Method for producing microstructure containing metallic magnesium, and said microstructure

The method of photolithography and electroplating allows for the production of microspicules with controlled shape and size, addressing the challenges of existing spicule technologies and improving drug delivery and cosmetic efficacy.

WO2026235200A1PCT designated stage Publication Date: 2026-11-12THE UNIV OF TOKYO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017693
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for producing artificial spicules, such as those derived from marine sponges or aluminum oxide, face challenges in achieving consistent shape and size, and laser processing of magnesium for precise shapes is difficult due to its reactivity and low melting point.

Method used

A method involving photolithography to create a predetermined pattern on a conductive substrate followed by electroplating is used to form microstructures with metallic magnesium, allowing for controlled shape and size production.

Benefits of technology

This method enables the production of microspicules with specific shapes and dimensions, enhancing transdermal drug delivery and cosmetic applications by improving skin permeability and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017693_12112026_PF_FP_ABST
    Figure JP2026017693_12112026_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide a novel method for artificially producing a microspicule having a specific shape and dimensions allowing for easy subcutaneous puncture. [Solution] A method for producing a microstructure containing metallic magnesium, the method comprising: (1) a step for providing, on a conductive substrate, a resist layer having a prescribed pattern formed by photolithography; and (2) a step for forming, by electrolytic deposition (electroplating) on the conductive substrate, a microstructure containing metallic magnesium within the pattern.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a microstructure containing metallic magnesium and said microstructure

[0001] The present invention relates to a method for producing a microstructure containing metallic magnesium that can be used as an artificial spicule, and to the microstructure itself.

[0002] Transdermal drug delivery systems (DDS) offer various advantages in skin treatment. These include reduced drug degradation, improved stability, and continuous, controlled drug delivery (Non-Patent Literature 1). In particular, they contribute to improved therapeutic efficacy through direct access to target sites and lesion sites.

[0003] On the other hand, the stratum corneum, the outermost layer of the skin, acts as a barrier protecting against the external environment. For this reason, the penetration rate of transdermal drugs with physicochemical properties suitable for local treatment is limited (Non-Patent Literature 2). To overcome this problem, microneedles aimed at increasing skin permeability are attracting attention. They have a length of 1 mm or less, minimizing pain during skin puncture. Furthermore, they can penetrate the stratum corneum, the skin's barrier, without damaging blood vessels or nerves, making them highly effective in drug delivery (Non-Patent Literature 3). In addition, as a similar physical approach, research on artificial spicules that can be adapted to any area of ​​the skin for transdermal drug delivery has recently attracted attention (Non-Patent Literature 1).

[0004] Spicule structures, derived from natural structures, have recently attracted attention as a technology for enhancing skin penetration. Spicules are bone needles derived from marine sponges (Sponge Haliclona spicules, hereinafter also referred to as "SHS"), and it has been shown that silica-based spicules can be used for transdermal drug delivery. SHS are a material that supports the structure in many sponges, and it has been reported that using SHS on the skin creates micropores, which significantly improves transdermal drug absorption (Non-Patent Literature 1).

[0005] However, SHS has the problem that, being a natural material, its shape and size are not consistent. Also, STAR particles, a type of artificial spicule composed of aluminum oxide or stainless steel, show excellent performance in transdermal drug delivery, but the laser processing method used to manufacture these STAR particles makes it difficult to produce them in precise shapes.

[0006] S. Zhang et al., “Skin delivery of hydrophilic biomacromolecules using marine sponge spicules,” Molecular Pharmaceutics, vol. 14, pp. 3188-3200, 2017. Y. Kim et al., “Tolerability, acceptability, and reproducibility of topical STAR particles in human subjects,” Bioengineering & Translational Medicine, vol. 8, no. 3, e10524, Apr. 2023.H. Jing et al., “Fabrication of a Polyglycolic Acid Porous Microneedle Array Patch Using the Non-Solvent Induced Phase Separation Method for Body Fluid Extraction,” Nano Select, vol. 5, no. 10, pp. 1-14, Oct. 2024.

[0007] The present invention aims to provide a novel method for artificially producing microspicules having a specific shape and dimensions that facilitate subcutaneous puncture. Furthermore, the present invention also aims to provide such microspicules having a specific shape and dimensions.

[0008] Microspicules are particles with tiny, star-shaped protrusions that can create microscopic pores in the stratum corneum of the skin. This mechanism is expected to significantly improve the delivery efficiency of locally administered drugs and to enable local administration of drugs that were previously limited to injections or oral administration.

[0009] Meanwhile, in the biomedical field, magnesium (Mg) is a material that has recently attracted attention due to its unique physiological properties. As a biocompatible material, Mg has the characteristic of naturally decomposing under physiological conditions and is attracting attention as a material for implantable medical devices and DDS (Drug Delivery Systems). Furthermore, although Mg is an essential mineral, it cannot be synthesized in the body and must be obtained from external sources. Therefore, in the body, externally derived Mg is absorbed and broken down, and mainly exists as Mg ions. It has been reported that an appropriate amount of Mg ions plays an important role in maintaining skin health, as opposed to adverse effects such as skin spasms, anxiety, and arrhythmias caused by Mg ion deficiency, in cellular energy metabolism (e.g., cofactor of ATP synthase), inflammation regulation (e.g., suppression of inflammatory cytokines (TNF-α, IL-6)), and tissue repair.

[0010] Therefore, the inventors focused on the effect of Mg ions and considered producing artificial spicules using Mg as the material. However, because Mg is highly reactive, has a low melting point, and is easily affected by temperature, it is difficult to produce precise shapes using the laser processing method used in the production of STAR particles in previous studies. To address this problem, the inventors conceived the idea that it would be possible to produce microstructures with controllable shape and size using Mg as the material by utilizing electrolytic deposition, or more specifically, electroplating. After diligent research, they completed the present invention.

[0011] In other words, the present invention has the following configuration: [1] A method for manufacturing a microstructure containing metallic magnesium, comprising: (1) the step of providing a resist layer having a predetermined pattern formed by photolithography on a conductive substrate; and (2) the step of forming a microstructure containing metallic magnesium inside the pattern on the conductive substrate by electroplating. [2] The method according to [1], wherein the conductive substrate is a metal electrode or metalloid electrode having a silicon substrate on at least one surface. [3] The method according to [1] or [2], wherein magnesium is used as the anode and the metal electrode or metalloid electrode is used as the cathode. [4] The method according to [2] or [3], wherein the metal electrode or metalloid electrode is an electrode of at least one metal selected from the group consisting of copper, stainless steel, graphite, molybdenum, titanium, platinum, nickel, and magnesium. [5] The manufacturing method according to [4] or [5], wherein the conductive substrate comprises a metal or semimetallic electrode, a layer containing a conductive adhesive provided on at least one surface of the electrode, and a silicon substrate provided on the layer containing the conductive adhesive. [6] The manufacturing method according to any one of [1] to [5], wherein the resist layer is a negative resist layer, a lift-off negative resist layer, a film-like negative resist layer, or a crosslinkable positive resist layer. [7] The manufacturing method according to any one of [1] to [6], wherein a magnesium-containing microstructure is formed in a size and shape corresponding to the pattern. [8] The manufacturing method according to any one of [1] to [7], wherein the pattern has a pointed shape. [9] The manufacturing method according to any one of [1] to [8], wherein the pattern is triangular, polygonal, star-shaped, elongated needle-shaped (for example, a sword-like shape), or a combination thereof.

[10] 1 to 100 mA / cm 2 range (preferably 30 to 60 mA / cm²) 2 A manufacturing method according to any one of items [1] to [9], wherein electroplating is performed at a current density of )

[11] 30 to 60 mA / cm 2

[10] A manufacturing method according to

[10] , wherein electroplating is performed at a current density in the range of [1].

[12] A manufacturing method according to any one of [1] to

[11] , wherein the microstructure is a particulate microneedle.

[13] A microstructure obtained by the manufacturing method according to any one of [1] to

[12] .

[14] A microstructure according to

[13] used as an artificial spicule.

[15] A cosmetic composition comprising the microstructure according to

[13] or

[14] .

[16] A microstructure comprising metallic magnesium, wherein the microstructure has a pointed shape.

[17] A microstructure according to

[16] , wherein the shape is triangular, polygonal, star-shaped, elongated needle-shaped (for example, a sword-like shape), or a combination thereof.

[18] A microstructure according to

[17] , wherein the side length in the shape is 20 μm to 1000 μm.

[19] A microstructure according to

[17] or

[18] , wherein the thickness is 10 to 50 μm.

[20] A microstructure according to any one of

[16] to

[19] , used as an artificial spicule.

[21] A cosmetic composition comprising a microstructure according to any one of

[16] to

[20] .

[0012] This invention makes it possible to create spicules of various arbitrarily designed shapes, which was not possible with existing randomly shaped spicules. Furthermore, by adjusting the electroplating conditions, the thickness of the spicules can be controlled, and applications are expected not only in transdermal drug delivery but also in other fields such as cosmetics.

[0013] A schematic diagram of the processing apparatus used in the example is shown. The results of pattern fabrication by photolithography are shown. The electrode arrangement diagram and fixing photographs are shown. Mg plating on a silicon substrate is shown (a: 10 minutes, b: 30 minutes). The results of microscopy, SEM, and EDS analysis of samples a and b are shown. The current density conditions for samples c and d are shown. The results of SEM and EDS elemental analysis of samples c and d are shown. The thickness of Mg formation in samples c and d is shown. The results of SEM and EDS elemental analysis of sample e are shown. Embodiment of the Invention

[0014] 1. Method for Manufacturing a Microstructure Containing Metallic Magnesium One embodiment of the present invention is a method for manufacturing a microstructure containing metallic magnesium, comprising: (1) a step of providing a resist layer having a predetermined pattern formed by photolithography on a conductive substrate; and (2) a step of forming a microstructure containing metallic magnesium inside the pattern on the conductive substrate by electroplating (electrolytic deposition) (hereinafter also referred to as "the manufacturing method of the present invention"). In this specification, "microstructure containing metallic magnesium" and "microstructure containing metallic magnesium" have the same meaning.

[0015] Spicles derived from marine sponges have the problem of not being consistent in shape and size because they are made from a natural material. In developing a method to artificially manufacture microspicules with specific shapes and dimensions that are easy to insert subcutaneously, the inventors focused on magnesium (Mg), which is biocompatible, as a material for artificial microspicules. However, Mg is highly reactive, has a low melting point, and is easily affected by temperature, making it difficult to manufacture precise shapes using the laser processing method used in the production of STAR particles in previous studies. Therefore, in order to manufacture artificial spicules using Mg as a material, a technology is required to process magnesium into a specific shape. In exploring Mg processing technologies, Melissa Tsang et al. reported on their research into Mg-based batteries (secondary batteries) that they were able to precisely process continuous and densely stacked Mg with a specific shape using electroplating (M. Tsang et al., “Development of electroplated magnesium microstructures for biodegradable devices and energy sources,” Journal of Microelectromechanical Systems, vol. 23, no. 6, pp. 1281-1289, Dec. 2014). Focusing on this, the present inventors developed a method for manufacturing microstructures with controllable shape and size using Mg as the material, utilizing electroplating (electrolytic deposition).

[0016] Electroplating is a processing technique that forms a film (or deposit) of metallic magnesium on a conductive substrate such as an electrode. However, in order to develop a process that can stably manufacture Mg microstructures of a specific shape, it is necessary to precisely control the shape of the magnesium film (or deposit) to be formed. In the manufacturing method of the present invention, a step is provided in which a pre-designed pattern is formed on a conductive substrate using photolithography. Through this step, magnesium is plated only inside the fabricated pattern, making it possible to manufacture Mg spicules with a specific shape.

[0017] The various components of the manufacturing method of the present invention are described in detail below.

[0018] (1) Step (1) The manufacturing method of the present invention includes, as step (1), a step of providing a resist layer having a predetermined pattern formed by photolithography on a conductive substrate.

[0019] (1-1) Conductive substrate The conductive substrate is preferably a metal electrode or metalloid electrode commonly used in electroplating. The metal or metalloid electrode is preferably an electrode made of at least one metal selected from the group consisting of copper, stainless steel, graphite, molybdenum, titanium, platinum, nickel, and magnesium.

[0020] As the conductive substrate, the metal or metalloid electrode described above can be used as is, but it is preferable to use a metal or metalloid electrode on which a silicon substrate is provided on at least one surface. Forming a predetermined pattern by photolithography usually involves steps such as coating a photoresist onto the substrate, exposing the photoresist layer to light, and removing unexposed areas with a developer. It is preferable to perform the formation of a predetermined pattern by such photolithography on a silicon substrate, which has excellent flatness and thermal stability.

[0021] Furthermore, in addition to silicon substrates, if a template is formed with photoresist on a thin metal film (which is also used as a metal electrode), a substrate compatible with photolithography (for example, a glass substrate) can also be used.

[0022] In one preferred embodiment of the manufacturing method of the present invention, the conductive substrate comprises a metal electrode or a metallometallic electrode, a layer containing a conductive adhesive provided on at least one surface of the metal electrode or metallometallic electrode, and a silicon substrate provided on the layer containing the conductive adhesive. By providing a layer containing a conductive adhesive between the silicon substrate and the metal or metallometallic electrode, the adhesion between the silicon substrate and the electrode can be stably maintained.

[0023] Various conductive adhesives can be used, such as epoxy, acrylic, and silicone-based adhesives. For example, conductive adhesives using silver powder as a filler and acrylic resin as a binder (such as Fujikura Chemical's Dotite D-550, D-362, and D-550) can be used.

[0024] To form a resist layer having a predetermined pattern formed by photolithography on a conductive substrate, either by directly forming the resist layer on the conductive substrate, or by first forming the resist layer on a substrate for resist layer formation, such as a silicon substrate, and then laminating the silicon substrate with the resist layer onto a metal electrode or a metalloid electrode (preferably laminating via a layer containing a conductive adhesive), the latter method is preferred. Below, a method for forming a resist layer having a predetermined pattern by photolithography will be described, specifically a method for first forming the resist layer on a substrate for resist layer formation, such as a silicon substrate (hereinafter referred to as a "silicon substrate" for simplicity of explanation).

[0025] (1-2) Formation of a resist layer having a predetermined pattern A method for forming a resist layer having a predetermined pattern on a silicon substrate by photolithography includes at least the steps of (a) applying a photoresist onto a conductive substrate to form a resist film, (b) exposing the resist film, and (c) removing unexposed areas with a developer. Each of steps (a) to (c) will be described below.

[0026] (a) A step of applying a photoresist onto a conductive substrate to form a resist film. (a-1) Photoresist It is preferable to use a photoresist that can produce a negative resist layer, a lift-off negative resist layer, a film-like negative resist layer, or a crosslinkable positive resist layer (hereinafter also referred to as "negative photoresist," "lift-off negative photoresist," "film-like negative photoresist," and "crosslinkable positive photoresist," respectively). It is more preferable to use a negative photoresist because the exposed portion hardens and can be used as a mold, and in step (2) described later, a film (microstructure) containing metallic magnesium can be effectively formed inside a predetermined pattern by electroplating.

[0027] Examples of negative-type photoresists include novolac resins, acrylic resins, epoxy resins (for example, thick-film negative-type photoresists such as SU-8), silsesquioxanes, and siloxane resins.

[0028] For lift-off negative photoresists, for example, Microchemicals' AZ 15nXT and AZ 125nXT-10B can be used. For film-type negative photoresists, for example, Nippon Kayaku's SU-8DFR series and KPM DFR series can be used. For crosslinkable positive photoresists, for example, Toray's LT and PW series can be used.

[0029] (a-2) Formation of the resist film To form a resist film on a silicon substrate, first, a photoresist is applied to the surface of the silicon substrate. The photoresist is usually applied to the substrate by applying a photoresist solution, which is a photoresist dissolved in an organic solvent, using a coater, coating machine, screen printing, etc. Preferably, the photoresist is applied by spin coating the photoresist solution onto the silicon substrate.

[0030] Before applying the photoresist, the surface of the silicon substrate may be cleaned and dried. After applying the photoresist solution to the substrate, the substrate is heated (pre-baked) before exposure to evaporate the solvent and form a resist film. Pre-baking can be done using an oven or hot plate, and the solvent is usually removed by heating at a temperature of around 100°C for several tens of seconds to several minutes. The heating temperature and heating time can be arbitrarily determined depending on the type of photoresist used.

[0031] Furthermore, a sacrificial layer may be provided before applying the photoresist. A metal layer is preferred as the sacrificial layer, and examples include aluminum-based (Al) and copper-based (Cu) metal layers. By providing a sacrificial layer in advance beneath the resist layer, when recovering microstructures containing metallic magnesium after formation, it is possible to recover the microstructures industrially and stably while maintaining and controlling the fine shape with pointed tips that the microstructures preferably have, by etching only the sacrificial layer. The metal sacrificial layer can be formed on the surface of the silicon substrate by sputtering, vapor deposition, plating, etc. After forming the metal sacrificial layer, the resist film can be formed after cleaning and drying the metal surface.

[0032] (b) Step of exposing the resist film The step of exposing the resist film includes irradiating the resist film obtained in step (a) with light using a photomask on which a predetermined pattern is drawn.

[0033] The type of light used to irradiate the resist film can be the same type of light commonly used in photolithography to form micron to submicron sized patterns. For example, g-line, i-line, KrF excimer lasers, and ArF excimer lasers can be used. Exposure equipment such as steppers and scanners can be used.

[0034] (c) Step of removing the unexposed portion with a developer The developer used for removing the unexposed portion can be arbitrarily determined according to the type of photoresist to be used. For example, an aqueous alkaline developer (e.g., an aqueous alkali hydroxide solution, an aqueous organic alkali solution such as tetramethylammonium hydroxide, etc.), or an organic solvent-based developer (a combination of an organic solvent and a weak alkali or weak acid) can be used. An aqueous alkaline developer or an organic solvent-based developer can be used for the negative photoresist, the lift-off negative photoresist, and the film-shaped negative photoresist described above. In addition, an aqueous alkaline developer can be suitably used for the above-described crosslinkable positive photoresist.

[0035] The step of removing the unexposed portion with a developer includes immersing the silicon substrate on which the resist layer is formed in the developer for development, and / or spraying the developer onto the resist layer. After development, washing with a rinse solution may be included.

[0036] After the step (c), the resist layer formed on the silicon substrate may be subjected to heat treatment (post-baking) in order to make the pattern formed by development more robust.

[0037] The formation of a resist layer having a predetermined pattern, including the above steps (a) to (c) and optionally post-baking, has been described by taking as an example a method of previously forming a resist layer on a substrate for forming a resist layer such as a silicon substrate (referred to as "silicon substrate" for convenience of description). However, the disclosure content regarding the steps (a) to (c) and post-baking described above can be similarly applied to a method in which a substrate for forming a resist layer such as a silicon substrate is laminated on a metal electrode or a metalloid electrode (preferably laminated via a layer containing a conductive adhesive) to prepare a conductive substrate composed of silicon substrate / (preferably a layer containing a conductive adhesive) / metal electrode or metalloid electrode, and then a resist layer having a predetermined pattern is formed on the substrate for forming a resist layer.

[0038] (1-3) Predetermined Pattern The predetermined pattern possessed by the above-mentioned resist layer can be realized by the fine pattern drawn on the photomask used in the step of exposing the resist film. The pattern of the resist layer preferably has a shape with a sharp tip. When the microstructure obtained by the production method of the present invention is used as an artificial spicule, a shape with a sharp tip facilitates subcutaneous puncture.

[0039] Furthermore, the pattern of the resist layer is preferably a triangular shape, polygonal shape, star shape, elongated needle shape (for example, a sword-like shape), or a combination thereof. These shapes have sharp tips and facilitate subcutaneous puncture when used as artificial spicules.

[0040] In the pattern of the resist layer, it is preferable to design the side lengths of the above-mentioned shapes (that is, triangular shape, polygonal shape, star shape, elongated needle shape (for example, a sword-like shape), or a combination thereof) such that the side lengths of the obtained microstructure are 20 μm to 1000 μm. When the side lengths of the obtained microstructure fall within this range, the microstructure has a sufficient length to pierce the skin and provide skin irritation to an extent that allows the magnesium effect within the skin to be obtained.

[0041] In the pattern of the resist layer, it is preferable to design the pattern size (height or depth) such that the thickness of the obtained microstructure is 10 to 50 μm. When the thickness of the obtained microstructure falls within this range, even if the microstructure pierces the skin, the thickness is such that only slight pain is caused. The height or depth of the pattern and the pattern size corresponding to the side lengths of the above-mentioned microstructure can be determined by measurement using an electron microscope (SEM).

[0042] (2) Step (2) The production method of the present invention includes, as step (2), a step of forming a microstructure containing metallic magnesium inside the pattern on the conductive substrate by an electrolytic deposition method (electroplating).

[0043] (2-1) Electrolytic Plating Method The manufacturing method of the present invention is important in that it uses electrolytic plating, or more specifically electroplating, to form microstructures containing metallic magnesium inside the pattern on a conductive substrate.

[0044] Electroplating is a plating method that uses electric current. Generally, it involves reducing a substance (such as metal) from a solution, molten salt, or solid electrolyte containing the substance to be plated, thereby forming a thin layer of that substance on an electrically conductive object. Electroplating also includes techniques where the substance to be plated is used as the anode. In this technique, the anode is immersed in an electrolyte, and an electric current is supplied to the anode, oxidizing the metal atoms forming the anode and causing them to dissolve into the electrolyte. At the cathode, the metal ions dissolved in the electrolyte are reduced at the interface between the electrolyte and the cathode, resulting in plating on the cathode surface. In the manufacturing method of the present invention, either the former or the latter method can be used, but the latter method, namely using magnesium as the anode and a metal or metalloid electrode as the cathode as detailed in step (1), is preferred. Using a metal with higher electrical conductivity and superior stability (for example, copper or platinum, as described later) as the cathode than the metal (magnesium) used as the anode improves the controllability of the plating process.

[0045] Figure 1 shows a schematic diagram of a non-limiting example of an electroplating apparatus that can be used in the manufacturing method of the present invention. In Figure 1, magnesium (Mg) is used as the anode, and copper (Cu) is used as the metal electrode of a conductive substrate for the cathode.

[0046] Here, as the metal or metalloid electrode of the conductive substrate used as the cathode, it is preferable to use at least one metal or metalloid electrode selected from the group consisting of copper, stainless steel, graphite, molybdenum, titanium, platinum, nickel, and magnesium, as described in step (1).

[0047] In Figure 1, a silicon (Si) substrate is laminated on one side of a Cu metal electrode as the conductive substrate of the cathode, preferably laminated (or bonded) via a layer containing a conductive adhesive.

[0048] In the manufacturing method of the present invention, an anode (preferably magnesium) and a cathode are immersed in an electrolytic cell, and an electric current is supplied to the anode to perform electroplating.

[0049] The electrolytic cell contains an electrolyte, and the electrolyte used in the manufacturing method of the present invention preferably contains a magnesium salt or a magnesium-containing compound (for example, PhMgCl). Furthermore, it is desirable to use an organic solvent (tetrahydrofuran) or a non-aqueous solvent (1,2-dimethoxyethane) as the solvent for the electrolyte.

[0050] Furthermore, the electrolyte may contain metal salts such as zinc or aluminum. Non-limiting examples of the electrolyte include the above-mentioned organic solvent (such as tetrahydrofuran) or non-aqueous solvent (such as 1,2-dimethoxyethane) containing magnesium salts or compounds containing magnesium (e.g., PhMgCl), metal salts such as zinc or aluminum (e.g., AlCl 3 The electrolyte also contains any components (e.g., surfactants, buffers, brighteners, etc.) that can be used in the process of forming a plating on a conductive substrate (preferably a metal electrode or semimetallic electrode having a silicon substrate on at least one surface), to the extent that the effects of the present invention are not impaired.

[0051] In the manufacturing method of the present invention, the current density is typically 1 to 100 mA / cm². 2 The range is preferably 30 to 60 mA / cm². 2 This is within the specified range. When the current density is within the above range, it is possible to obtain a microstructure containing Mg with sufficient thickness and suppressed increase in surface roughness, resulting in good shape stability of the obtained microstructure.

[0052] In the manufacturing method of the present invention, the electrolysis time is preferably 15 minutes to 1 hour, and more preferably 20 minutes to 40 minutes. By performing electroplating within the above range of electrolysis time, the shape stability of the Mg-containing microstructure is improved.

[0053] In the manufacturing method of the present invention, a resist layer having a predetermined pattern is provided on a conductive substrate, so that a microstructure containing metallic magnesium can be formed inside the pattern. Furthermore, in the manufacturing method of the present invention, preferably, a microstructure containing magnesium can be formed with a size and shape corresponding to the predetermined pattern of the resist layer.

[0054] In the manufacturing method of the present invention, preferably, the resulting microstructure is a particulate microneedle. Until now, the only methods available for obtaining particulate microneedles as a microstructure containing metallic magnesium were individual laser processing, which were not suitable for mass production. Furthermore, since cutting was the basic processing method, there were problems with the lack of dimensional control and high precision. In the manufacturing method of the present invention, the bottom-up type allows for greater freedom in shape design according to the shape of the mold (a predetermined pattern formed by photolithography). In addition, since the manufacturing method of the present invention can form particulate needles with a similar pattern across the surface of the substrate, it can provide a processing method suitable for mass production. Thus, the manufacturing method of the present invention makes it possible to stably manufacture particulate microneedles as a microstructure containing metallic magnesium with high dimensional precision.

[0055] After forming microstructures containing metallic magnesium within a pattern, they can be recovered by physically peeling them directly from the pattern. However, to recover the microstructures stably without damaging their fine, pointed shapes, it is desirable to pre-prepare a sacrificial layer beneath the resist layer and recover them by etching only the sacrificial layer. By etching only the sacrificial layer in this way, the thin resist film above it and the metallic magnesium-containing microstructures can be floated and recovered, enabling industrially stable recovery of the microstructures while maintaining and controlling their fine, pointed shapes. A metal layer is preferred as the sacrificial layer, such as aluminum (Al) or copper (Cu) metal layers. For etching, an etching solution (e.g., acid-based, chloride-based, etc.) can be selected according to the type of metal in the sacrificial layer. For example, if the sacrificial layer is an aluminum-based metal layer, wet etching with an acid-based mixed acid can be performed; if it is a copper-based (Cu) metal layer, wet etching with a chloride-based solution, ammonia-based solution, etc., can be performed.

[0056] (3) Microstructures obtained by the manufacturing method of the present invention Another aspect of the present invention is a microstructure obtained by the manufacturing method of the present invention (hereinafter also referred to as "microstructure of the present invention"). One preferred aspect of the microstructure of the present invention is a particulate microneedle. The particulate microneedle of the present invention has the characteristic of having controlled dimensions and high dimensional accuracy. Furthermore, the microstructure obtained by the manufacturing method of the present invention has a specific shape and dimensions that make it easy to puncture subcutaneously, and can therefore be suitably used as an artificial spicule.

[0057] Another aspect of the present invention is a cosmetic composition containing a microstructure obtained by the manufacturing method of the present invention (the microstructure of the present invention) (hereinafter also referred to as "the cosmetic composition of the present invention").

[0058] The content of the microstructure of the present invention is not particularly limited, but preferably it can be 0.1 to 5 parts by weight based on 100 parts by weight of the cosmetic composition. The above composition can best exhibit the transdermal absorption rate and skin exfoliation effect.

[0059] The skin-improving active ingredients contained in the cosmetic composition may include ingredients that improve or enhance skin function, ingredients that suppress deterioration of skin condition, or ingredients that complement the shortcomings of the skin or highlight its advantages. The content of the active ingredients is not particularly limited, but is preferably 0.05 to 1 part by weight based on 100 parts by weight of the cosmetic composition. In addition to the active ingredients, the cosmetic composition of the present invention may also contain various ingredients that are normally found in cosmetic compositions. For example, it may contain all substances that are normally used in mask sheets, such as all dispersants, thickeners, surfactants, preservatives, humectants, stabilizers, solubilizers, pigments, and fragrances.

[0060] In one aspect of the cosmetic composition of the present invention, the cosmetic composition may have a skin exfoliating effect.

[0061] In one aspect of the cosmetic composition of the present invention, the cosmetic composition may have a wrinkle-improving effect.

[0062] The cosmetic composition of the present invention may further contain purified water, antioxidants, stabilizers, pigments, or fragrances that are commonly used in the field of cosmetic compositions.

[0063] Furthermore, the cosmetic compositions of the present invention can be manufactured in conventional dosage forms. Specifically, they can be manufactured in dosage forms including lotions (skin lotions), skin soaps, skin toners, astringents, lotions, milk lotions, moisturizing lotions, nourishing lotions, massage creams, nourishing creams, moisturizing creams, eye creams, hand creams, foundations, essences, nourishing essences, eye essences, packs, soaps, cleansing foams, cleansing lotions, cleansing creams, body lotions, body creams, body cleansers, suspensions, gels, powders, pastes, mask packs or sheets, or aerosol compositions. They can also be applied as various phases suitable for providing a moisturizing sensation to the skin, such as gels or creams, pastes, or solid phases, and can specifically be gel-creams with a particulate texture like sherbet or slush. Compositions in such dosage forms can be manufactured by methods conventional in the art.

[0064] The cosmetic composition of the present invention may further contain, for example, one or more selected from the group consisting of oils, purified water, emulsifiers, dispersants, pigments, fragrances, UV-blocking agents, sweeteners, vitamins, and metal ion chelating agents. Furthermore, the cosmetic composition of the present invention may further contain, for example, 0.1% to 3.0% by weight of a preservative.

[0065] The amount of additional components such as the aforementioned oils can be appropriately selected by those skilled in the art within a range that does not impair the purpose and effects of the present invention.

[0066] The cosmetic composition of the present invention may preferably be in the form of a cream.

[0067] The cosmetic composition of the present invention may further contain any common cosmetic ingredients selected from additional ingredients commonly used in cosmetics, such as dispersants, thickeners, pigments, fragrances, fillers, preservatives, antimicrobials, neutralizing agents, UV blockers, sweeteners, vitamins, free radical scavengers, metal ion chelating agents, and mixtures thereof.

[0068] 2. Microstructure containing metallic magnesium Another embodiment of the present invention is a microstructure containing metallic magnesium, wherein the microstructure has a pointed shape (hereinafter also referred to as "microstructure 1 of the present invention").

[0069] The microstructure 1 of the present invention can be suitably manufactured by the manufacturing method of the present invention described in detail in the preceding paragraph.

[0070] One preferred embodiment of the microstructure 1 of the present invention is a particulate microneedle. The particulate microneedle of the present invention has the characteristics of controlled dimensions and high dimensional accuracy. The microstructure 1 of the present invention contains biocompatible metallic magnesium, has a shape that facilitates subcutaneous puncture, and can be suitably used as an artificial spicule.

[0071] The microstructure 1 of the present invention preferably has a triangular shape, a polygonal shape, a star shape, an elongated needle shape (for example, a sword shape), or a combination thereof.

[0072] The microstructure 1 of the present invention preferably has a side length of 20 μm to 1000 μm in the above-described shape (i.e., triangular, polygonal, star-shaped, elongated needle-shaped (e.g., sword-like shape), or a combination thereof). This range is sufficient to allow the particulate needles to penetrate the skin and provide skin stimulation to the extent that a magnesium effect can be obtained within the skin.

[0073] The microstructure 1 of the present invention preferably has a thickness of 10 to 50 μm. This thickness range is such that even if it penetrates the skin, it will only cause minor pain. The height or depth of the microstructure 1 and the length of the sides of the microstructure 1 can be determined by measuring with an electron microscope (SEM).

[0074] Another preferred embodiment of the present invention is a cosmetic composition comprising the microstructure 1 of the present invention. Details of the cosmetic composition comprising the microstructure 1 of the present invention are as described in detail in the preceding paragraph.

[0075] The present invention will be described below with reference to examples, but the scope of the present invention is not limited to these examples.

[0076] The objective of this research is to fabricate particulate microneedles to improve drug penetration efficiency into the skin, and to develop and verify a novel processing method for Mg particulate microneedles with controllable shape and dimensions using electroplating. Therefore, the development of a stable processing process for Mg of specific shapes and the evaluation of Mg processed products are required. In addition, the initial target processed shapes were set to be a triangle with a pointed tip and a star shape.

[0077] 1. Plating Process (1) Overview of the Process and Equipment Configuration Diagram 1 shows the basic configuration of the processing equipment used in this study. Magnesium (Mg) was used as the anode and copper (Cu) as the cathode. Furthermore, in order to process the Mg into a specific shape, a silicon (Si) substrate having a specific pattern was bonded to the Cu electrode using a conductive adhesive (D-550, Dotite). The processing method for the Si substrate will be described in detail in Example 1.

[0078] (2) Reaction principle of plating process In the processing process described above, the flow of electric current causes Mg to be oxidized at the anode and become Mg ions. Then, by appropriately controlling the current density, the Mg ions are reduced at the cathode, and at that time, Mg is generated and grown on the Si substrate.

[0079] [Example 1] (1) Fabrication of artificial magnesium spicules (1-1) Experimental overview As described above, this study aims to plate Mg of a specific shape on a Si substrate fixed on a Cu electrode. For this reason, in this study, a pre-designed pattern was fabricated on a Si wafer using photolithography. Through this process, Mg is plated only inside the fabricated pattern, thereby producing Mg spicules with a specific shape.

[0080] (1-2) As design patterns, two types of patterns, triangular and hexagonal, were designed to investigate the effect of different patterns on Mg generation. The triangular and hexagonal patterns were designed with side lengths ranging from 20 μm to 200 μm (Figure 2).

[0081] (1-3) Photolithography Next, a photoresist is applied to the Si substrate and a pattern is formed by photolithography. In this study, a negative resist SU-8 (SU-8 3025, Kayaku Advanced Materials, Inc.) was used, in which the areas exposed to light harden and the unexposed areas are removed. SU-8 was adopted as a mold material in the initial stage of optimizing processing conditions due to its chemical insolubility in solvents and excellent adaptability in lithography. SU-8 was spin-coated (Mikasa Corporation, spin coater, 1H-D7) to produce a 20 μm thick SU-8 thin film. This thickness is set as a thickness index for Mg generation. Figure 2 shows two examples of patterns fabricated by photolithography (Union Corporation, double-sided mask aligner, PEM800).

[0082] (1-4) Electrode Design and Assembly The overall dimensions of the Cu (500 μm thick) electrode and Mg electrode (50 μm thick) were 40 mm in length and 4 mm in width, respectively. The pattern substrate was cut to approximately 15 × 4 mm and fixed to the Cu electrode using conductive adhesive. A block made of polytetrafluoroethylene (PTFE) was fabricated to maintain the spacing between the electrodes, and the electrodes were fixed as shown in Figure 3. THF was used as the electrolyte solvent, and AlCl 3 After dissolving, PhMgCl is added dropwise, and finally, PhMgCl:AlCl 3 0.4 M APC / THF was used, mixed to achieve a composition of 2:1.

[0083] (1-5) Experimental environment and analysis method The plating was performed in a glove box filled with argon gas to prevent the magnesium material from coming into contact with oxygen and moisture. Each electrode was connected to a constant current power supply device (HZ5000, Hokuto Denko Corporation) through a conducting wire, and plating was performed while precisely controlling the current density. The plating results were observed with an optical microscope (VH-5500, Keyence Co.) and an electron microscope (SEM, JSM-6510LV, JEOL Ltd.). In the SEM observation, the formation state of Mg was observed under the conditions of an acceleration voltage of 15 kV and a working distance of 10 mm. Furthermore, elemental analysis of the plated portion was performed using energy dispersive X-ray spectroscopy (EDS).

[0084] (2) Evaluation of magnesium artificial spicules First, plating was performed for 10 minutes (a) and 30 minutes (b) using a silicon substrate without a pattern to confirm Mg formation. The sample and current density conditions are shown in Figure 4, and the results of the respective optical microscope, SEM, and EDS elemental analysis are shown in Figure 5.

[0085] From these results, it was confirmed that Mg can be formed on the Si surface by the plating process. Next, using a sample with a hexagonal pattern, the current density was set to 30 mA / cm with reference to previous research 2 (c) and 90 mA / cm 2 (d), and plating was performed for 30 minutes to investigate the effect of different current densities on Mg formation. The sample and current density conditions are shown in Figure 6, and the results of the respective optical microscope, SEM, and EDS elemental analysis are shown in Figure 7.

[0086] At the current densities of 30 mA / cm 2 and 90 mA / cm 2 , it was confirmed that Mg was uniformly formed within the pattern. In particular, at the current density of 30 mA / cm 2 , Mg was thinly formed only at the bottom of the pattern, whereas at the current density of 90 mA / cm 2 , it was observed that Mg was also formed outside the pattern. Then, in order to investigate the effect of different current densities on Mg formation in more detail, the thickness of each formed Mg was confirmed using cross-sectional SEM photographs. The results are shown in Figure 8.

[0087] 30 mA / cm 2 When plating was performed for 30 minutes at a current density of 90 mA / cm², the thickness of the generated Mg was approximately 10 μm. 2 Approximately 20 μm of Mg was produced. Furthermore, the coarseness of the obtained Mg was consistent with the trend in previous studies where coarser material increased with increasing current density (O. Mizrah et al., “Electrolyte solutions with a wide electrochemical window for rechargeable magnesium batteries,” Journal of The Electrochemical Society, vol. 155, no. 2, pp. A103-A109, Feb. 2008). Based on the above manufacturing results, 60 mA / cm 2 Plating was performed for 30 minutes at the specified current density. The results are shown in Figure 9.

[0088] From these results, we can see that 60 mA / cm² 2 Under the specified current density conditions, the formation of Mg artificial spicules with a thickness of approximately 20 μm was confirmed for 30 minutes.

[0089] This study established the design and setup of electroplating experiments for magnesium microstructures, and the basic fabrication process for Mg artificial spicules using photoresist patterns. Subsequently, plating was performed only within specific patterns, and the effects of current density and electrolysis time on Mg growth were evaluated. From the experimental results, 60 mA / cm² was found to be the optimal current density. 2 It was confirmed that a Mg layer of approximately 20 μm was formed at the given current density. Furthermore, a tendency for the roughness of the Mg surface to increase with increasing current density was observed, confirming that appropriate control of current density and electrolysis time plays an important role in shape stability. Since the phenomenon of Mg overflowing outside the pattern was observed at excessively high current densities, uniform Mg plating within the pattern was achieved by adjusting the current density in stages. These results identify important parameters in the shape control of Mg artificial spicules and will serve as a basis for future process optimization.

Claims

1. A method for manufacturing a microstructure containing metallic magnesium, comprising: (1) a step of providing a resist layer having a predetermined pattern formed by photolithography on a conductive substrate; and (2) a step of forming a microstructure containing metallic magnesium inside the pattern on the conductive substrate by electrolytic deposition.

2. The manufacturing method according to claim 1, wherein the conductive substrate is a metal electrode or metalloid electrode having a silicon substrate on at least one surface.

3. The manufacturing method according to claim 2, wherein magnesium is used as the anode and the metal electrode or semimetallic electrode is used as the cathode.

4. The manufacturing method according to claim 3, wherein the metal electrode or metalloid electrode is an electrode of at least one metal selected from the group consisting of copper, stainless steel, graphite, molybdenum, titanium, platinum, nickel, and magnesium.

5. The manufacturing method according to claim 4, wherein the conductive substrate comprises a metal or semimetallic electrode, a layer containing a conductive adhesive provided on at least one surface of the electrode, and a silicon substrate provided on the layer containing the conductive adhesive.

6. The manufacturing method according to claim 1, wherein the resist layer is a negative resist layer, a lift-off negative resist layer, a film-like negative resist layer, or a crosslinkable positive resist layer.

7. The manufacturing method according to claim 1, comprising forming a magnesium-containing microstructure having a size and shape corresponding to the pattern.

8. The manufacturing method according to claim 1, wherein the pattern has a pointed shape.

9. The manufacturing method according to claim 8, wherein the pattern is triangular, polygonal, star-shaped, elongated needle-shaped (for example, a sword-like shape), or a combination thereof.

10. 1-100mA / cm 2 range (preferably 30 to 60 mA / cm²) 2 The manufacturing method according to claim 1, wherein electroplating is performed at a current density of ).

11. 30-60mA / cm 2 The manufacturing method according to claim 10, wherein electroplating is performed at a current density within the range of .

12. The manufacturing method according to claim 1, wherein the microstructure is a particulate microneedle.

13. A microstructure obtained by the manufacturing method described in any one of claims 1 to 12.

14. The microstructure according to claim 13, which is used as an artificial spicule.

15. A cosmetic composition comprising a microstructure obtained by the manufacturing method described in any one of claims 1 to 12.

16. A microstructure containing metallic magnesium, wherein the microstructure has a pointed shape.

17. The microstructure according to claim 16, wherein the shape is triangular, polygonal, star-shaped, elongated needle-shaped (for example, a sword-like shape), or a combination thereof.

18. The microstructure according to claim 17, wherein the side length in the shape is 20 μm to 1000 μm.

19. The microstructure according to claim 17, wherein the thickness is 10 to 50 μm.

20. The microstructure according to claim 16, which is used as an artificial spicule.