacturing the same.

[0007] However, these tasks are exemplary and the technical idea of ​​the present invention is not limited thereto.

[0008] According to one aspect of the present invention for solving the above problem, a method for manufacturing a plated steel includes the steps of: (a) providing a base iron; (b) passing the base iron through a plating bath containing aluminum (Al), magnesium (Mg), and zinc (Zn), thereby forming a plated layer on the base iron, the plated layer comprising 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities; and (c) cooling the plated layer at a cooling rate of 10 to 30°C / sec, wherein the weight ratio of aluminum to magnesium in the plated layer is 1.2 or more.

[0009] In the above method for manufacturing the plated steel, the thickness of the plated layer may be 15 µm to 50 µm.

[0010] In the above method for manufacturing the plated steel, the plated layer after performing the cooling step includes a primary Zn phase structure and a eutectic structure, and the primary Zn phase structure may have a multilayer structure in the height direction of the plated layer.

[0011] In the above method for manufacturing the plated steel, the area fraction of the primary Zn phase structure having the multilayer structure in the plated layer may be 30% or more.

[0012] In the above method for manufacturing the plated steel, the primary Zn phase structure may be first created in the cooling step, and the process structure may be created after the primary Zn phase structure is created.

[0013] According to one aspect of the present invention for solving the above problem, a plated steel material comprises: a base steel; and a plating layer formed on the base steel, the plating layer comprising 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities; wherein the weight ratio of aluminum to magnesium in the plating layer is 1.2 or more.

[0014] In the above-mentioned plated steel, the plating layer includes a primary Zn phase structure and a eutectic phase structure, and the primary Zn phase structure may have a multi-layer structure in the height direction of the plating layer.

[0015] In the above-mentioned plated steel, the area fraction of the primary Zn phase structure having the multilayer structure within the plated layer may be 30% or more.

[0016] In the above-mentioned plated steel, the thickness of the plated layer may be 15 µm to 50 µm.

[0017] According to an embodiment of the present invention, a plated steel having excellent corrosion resistance at a processed area and a method for manufacturing the same can be realized. Specifically, by forming a multilayer structure of a primary zinc phase in the plated layer, a highly corrosion-resistant plated steel having excellent crack resistance at a processed area and excellent corrosion resistance and a method for manufacturing the same can be realized.

[0018] Of course, the scope of the present invention is not limited by these effects.

[0019] FIG. 1 is a flowchart illustrating a method for manufacturing a plated steel according to one embodiment of the present invention.

[0020] Figure 2 is a photograph of a cross-section of a plating layer in a plated steel according to Comparative Example 5 as an experimental example of the present invention.

[0021] Figure 3 is a photograph of a cross-section of a plating layer in a plated steel according to Example 3 as an experimental example of the present invention.

[0022] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. These embodiments are provided to more fully explain the technical concept of the present invention to those skilled in the art. The following embodiments may be modified in various ways, and the scope of the technical concept of the present invention is not limited to the following embodiments. Rather, these embodiments are provided to more faithfully and completely explain the present disclosure and to fully convey the technical concept of the present invention to those skilled in the art.

[0023] A plated steel material with excellent corrosion resistance at the machined portion and a method for manufacturing the same according to an embodiment of the present invention are described in detail. The terms described below have been appropriately selected in consideration of their functions in the present invention, and their definitions should be based on the contents of this specification.

[0024] FIG. 1 is a flowchart illustrating a method for manufacturing a plated steel according to one embodiment of the present invention.

[0025] Referring to FIG. 1, a method for manufacturing a plated steel according to an embodiment of the present invention includes (a) a step of providing a base steel (S10); (b) a step of annealing the base steel (S20); (c) a step of passing the annealed base steel through a plating bath containing aluminum (Al), magnesium (Mg), and zinc (Zn) to form a plated layer on the base steel composed of 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities (S30); and (d) a step of cooling the plated layer at a cooling rate of 10 to 30°C / sec (S40).

[0026] In the case of high-corrosion-resistant plating steel, Al phase, Zn phase, and MgZn2 phase are formed in the plating layer depending on the amount of Al and Mg added to the Zn plating bath. A binary eutectic phase with a lamellar shape, a ternary eutectic phase with a MgZn2 phase containing Al and a Zn phase with a lamellar shape, and a polygonal MgZn2 phase are formed.

[0027] The Al phase with a dendritic structure and the MgZn2 phase with a polygonal structure are mainly formed in compositions with high amounts of Al and Mg added. In the present invention, the composition range where the Al phase with a dendritic structure and the MgZn2 phase with a polygonal structure are formed is excluded to improve the workability of the plating layer. For this purpose, the amount of Al added in the present invention can be controlled to 3 wt% or less, and the amount of Mg added can be controlled to 2 wt% or less.

[0028] The present invention improves the structure of the primary Zn phase of the plating layer in order to improve the phenomenon of corrosion resistance being reduced due to crack propagation within the plating layer of the processed portion in a high-corrosion-resistant plating steel.

[0029] In the case of highly corrosion-resistant plated steel, cracks typically originate from the intermetallic compounds present in the plating layer during the process and propagate to the boundary where the plating layer and the substrate steel meet, exposing the substrate steel. These cracks in the plating layer, when exposed to external corrosive environments, rapidly reduce corrosion resistance.

[0030] To minimize the number of these cracks, the fraction of the primary Zn phase must be increased. However, this simultaneously reduces the fraction of the process that improves corrosion resistance, thereby reducing corrosion resistance again. Furthermore, when the primary Zn phase is coarsened to increase the fraction of the primary Zn phase, the primary Zn phase is formed as a single layer, as shown in Fig. 2.

[0031] The primary Zn phase single layer structure can be defined as a plating layer microstructure structure in which the primary Zn phase is continuously connected from the plating layer surface to the base iron for at least 80% of the plating layer thickness based on the cross-section of the plating layer.

[0032] Although the primary Zn-phase single-layer structure itself exhibits excellent crack resistance in the plating layer, cracks easily progress because the surrounding process lacks sufficient Zn to impede crack propagation. Furthermore, the single-layer Zn phase is insufficient to form a robust passive film during corrosion in a corrosive environment. Therefore, excessive formation of the primary Zn-phase single-layer structure is not advantageous from a corrosion resistance perspective.

[0033] In order to solve these technical problems, the present invention discloses a technical idea of ​​minimizing crack propagation and improving corrosion resistance by forming a structure of a primary Zn phase existing in a plating layer from a single-layer structure to a multi-layer structure.

[0034] The multilayer structure of the primary Zn phase refers to the microstructure of the plating layer in which the area fraction of two or more primary Zn phases overlapping each other and existing in a multilayer structure is 30% or more based on the cross-section of the plating layer, as shown in Fig. 3. Here, the existence of two or more primary Zn phases overlapping each other in a multilayer structure may mean that when the plating layer is viewed vertically from the top to the bottom, two or more primary Zn phases exist in a multilayer structure in a position where they at least partially overlap.

[0035] In addition, the above-described primary Zn phase multilayer structure may include a structure in which the primary Zn phase is divided into two or more separate layers in the thickness height direction of the cross-section of the plating layer. In this case, a predetermined separation space may be interposed between the primary Zn phases divided into separate layers in the above-described primary Zn phase multilayer structure, and the width of the predetermined separation space may be in the range of 0.1 to 5 ㎛.

[0036] Each of the primary Zn phases constituting the above primary Zn phase multilayer structure may exist, for example, at least two or more throughout the thickness of the plating layer from the surface of the plating layer to the base iron.

[0037] In order to form the microstructure of the present invention, it is possible to control the solidification phase shape through the ratio of aluminum (Al) and magnesium (Mg) components and the cooling rate.

[0038] The composition range of the plating bath (plating layer) according to the technical idea of ​​the present invention is proposed as aluminum (Al): 1 to 3 wt%, magnesium (Mg): 1 to 2 wt%, and the remainder zinc (Zn). In this specification, the composition of the plating bath and the composition of the plating layer can be considered to be almost the same.

[0039] When aluminum (Al) is added in amounts less than 1 wt%, it cannot sufficiently reduce the oxidation of magnesium (Mg). When aluminum (Al) is added in amounts exceeding 3 wt%, it can generate a large number of cracks during processing due to the formation of a large amount of ternary process phase.

[0040] When magnesium (Mg) is added in an amount of less than 1 wt%, the fraction in the process for exhibiting corrosion resistance is not sufficient, and when magnesium (Mg) is added in an amount exceeding 2 wt%, the formation of a large amount of process phase increases the occurrence of cracks during processing.

[0041] In addition, the ratio of aluminum (Al) and magnesium (Mg) added to the plating bath should be at least 1:1 to minimize magnesium (Mg) oxidation, and preferably 1.2:1 or more. That is, the weight ratio of aluminum and magnesium in the plating bath is preferably 1.2 or more.

[0042] Aluminum (Al) present in the molten metal reacts with oxygen in the air to form a dense oxide film, thereby preventing oxygen from being supplied to the surface of the molten metal, thereby preventing magnesium (Mg) from being oxidized.

[0043] In the composition range of the present invention, the order of phases generated during solidification is that the primary Zn phase is generated first, and the eutectic phase solidifies after the formation of the primary Zn phase structure. In order to realize the composition desired by the invention within the plating layer, the cooling rate must be controlled within the range of 10 to 30°C / s, and can be strictly controlled within the range of 12 to 25°C / s.

[0044] When the cooling rate is less than 10℃ / s, the Zn single phase may solidify and exist as a single layer in the plating layer. When the cooling rate exceeds 30℃ / s, there is a risk that the plating surface shape may be deformed by the high-pressure cooling gas.

[0045] In addition, there is a limitation on the thickness of the plating layer in order for the primary Zn phase to form a multilayer structure in the plating layer. The thickness of the plating layer must be at least 15㎛ thick and 50㎛ thinner. If the thickness of the plating layer is thinner than 15㎛, it is not sufficient to form a multilayer structure of the primary Zn single phase, and if the thickness of the plating layer exceeds 50㎛, a flow pattern is created on the plating surface during solidification, which deteriorates the plating quality. In order for the primary Zn phase of the multilayer structure to sufficiently prevent crack propagation and improve corrosion resistance, the primary Zn phase of the multilayer structure must be composed of a phase fraction of 30% or more based on the cross-section of the plating layer.

[0046] The plated steel and its manufacturing method according to the technical idea of ​​the present invention described above can be summarized as follows.

[0047] A method for manufacturing a plated steel according to one embodiment of the present invention comprises the steps of: (a) providing a base iron; (b) passing the base iron through a plating bath containing aluminum (Al), magnesium (Mg), and zinc (Zn), thereby forming a plating layer on the base iron, the plating layer comprising 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities; and (c) cooling the plating layer at a cooling rate of 10 to 30°C / sec, wherein the weight ratio of aluminum to magnesium in the plating layer is 1.2 or more, and the thickness of the plating layer may be 15 μm to 50 μm. The plating layer after performing the cooling step may include a primary Zn phase structure and a eutectic structure, wherein the primary Zn phase structure may have a multilayer structure in the height direction of the plating layer. The area fraction of the primary Zn phase structure having the multilayer structure in the plating layer may be 30% or more. In the above cooling step, the primary Zn phase structure is first created, and the process phase structure can be created after the creation of the primary Zn phase structure.

[0048] Meanwhile, a plated steel according to an embodiment of the present invention includes: a base steel; and a plating layer formed on the base steel, the plating layer being composed of 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities; wherein the weight ratio of aluminum to magnesium in the plating layer is 1.2 or more. The plating layer includes a primary Zn phase structure and a eutectic structure, and the primary Zn phase structure may have a multilayer structure in the height direction of the plating layer. The area fraction of the primary Zn phase structure having the multilayer structure in the plating layer may be 30% or more. The thickness of the plating layer may be 15 μm to 50 μm.

[0049] To aid in understanding the present invention, preferred experimental examples are presented below. However, the following experimental examples are provided solely to aid in understanding the present invention, and the present invention is not limited to the following experimental examples.

[0050] Experimental example

[0051] Prepare a 0.7 mm thick steel specimen by immersing it in a 50°C alkaline solution for 30 minutes, then washing it with water to remove any foreign matter and oil from the surface. This specimen is then annealed and plated. Annealing is performed in a reducing atmosphere consisting of 5–20% hydrogen and 80–95% nitrogen, and the annealing heat treatment temperature is 700–850°C.

[0052] Plating is performed by cooling the annealed heat-treated specimen to the plating bath temperature, immersing it in the plating bath for 2 seconds, then pulling it up and adjusting the plating thickness according to conditions through nitrogen wiping. At this time, the plating bath temperature is set to 430℃ to 480℃.

[0053] The cold rolled steel sheet constituting the above-mentioned base steel has a composition of carbon: 0.15 wt%, manganese: 0.6 wt%, phosphorus: 0.05 wt%, sulfur: 0.05 wt%, and the remainder being iron (Fe).

[0054] Table 1 shows the composition and process conditions of the plated steel according to the experimental examples of the present invention, and the evaluation results for the processability of the plated layer, corrosion resistance of the processed area, and appearance quality of the plated surface according to the composition. It can be understood that the composition implementing the example among the experimental examples has a manufacturing tolerance of ±5% within the proposed composition range.

[0055] In Table 1, the Zn, Al, and Mg items represent the composition (unit: weight%) in the plating process, the plating thickness item is the thickness of the final plating layer, the cooling rate is the cooling rate in the cooling step (S40) illustrated in Figure 1, and the multilayer structure primary Zn phase fraction item represents the area fraction of the primary Zn phase multilayer structure based on the cross-section of the final plating layer.

[0056] In the evaluation of the plating layer processability, the evaluation was conducted based on the degree of crack occurrence in the processed area after 3T bending, using the following criteria. ◎ indicates cases where no cracks are observed visually, ○ indicates cases where relatively thin and fine cracks are observed visually, △ indicates cases where relatively thick and small cracks are observed visually, but there are concerns about the plating layer peeling due to the large number of cracks, and X indicates cases where relatively thick and large cracks are observed visually.

[0057] In the corrosion resistance evaluation of the machined part, the time for red rust occurrence was evaluated using a salt spray test with a 5% NaCl solution at 35℃ for the machined part after 3T bending. ◎ item corresponds to a case where the time for red rust occurrence is 1100 hours or more, ○ item corresponds to a case where the time for red rust occurrence is approximately 900 hours, △ item corresponds to a case where the time for red rust occurrence is approximately 700 hours, and X item corresponds to a case where the time for red rust occurrence is approximately 600 hours.

[0058] In the evaluation of the appearance quality of the plating surface, an item ○ is when there is no visible flow pattern, no oxide dross attachment, and no oxide wrinkles, and an item X is when there is any one of the visible flow pattern, oxide dross, or oxide wrinkles.

[0059]

[0060] ClassificationZnAlMg plating thickness(㎛)Cooling speed(℃ / s)Multilayer structurePrimary Zn phase fractionPlating layerProcessabilityProcessed areaCorrosion resistancePlating surface appearanceQualityComparative example 1Bal.0.2----◎X○Comparative example 2Bal.10.515125◎○○Comparative example 3Bal.12151231○◎xComparative example 4Bal.21101217△△○Comparative example 5Bal.21.215523△△○Comparative example 6Bal.21.2521262◎◎XComparative example 7Bal.3.51.2201041△△○Comparative example 8Bal.21.2253538◎◎XComparative example 9Bal.22.252 1225△△○Embodiment 1Bal.21151235○○○Embodiment 2Bal.21.2201236○○○Embodiment 3Bal.21.5251540◎◎○Embodiment 4Bal.21.5202551◎◎○Embodiment 5Bal.2.51.5302054◎◎○Embodiment 6Bal.1.71301567◎◎○Embodiment 7Bal.1.51251062○○○Embodiment 8Bal.1.81.4201052◎◎○

[0061]

[0062] Referring to Table 1, Examples 1 to 8 satisfy the composition range of aluminum (Al): 1 to 3 wt%, magnesium (Mg): 1 to 2 wt%, and the balance zinc (Zn), and among them, the weight ratio of aluminum and magnesium is 1.2 or more, and the base iron is immersed in a plating bath having a temperature of 430°C to 480°C, and then a plating layer having a thickness of 15 μm to 50 μm is formed by nitrogen wiping, and then cooling at a cooling rate of 10 to 30°C / sec, so that it can be confirmed that the area fraction of the primary Zn phase structure having a multilayer structure in the formed plating layer is 30% or more. Accordingly, in Examples 1 to 8, no visible cracks were observed in the processed portion after 3T bending, indicating excellent plating layer processability. In addition, when the red rust occurrence time was evaluated by a salt spray test using a 5% NaCl solution at 35°C on the processed portion after 3T bending, the red rust occurrence time was 1100 hours or more, indicating excellent corrosion resistance in the processed portion, and furthermore, it can be confirmed that the appearance quality of the plating surface is good.

[0063] In contrast, Comparative Example 1 is a Zn-Al plated steel without magnesium (Mg) added. The time for red rust occurrence was evaluated by a salt spray test using a 5% NaCl solution at 35°C on the processed area after 3T bending. As a result, the time for red rust occurrence was measured to be approximately 600 hours, confirming that the corrosion resistance of the processed area is not good.

[0064] Comparative Example 2 is a case where the magnesium (Mg) content does not satisfy the range of 1 to 2 wt% and falls below the range where the area fraction of the primary Zn phase having a multi-layer structure within the plating layer is 30% or more and falls below the range. In addition, when the red rust occurrence time is evaluated through a salt spray test at 35°C with a 5% NaCl solution on the processed area after 3T bending, it can be confirmed that the red rust occurrence time is about 900 hours and not 1100 hours. In addition, when magnesium (Mg) is added less than 1 wt%, the fraction in the process for exhibiting corrosion resistance is not sufficient, so the corrosion resistance of the processed area may not be sufficient.

[0065] Comparative Example 3 is a case where the plating bath composition satisfies the composition range of aluminum (Al): 1 to 3 wt%, magnesium (Mg): 1 to 2 wt%, and the balance zinc (Zn), but the weight ratio of aluminum to magnesium in the plating bath is lower than 1.2 or more, and it can be confirmed that the degree of cracking in the processed area after 3T bending is not so high that no cracks are observed with the naked eye, but rather relatively thin and fine cracks are observed with the naked eye, and it can be confirmed that the appearance quality of the plating surface is not good. When the weight ratio of aluminum to magnesium in the plating bath is lower than 1.2 or more, the aluminum added to minimize the oxidation of magnesium (Mg) in the plating bath is insufficient, and the supply of oxygen to the surface layer of the molten metal is not sufficiently blocked, which causes magnesium (Mg) to be oxidized, which may result in poor appearance quality of the plating surface.

[0066] Comparative Example 4 is a case where the plating bath composition satisfies the composition range of aluminum (Al): 1 to 3 wt%, magnesium (Mg): 1 to 2 wt%, and the balance zinc (Zn), and the weight ratio of aluminum and magnesium in the plating bath is 1.2 or more, but the thickness of the plating layer does not satisfy the range of 15 ㎛ to 50 ㎛ and falls short. If the plating layer thickness is thinner than 15 ㎛, it is not sufficient to make the primary Zn single phase into a multilayer structure, and it is confirmed that the area fraction of the primary Zn phase structure having a multilayer structure in the plating layer does not satisfy the range of 30% or more and falls short. After 3T bending, relatively thick and small cracks are observed with the naked eye in the processed area, but it is confirmed that there are many cracks and the plating layer is likely to fall off, so the plating layer processability is not good. After 3T bending, the red rust occurrence time was evaluated by a salt spray test in a 5% NaCl solution at 35℃ on the processed area, and as a result, the red rust occurrence time was approximately 700 hours. You can see that it doesn't reach 1100 hours.

[0067] Comparative Example 5 satisfies the composition range of aluminum (Al): 1 to 3 wt%, magnesium (Mg): 1 to 2 wt%, and the balance zinc (Zn), and the weight ratio of aluminum and magnesium in the plating bath is 1.2 or more, and the thickness of the plating layer satisfies the range of 15 μm to 50 μm, but in the cooling step of Fig. 1, if the cooling speed does not satisfy the range of 10 to 30°C / sec and falls below, the Zn single phase solidifies and exists as a single layer in the plating layer, and it is confirmed that the area fraction of the primary Zn phase structure having a multilayer structure in the plating layer does not satisfy the range of 30% or more and falls below, and after 3T bending, relatively thick and small cracks are observed with the naked eye in the processed area, but it is confirmed that there are many cracks and the plating layer is likely to fall off, so the plating layer processability is not good, and as a result of evaluating the red rust occurrence time by a salt spray test with a 5% NaCl solution at 35°C on the processed area after 3T bending, red rust It can be confirmed that the occurrence time is approximately 700 hours and less than 1100 hours.

[0068] Comparative Example 6 is a case where the plating bath composition satisfies the composition range of aluminum (Al): 1 to 3 wt%, magnesium (Mg): 1 to 2 wt%, and the balance is zinc (Zn), and the weight ratio of aluminum and magnesium in the plating bath satisfies 1.2 or more, but the thickness of the plating layer does not satisfy the range of 15 ㎛ to 50 ㎛ and exceeds it, and it can be confirmed that a flow pattern is created on the plating surface during solidification, so the appearance quality of the plating surface is not good.

[0069] Comparative Example 7 is a case where the aluminum (Al) content in the plating bath exceeds 3 wt%, which results in the generation of a large amount of ternary eutectic phase within the plating layer, resulting in the generation of a large number of plating layer cracks. In this case, the corrosion resistance of the processed area decreases due to the generation of a large number of plating layer cracks during processing due to a decrease in the fraction of the primary Zn phase and an increase in the fraction of the ternary eutectic phase.

[0070] Comparative Example 8 is a case where the cooling speed exceeds 30°C / sec, and due to the high cooling pressure, uneven oxidation wrinkles are created on the plating surface, which deteriorates the appearance quality of the plating surface.

[0071] Comparative Example 9 is a case where the plating bath composition exceeds 2 wt% of magnesium (Mg), and a large amount of two-phase phase is generated within the plating layer, resulting in a large number of plating layer tracks. Even in this case, as in Comparative Example 7, the corrosion resistance of the processed area is reduced due to the generation of a large number of cracks in the plating layer during processing due to a decrease in the fraction of the primary Zn phase and an increase in the fraction of the two-phase phase.

[0072] According to the experimental examples described above, it can be confirmed that by controlling the ratio of aluminum (Al) and magnesium (Mg) components and the thickness of the plating layer and controlling the solidification phase shape through the cooling rate, the structure of the primary Zn phase of the plating layer can be controlled from a single layer to a multi-layer structure, thereby realizing a highly corrosion-resistant plating steel having excellent crack resistance at the processed part and excellent corrosion resistance and a manufacturing method thereof.

[0073] While the above description focuses on specific embodiments of the present invention, those skilled in the art will appreciate that various modifications and variations can be made. As long as such modifications and variations do not depart from the scope of the present invention, they are considered to be within the scope of the present invention. Therefore, the scope of the present invention should be determined by the claims set forth below.

Claims

1. (a) Step of providing a possession iron; (b) a step of passing the base iron through a plating bath containing aluminum (Al), magnesium (Mg), and zinc (Zn), thereby forming a plating layer on the base iron composed of 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities; and (c) a step of cooling the plating layer at a cooling rate of 10 to 30°C / sec; including, The weight ratio of aluminum and magnesium in the above plating layer is 1.2 or more, Method for manufacturing galvanized steel.

2. In paragraph 1, The thickness of the plating layer is characterized by being 15㎛ to 50㎛. Method for manufacturing galvanized steel.

3. In paragraph 2, The plating layer after performing the cooling step includes a primary Zn phase structure and a process phase structure, wherein the primary Zn phase structure has a multilayer structure in the height direction of the plating layer. Method for manufacturing galvanized steel.

4. In paragraph 3, The area fraction of the primary Zn phase structure having the multilayer structure in the plating layer is 30% or more, Method for manufacturing galvanized steel.

5. In paragraph 3, In the cooling step, the primary Zn phase structure is first formed and the process phase structure is formed after the primary Zn phase structure is formed. Method for manufacturing galvanized steel.

6. So Ji-cheol; and A plating layer formed on the above-mentioned base material, comprising 1 to 3 wt% of aluminum (Al), 1 to 2 wt% of magnesium (Mg), and the remainder being zinc (Zn) and other unavoidable impurities; The weight ratio of aluminum and magnesium in the above plating layer is 1.2 or more, Galvanized steel.

7. In paragraph 6, The above plating layer includes a primary Zn phase structure and a process phase structure, The above-mentioned Zn phase structure has a multi-layer structure in the height direction of the plating layer. Galvanized steel.

8. In paragraph 7, The area fraction of the primary Zn phase structure having the multilayer structure in the plating layer is 30% or more, Galvanized steel.

9. In paragraph 7, The thickness of the plating layer is characterized by being 15㎛ to 50㎛. Galvanized steel.

Citation Information

Patent Citations

  • High yield ratio and high strength cold-rolled steel plate and high yield ratio and high strength galvanized steel plate excellent in weldability and ductility, and high yield ratio and high strength alloyed galvanized steel plate and its manufacturing method

    JP2005105367A

  • Coated steel plate and mehtod for manufacturing the same

    KR1020150135605A

  • A connector with built-in a cooling fan

    KR1020220052108A

  • System for detecting action of object by using infrared thermography image

    KR1020240011512A

  • Energy Saving Apparatus

    KR1020240128209A