Method for producing a modified carbon powder with plasma

WO2026196148A4PCT designated stage Publication Date: 2026-11-12BESCA AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/052534
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-03-17
Filing Date
2026-03-16
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional methods for producing hard carbon for sodium-ion batteries face challenges such as high energy consumption, high greenhouse gas emissions, inconsistent properties, and limited scalability, which affect the electrochemical performance and economic viability of the anode material.

Method used

A plasma-assisted method is used to convert biochar into hard carbon, utilizing microwave-generated plasma in an inert gas atmosphere to control carbonization, reducing energy consumption and emissions, and enabling continuous production.

Benefits of technology

The method produces high-quality hard carbon with consistent electrochemical properties, improving sodium-ion battery performance and scalability, while reducing environmental impact and operational costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026052534_12112026_PF_FP_ABST
    Figure IB2026052534_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a modified carbon powder by subjecting carbon powder to plasma in the presence of a first ionizable gas, thereby generating a modified carbon powder. The method also provides the option to further add elements to the modified powder to make it suitable for e.g., anodes to be used in batteries. The invention also provides a modified carbon powder produced by the method.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] NOVEL METHOD AND PRODUCT

[0002] BACKGROUND

[0003] Sodium-ion batteries (SIBs) are emerging as a cost-effective and sustainable alternative to lithium-ion batteries (LIBs), driven by the abundance and lower cost of sodium relative to lithium. As global demand for energy storage solutions increases, SIBs offer a promising option, particularly for grid-scale and stationary storage applications. A crucial component of SIBs is the anode material, which significantly impacts battery performance, cycle life, and efficiency. Among various anode candidates, hard carbon has demonstrated substantial potential due to its favorable electrochemical properties, including high capacity, good rate capability, and structural stability.

[0004] Challenges with Traditional Hard Carbon Production

[0005] Conventional methods for producing hard carbon, such as thermal carbonization, face several limitations that hinder their scalability and economic viability. These methods, including pyrolysis and hydrothermal carbonization, present the following challenges: The production of hard carbon typically requires high temperatures, often exceeding 1000°C. This intensive energy demand results in elevated operational costs and limits the feasibility of large-scale production US9,502,983. Biomass conversion to hard carbon via thermal carbonization suffers from low yield due to incomplete carbonization and material losses. This inefficiency contributes to increased waste and higher costs (Smith et al., "Advances in Biomass Pyrolysis for Carbon Materials," Journal of Electrochemical Energy, 2020). The high-temperature processing required for conventional hard carbon synthesis contributes to greenhouse gas emissions. Additionally, extended processing times further exacerbate energy use and environmental footprint EP3167432B1. The properties of hard carbon, such as porosity, surface area, and crystallinity, vary depending on the feedstock composition and carbonization conditions. This inconsistency affects the electrochemical performance of SIBs, limiting the reliability of commercially produced hard carbon materials (Doe et al., "Hard Carbon Performance in Sodium-lon Batteries," Materials Science Journal, 2021).Biochar can be derived from diverse biomass sources, including agricultural residues, forestry waste, and organic byproducts. This ensures a sustainable and renewable supply of raw materials US10,345,678. The utilization of biochar derived from waste biomass significantly reduces raw material costs compared to conventional carbon precursors such as petroleum coke or synthetic carbon sources. The production and use of biochar contribute to carbon sequestration, mitigating greenhouse gas emissions. Additionally, biochar byproducts can be used for soil amendment, further enhancing its environmental benefits WO2022 / 078234.

[0006] SUMMARY

[0007] Biochar, a carbon-rich material derived from the pyrolysis of biomass, presents an attractive alternative feedstock for hard carbon production. Its use offers multiple advantages: Biochar can be derived from diverse biomass sources, including agricultural residues, forestry waste, pulp and paper industry residue in the form of lignin and organic byproducts.

[0008] Biochar-based hard carbon exhibits high surface area, tunable porosity, and chemical stability, making it highly suitable for sodium-ion storage applications. These attributes can improve sodium ion diffusion and enhance battery performance.

[0009] To address the above-mentioned limitations of traditional hard carbon synthesis methods, plasma technology presents a novel and innovative approach for converting biochar into high-quality hard carbon suitable for SIB anodes. Plasma-assisted processing offers several advantages over conventional thermal methods.

[0010] Plasma processing enables rapid and controlled carbonization at lower overall energy consumption compared to conventional high-temperature pyrolysis, allowing precise control over carbon structure, improving the consistency of electrochemical properties critical for SIB anode performance. Elimination of prolonged high-temperature processing reduces carbon emissions, thereby contributing to a more sustainable manufacturing process.In addition, plasma processing techniques can be adapted to continuous production systems, improving scalability and making large-scale implementation viable for commercial applications.

[0011] The present invention represents a significant advancement in energy storage materials, leveraging biochar’s sustainability and the efficiency of plasma technology to produce high-performance hard carbon for sodium-ion batteries. By addressing critical challenges in traditional synthesis methods, this approach has the potential to enhance the economic and environmental viability of next-generation battery technologies.

[0012] CN113363468 discloses a method to modify hard carbon by plasma in an oxygen containing atmosphere to produce sodium battery electrodes.

[0013] The present invention provides a novel method to produce so-called hard carbon. According to the invention, carbon powder is treated by plasma in the presence of an ionizable gas, producing a hard carbon powder which is suitable for use in sodium-ion battery anodes. The invention also provides the carbon powder produced by the method and to products incorporating such carbon powder.

[0014] The invention is based on a method wherein carbon powder is subjected to plasma in the presence of an ionizable gas. The method can be modified by adding steps to further modify the carbon powder so that it incorporates additional elements, such as silicon, sodium, lithium, boron, phosphorous, nitrogen, functional groups such as alkyl groups. This step may also be referred to as pre-lithiation, or pre-sodiation.

[0015] The unique advantages of the hard carbon material produced via methods according to the invention are improved formation and stability of a solid electrolyte interface (SEI), improved mixability, and spreadability via slurry, and improved cycling stability.

[0016] BRIEF DESCRIPTION OF THE DRAWINGS.

[0017] Figure 1. Schematic overview of the method and system according to the invention. Figure 2. Overview of one embodiment according to the invention. The figure shows a schematic arrangement of the various components, feeding port; gas inlet, or manifold;powder hopper; powder feed screw; microwave source; waveguide; microwave reflector / tuner; quartz process tube; vacuum port; rotary motor and fitting for process tube; and a carbon products collection unit to collect the final modified carbon powder.

[0018] DETAILED DESCRIPTION

[0019] The present invention provides a method for producing a modified carbon powder by subjecting carbon powder to plasma in the presence of a first, ionizable gas. The method is carried out in a furnace, within which the microwave-generated plasma may be produced.

[0020] The microwave-generated plasma is preferably formed and stabilized in the furnace prior to injection of the carbon powder into the furnace plasma zone. In this context, a stable plasma is defined by minimized reflected power and minimal fluctuations in plasma power and temperature, comparable to process temperature stability in conventional industrial heating processes. This approach removes the need to add a Microwave Absorbing Material (MWA) or other conductive additive to the powder, thereby eliminating the need for an additional input and post-processing filtration or separation step, which is critical for continuous processing. Maintaining the stability of the plasma is vital for ensuring smooth operation and uniform material treatment, and requires different considerations for continuous operation than batch operation. In a continuous operating mode plasma stability is perturbed both by the physical disruption of the powder tumbling through the gas flows within the process tube, and the offgassing from the volatilized compunds being released from the powder during heating, leading to pressure spikes and potentially quenching of the plasma. This operational issue is non-trivial, and is one of the major factors dictating the scalability of the process as claimed, since it is directly impacted by material throughput.

[0021] The starting material, carbon powder, can be any type of carbon powder and is preferably a carbon powder with a reasonably uniform average particle size.

[0022] The method according to the invention is intended for the production of hard carbon powder and variants thereof and materials based on hard carbon powder by subjecting carbon powder, such as biochar, to conditions wherein an ionizable gas is ionized, usingelectromagnetic radiation for creating a plasma in the presence of a first, ionizable gas, thereby generating a modified carbon powder. The resulting modified carbon powder may thus be a hard carbon. The particles of the modified carbon powder obtained using the method of the invention may contain surface-bound functional groups derived from the chemistry of the plasma and the conditions of the process.

[0023] All aspects and embodiments disclosed herein can be combined with any other aspect and / or embodiment disclosed herein.

[0024] In accordance with the method, the carbon powder is subjected to plasma. The generation of the plasma can be done in different ways. Glow discharge, Capacitively coupled plasma (CCP), Inductively coupled plasma (ICP), Wave heated plasma (such as using helicon discharge or electron cyclotron resonance), Arc discharge, Corona discharge, Dielectric barrier discharge (DBD), Capacitive discharge, Piezoelectric direct discharge plasma, and Radiofrequency (RF) Plasma. Preferably, the plasma is generated by microwaves. Thus, the carbon powder may be heated by a microwave generated plasma.

[0025] By way of the above plasma-generation methods disclosed herein, microwave absorbing material (MWA) is not being utilized when producing the microwave-generated plasma. The method is carried out in a furnace, preferably a microwave transparent furnace. An example of such a furnace is a furnace made of quartz. It should be noted that the term furnace means any type of container that can contain plasma and ionizable gas at ambient atmosphere. In a preferred embodiment, the furnace is a closed furnace, thus allowing a pressure higher or lower than ambient pressure.

[0026] The furnace is preferably rotatable to promote uniform and time-controlled powder exposure to the plasma, as well as to facilitate movement of the powder through the furnace. It is standard industry practice to tumble powders and granules during thermal treatments, to ensure even heating and exposure, and this is still true with plasma treatment. In addition, the tumbling creates a mechanical polishing effect, thus rounding and smoothing the powder particles, thereby improving flowability thereof and promoting uniform powder shape. The rate of rotation of the furnace and the features of the mixing flights further contribute to the rate and aggressiveness of this mechanical polishing effect.There is also a non-negligible effect on the stability of the plasma, by the rotation Laminar flows created by the rotation of the furnace promote smoothing vortices within the outer edges of the formed plasma during operation.

[0027] As used herein, process tube means a tube traversing the furnace. Alternatively, the furnace may in itself constitute the process tube. The furnace or process tube is rotatable. Disclosures herein relating to the furnace being rotatable include the alternative of a process tube traversing the furnace being rotatable.

[0028] In one embodiment, the furnace rotates at 0.01 - 100 rpm, e.g. 0.1 - 50 rpm, preferably 1 - 10 rpm, in intervals defined by the resolution of the rotary motor.

[0029] The carbon powder may enter the furnace by way of a continuous feed mechanism, preferably one or more powder feed screws. Likewise, the plasma-treated carbon powder may be removed from the furnace by a continuous feed mechanism, which may be the same feed mechanism as the feed mechanism introducing the carbon powder into the furnace.

[0030] When a continuous feed mechanism is not being used, the furnace angle is preferably set at an appropriate degree, ranging from 5 to 60 degrees to the horizontal, to ensure proper entry and removal of the powder from the furnace. When the furnace is rotating, the furnace angle may be 0 degrees also in the absence of any continuous feed mechanism.

[0031] In one embodiment, a continuous feed mechanism is being used, and / or the furnace angle is set at a degree from 5 to 60 degrees to the horizontal. In one embodiment, the furnace angle is in a range from 5 to 60 degrees to the horizontal, and the furnace is rotating. Thereby, a continuous feed mechanism may be dispensed with.

[0032] The carbon powder’s particle residence time in the furnace depends on the combination of one or more of the following three factors: rotation speed, continuous feed mechanism speed, and furnace incline. Adjusting these factors results in a precise and adjustable carbon powder residence time in the furnace. The method and system as disclosed enables large-scale treatment of coal powder.By the combination of any or several of rotation speed, continuous feed mechanism speed, and furnace incline, entry of the coal powder into the furnace is facilitated. Thereby, a wider range of powder sizes may be the subject for treatment. Hence, larger coal particles may also be made use of. Sieving and size exclusion steps may be dispensed with.

[0033] In accordance with the invention, a conveying gas is not used to feed carbon powder into the furnace, nor to facilitate powder removal from the furnace.

[0034] In one embodiment, the carbon powder has a particle size distribution such that 80% of the particles are in the size range of about 5 pm to 75 pm, preferably from about 10pm to 50 pm, more preferably from about 10pm to about 20pm. The size distribution can be measured by sieve analysis, laser scattering, or other methods known by the skilled person for determining particle sizes according to known methods.

[0035] In one embodiment, the carbon powder has an average particle size of from about 0.01 pm to 10000 pm, preferably from about 10 pm to about 50 pm.

[0036] In one embodiment, the carbon powder is biochar.

[0037] In one embodiment, the first ionizable gas is at least one gas chosen from the group comprising nitrogen, helium, neon, argon, xenon, krypton, carbon dioxide, methane, and hydrogen. Preferably, the gas is selected from nitrogen, argon, xenon, krypton, carbon dioxide, methane, and hydrogen. In one embodiment, the first ionizable gas is an inert gas.

[0038] In one preferred embodiment, the method is carried out at an atmosphere essentially free from oxygen.

[0039] In a preferred embodiment, the amount of oxygen during plasma treatment is below 10% by volume, preferably below 5%, more preferably below 1%, most preferably below 10ppm, by volume.

[0040] The first gas composition is ideally 99.9% nitrogen and 0.1% oxygen.The hard carbon material characteristics are tunable by adjusting process parameters, including the following: plasma processing time up to 600 minutes, amount of oxygen present during plasma treatment, and microwave output power.

[0041] In one embodiment, the microwave energy output ranges from 0.1-100kW, and is preferably at least 10kW.

[0042] In a further embodiment, at least one additional element is added to the coal powder, using a second gas. The second gas may be chosen for incorporating functional groups or elements such as silicon, lithium, sodium, nitrogen, boron, methane, phosphorous, sulfur, or a mixture of two or more of these. In one embodiment, at least one additional element, chosen from the group comprising silicon, sodium, lithium, boron, phosphorous, nitrogen, and functional groups, such as alkyl groups, is added in the furnace using a second gas.

[0043] An additional element may be added by plasma enhanced chemical vapor deposition (PECVD). Preferably, at least one additional element, chosen from the group comprising silicon, sodium, lithium, boron, phosphorous, nitrogen, and functional groups, such as alkyl groups, is added in the furnace using a second gas.

[0044] In one embodiment, the carbon powder is introduced into the furnace by a continuous feed mechanism.

[0045] In one embodiment, the plasma treated carbon powder is removed from the furnace by a continuous feed mechanism.

[0046] Volatiles contained within the carbon powder material are evaporated and broken down within the plasma.

[0047] In another aspect, the invention provides a system for producing a modified carbon powder, comprising a furnace which houses a first continuous aligned feed-in device arranged at an angle of from 0 degrees to 60 degrees to the horizontal and a microwave plasma generator; and a waveguide to direct the energy from the microwave plasma generator to the furnace. All components contained in the system as described are located in proximity to the main process tube such that the ionizing radiation is directed to and constrained within the desired process reaction zone without impeding theinclination or rotation of the process tube, or the operation of the powder feed-in device. In one configuration, the microwave plasma generator and associated waveguide / tuning components are mounted directly adjacent to the process tube such that they may move as the inclination of the process tube is changed. In another configuration, the microwave plasma generator may be located adjacent or in proximity to the main system including the process tube, and the ionizing radiation is guided a short distance via the waveguides to the furnace reaction zone within the process tube, where reflectors and tuning components may focus and shape it to obtain a stable and uniform plasma.

[0048] The waveguide and reflector / tuner assembly enables the ionizing radiation to be directed to and confined within the desired furnace reaction zone. The waveguide and tuner components are designed such that a stable and uniform plasma is generated and maintained within the furnace reaction zone, while minimizing excess radiation leakage into the working environment.

[0049] The system may further comprise a powder mill, which may be located adjacent or external to the plasma treatment system, or connected directly to the powder delivery system. Preferably, the powder mill is located prior to the furnace. The powder mill ensures that the carbon powder is of a desired size, prior to modification thereof. In situations where the powder mill is utilized, its purpose is to ensure powder feedstock is of a desired particle dimension and uniformity as per application requirements.

[0050] In a further embodiment, the system comprises a waveguide to direct the energy to the furnace.

[0051] In one embodiment according to Figure 2, the system comprises a powder hopper and powder feed screw which holds the input carbon powder and feeds it into the furnace at a controlled rate. The furnace, associated with a microwave source equipped with a tuning system and a wave guide, endcaps, rotary motor, fixtures, gas manifold, and mount to ensure the entire assembly is preferably arranged at a specific angle of from 0 degrees to 60 degrees to the horizontal, or 5 to 60 degrees to the horizontal, preferably 5 to 30 degrees to the horizontal, more preferably at an angle of 5 degrees from the horizontal. The incline of the furnace is adjustable during operation of the method and system.In a further embodiment, the modified carbon collection unit includes a filter to separate the process exhaust gasses from the modified carbon powder, and optionally a vacuum line connected to a vacuum pump, allowing for flow and removal of process exhaust gasses, and optionally a vessel for catching and storing the modified carbon powder, and optionally airtight fittings to ensure that the modified carbon powder is not exposed to atmospheric oxygen before it has had time to cool to suitable temperature.

[0052] The powder delivery hopper and collection hopper are both standard systems which can be purchased off the shelf and integrated.

[0053] In one embodiment, the invention provides a system according to Figure 2.

[0054] The method can be described in a non-limiting fashion as follows.

[0055] The powder may be fed directly into a hopper with a gas-tight lid and screw feed. The air may then be replaced with a gas such as nitrogen or argon.

[0056] The internal volume of the furnace may be purged of oxygen via a combination of vacuum suction and purging with gas such as nitrogen or argon.

[0057] The furnace angle may be set to an appropriate degree, ranging from 0 to 60 degrees, but ideally at a 5-degree incline from the horizontal.

[0058] Furnace rotation may be initiated at a speed ranging from 0.01 to 100 rotations per minute (rpm), with an ideal setting of 5 rpm.

[0059] A first gas, potentially comprising any percentage of inter alia nitrogen, argon, carbon dioxide, oxygen, air, methane, hydrogen, or a mixture thereof, may then be introduced into the furnace at a set flow rate ranging from 0.01 - 100L / min. The gas composition may consist of 99.9% nitrogen and 0.1% oxygen, and the flow rate is ideally 1L / min. Once a suitable operating pressure ranging from 133Pa to 101 kPa (or atmospheric pressure) and gas composition is reached, the furnace interior is subjected to electromagnetic radiation, such as microwave radiation, generating plasma within the furnace. The furnace may be a quartz chamber.

[0060] A motorized tuning paddle is used to minimize reflected energy and to stabilize the plasma.Once the plasma is stable, the powder feed is activated, and the carbon powder, such as biochar, is fed into the plasma reactor at a rate between 0.001 kg / min and 100kg / min, such as 1 kg / min.

[0061] The carbon powder is moved through the active plasma zone by rotation of the furnace in combination with gravity from the tilt angle, allowing it to be carbonized and converted into modified carbon powder, such as hard carbon, in a rapid and continuous manner. Volatiles contained within the carbon powder material are evaporated and broken down within the plasma and carried away as atomic gases via an exhaust system.

[0062] As the modified powder exits the process tube the process gas is filtered out and pumped to the exhaust via a vacuum pump. The modified powder is collected in a collection chamber, wherein the processed powder is held until the operation is completed and the powder has cooled to a temperature below its auto-ignition temperature. To prevent contamination or accidental oxidation, the powder is kept under the same atmosphere as was applied at the start of the process.

[0063] The main component of the plasma system is an electromagnetic source, such as a microwave source, which may be a magnetron or a solid-state semiconductor, having a microwave energy output ranging from 1 -100 kW, but preferably in an arrangement where at least 10kW of microwave energy is delivered to each process tube. The microwave system may include a waveguide to direct the energy to the process tube, or to split the microwave energy evenly and redirect it to multiple process tubes, as well as a motor-driven tuning paddle which is moved to adjust reflected microwave energy and minimize the potential for damaging heat buildup within the microwave source. The process tube is fabricated with high purity quartz glass, and is oriented horizontally, or about 3 to about 15 degrees from the horizontal plane, transversely to the direction of the microwave radiation from the microwave source. Quartz is transparent to microwave radiation and therefore allows the microwaves to pass through the sidewalls and ionize the process gasses flowing within tube. This configuration of magnetron and process tube simplifies the function of the system and allows for a plasma zone large enough for commercial scale operations to be generated. More importantly, it allows the powder material to beexposed to the process plasma for a longer amount of time while still allowing for continuous throughput.

[0064] From a commercial production perspective, this process requires at least 50% less input energy, 24x reduction in time per kg produced, 50% less footprint in terms of equipment floorspace per kg produced, and 100% reduction in chemical waste produced per kg compared to conventional methods as described above.

[0065] The carbon footprint per kg produced using this process is estimated to be significantly less than conventional methods utilizing carbon feedstocks from non-renewable sources. In yet another aspect, the invention provides a hard carbon powder which is obtainable by the method according to the first aspect and embodiments thereof.

[0066] In one aspect of the invention, there is provided a modified carbon powder characterized in that the particles of the modified carbon powder have a higher surface energy compared with particles of a non-plasma treated carbon powder. The modified carbon powder is obtainable using the method disclosed herein.

[0067] The hard carbon powder may be characterized by porosity, specific surface area, specific hardness, X-ray diffraction properties, Raman spectroscopic properties, electron paramagnetic resonance properties and four-point electrical conductivity measurements, using methods known to the skilled person.

[0068] Furnace rotation provides a continuous grinding and polishing effect on the powder particles, through particle-particle and particle-furnace wall contact, leading to removal of outer oxide layers, improved particle sphericity and general surface purity Hence, one aspect of the invention relates to particles of the modified carbon powder being devoid of any oxide layer. In one embodiment of the invention, supplemental powders may be added to the feedstock to further improve the grinding and polishing effect.

[0069] The method and system according to the invention provides high production capacity. The plasma treatment zone may extend throughout the furnace, which may moreover be extended commensurate with the manufacturing needs, since the plasma reaction zone is uniform. The production capacity may be, or exceed, 100 kg modified carbon powder per hour.One aspect of the invention relates to an anode material containing carbon powder according to the above.

[0070] Yet another aspect of the invention relates to a battery comprising an anode material according to the above aspect.

[0071] In a sodium cell anode, comprising the hard carbon according to the invention, cyclic voltammetry curves show functional charge / discharge characteristics indicative of sodium intercalation within the hard carbon structure.

Claims

AMENDED CLAIMSreceived by the International Bureau on 23 September 2026 (23.09.2026)1. Method for producing a modified carbon powder by subjecting carbon powder to plasma in the presence of a first, ionizable gas, characterized in that the method is carried out in a rotatable furnace set at an angle to the horizontal from 0 to 60 degrees, wherein the carbon powder is subjected to treatment with microwave- generated plasma generated and contained within the furnace plasma zone, and an ionizable gas, thereby generating a modified carbon powder, and wherein the carbon powder enters the furnace by a continuous feed mechanism, and the plasma treated carbon powder is removed from the furnace by a continuous feed mechanism.

2. Method according to claim 1 , wherein the microwave-generated plasma is formed and stabilized in the furnace prior to introduction of the carbon powder into the furnace plasma zone.

3. Method according to claim 1 or 2, wherein microwave absorbing material (MWA) is not being utilized when producing the microwave-generated plasma.

4. Method according to any of the preceding claims, characterized in that a conveying gas is not used to feed carbon powder into the furnace.

5. Method according to claim 4, wherein the furnace is set at an angle to the horizontal ranging from 5 to 60 degrees.

6. Method according to claim 5, wherein the furnace is set at an angle to the horizontal of 5 degrees.

7. Method according to claim 6, wherein the furnace rotates at 0.01 - 100 rpm.

8. Method according to any of the preceding claims, wherein the carbon powder has an average particle size distribution such that at least 80% of the particles are in the size range of about 5 pm to 75 pm.

9. Method according to any one of claims 1 - 8, wherein the carbon powder has an average particle size of from about 0.01 pm to 10000 pm, preferably from about 10 pm to about 50 pm.

10. Method according to any of the preceding claims, wherein the carbon powder is biochar.

11. Method according to any one of the preceding claims, wherein at least one additional element, chosen from the group comprising silicon, sodium, lithium, boron, phosphorous, nitrogen, and functional groups such as alkyl groups is added in the furnace, using a second gas.

12. Method according to any one of the preceding claims, wherein at least one additional element, chosen from the group comprising silicon, sodium, lithium, boron, phosphorous, nitrogen, and functional groups such as alkyl groups is added in the furnace by plasma enhanced chemical vapor deposition (PECVD).

13. Method according to any one of the preceding claims, wherein the first, ionizable gas is at least one gas chosen from the group comprising nitrogen, argon, xenon, krypton, carbon dioxide, methane, and hydrogen.

14. Method according to any of the preceding claims, wherein the amount of oxygen during plasma treatment is below 10% by volume, preferably below 5%, and more preferably below 1%.

15. Method according to claim 14, wherein the method is carried out in an atmosphere of less than 10 ppm oxygen, by volume, preferably an atmosphere essentially free from oxygen.

16. Method according to any of the preceding claims, wherein the resulting modified carbon is hard carbon.

17. System for producing a modified carbon powder, comprising a rotatable furnace arranged at an angle of from 0 degrees to 60 degrees to the horizontal which houses a first continuous aligned feed-in device comprising one or more powder feed screws; a microwave plasma generator; and a waveguide to direct the energy from the microwave plasma generator to the furnace.

18. System according to claim 17, further comprising a powder mill located prior to the furnace.

19. Modified carbon powder obtainable by the method according to any one of claims 1 to 16.

20. Modified carbon powder obtainable by the method according to any of claims 1- 16, characterized in that the particles of the modified carbon powder have a higher surface energy compared with particles of a non-plasma treated carbon powder.21.Anode material comprising or containing a carbon powder according to any one of claim 19 - 20.

22. Battery comprising an anode material according to claim 21.