Glass passivated surface mount diode and manufacturing method thereof
By using an electrode sheet connected to an N-type single crystal silicon wafer with a thickness of 200~350μm and a steamed aluminum layer, combined with a glass slurry packaging, the problem of large external size of the existing diode is solved, and a smaller and thinner diode shape is achieved. The effect of reducing costs is suitable for miniaturization of electronic systems.
Patent Information
- Application Number
- CN202011060720.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-30
AI Technical Summary
The existing glass passivation surface-packaged diodes have a large appearance size, which is difficult to meet the needs of miniaturization, ultra-thinization and lightweighting of electronic systems.
The N-type single crystal silicon wafer with a thickness of 200~350μm is used as the core, and is connected to the electrode sheet through a vaporized aluminum layer. The electrode sheet extends radially in the die-cast glass and is shaped outside the passivation glass, combined with the glass slurry packaging to achieve Smaller, thinner diode profile.
A smaller and thinner diode profile is achieved, reducing manufacturing costs, and different package profiles can be manufactured as needed to meet the size requirements of the electronic system.
Smart Images

Figure CN112186043B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a glass passivated surface-mount diode and a manufacturing method thereof, belonging to the technical field of diodes. Background Art
[0002] As electronic systems develop towards miniaturization, ultra-thinness and lightness, the demand for miniaturized SMD devices is increasing. Although plastic-encapsulated SMD devices meet the size requirements, they are limited by the inherent characteristics of plastic encapsulation, are prone to moisture absorption and delamination, and have low reliability, so they can only be used in the mid- and low-end civilian markets. Glass-passivated solid-package diodes are widely used in mid- and high-end fields due to their high-temperature stability, strong radiation resistance, high reliability and low cost.
[0003] The Chinese patent document with publication number CN108172514A discloses a method for manufacturing a glass-passivated surface-mount packaged transient voltage suppressor diode, comprising the following steps: (1) obtaining chips of specified size by splitting a silicon wafer with a diffusion-evaporated metallization layer; (2) bonding the electrode lead to the chip by solder fusion welding; (3) coating the surface of the product with passivated packaging glass slurry after etching, cleaning, and passivation of the electrode assembly, and forming the product at high temperature in a chain manner to complete the packaging molding; (4) welding the axial product and the electrode sheet at high temperature by special solder, and realizing glass-passivated surface-mount packaging after cutting off the lead. The U-shaped glass-passivated surface-mount packaging is easier to install than the traditional axial device.
[0004] However, the electrode leads in the diode extend along the axial direction of the chip, and the diode has a large outer dimension, which makes it difficult to meet the requirements of miniaturization, ultra-thinness and lightness of electronic systems. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a glass passivated surface mount diode and a manufacturing method thereof.
[0006] The present invention is achieved through the following technical solutions:
[0007] A glass passivated surface-mount diode comprises a tube core and two electrode sheets, wherein the tube core is located between the two electrode sheets, the electrode sheet is connected to the tube core via an aluminum vaporization layer, the tube core, the two electrode sheets and the aluminum vaporization layer are all encapsulated in a passivation glass, and an end of the electrode sheet away from the tube core extends radially along the tube core to the outside of the passivation glass.
[0008] The tube core is made of an N-type single crystal silicon wafer with a thickness of 200-350 μm, and the tube core is located at the center of the passivation glass.
[0009] The thickness of the aluminum vaporization layer is 6-16 μm.
[0010] The electrode sheet is a molybdenum sheet.
[0011] One end of the two electrode sheets away from the tube core passes through the left and right sides of the passivation glass respectively.
[0012] The middle part of the electrode sheet is bent toward the tube core, and after being flush with the tube core, it passes through the passivation glass in the radial direction of the tube core. The end of the electrode sheet outside the passivation glass is first bent downward, then bent toward the center of the passivation glass, and rests against the bottom of the passivation glass.
[0013] The upper part and the lower part of the passivation glass are both in a trapezoidal structure.
[0014] A method for manufacturing a glass passivated surface mount diode comprises the following steps:
[0015] Step 1: Single crystal wafer: Select N-type single crystal silicon wafer with resistivity of 0.003Ω·cm~500Ω·cm.
[0016] Step 2: Phosphorus-boron diffusion: Phosphorus and boron are diffused on N-type single crystal silicon wafers to form a P+NN+ chip structure. The diffusion temperature is 1100~1280℃, the diffusion time is 5~50h, the phosphorus junction depth is 10~80μm, and the sheet resistance is ≤3Ω / □. The boron junction depth is 10~80μm, and the sheet resistance is ≤5Ω / □.
[0017] Step 3: Sandblasting: Use compressed air to carry diamond sand to remove the borosilicate glass layer formed on the boron diffusion surface.
[0018] Step 4: Aluminum evaporation: Aluminum is evaporated on the phosphorus and boron diffusion surfaces of the chip to form an aluminum vapor layer, and then it is placed in a vacuum sintering furnace to weld the chip and the aluminum vapor layer together. The welding temperature is 450-550°C and the constant temperature time is 5-20 minutes.
[0019] Step 5: Splitting: Use ultrasonic cutting to split the chip into the required die size, use a solution with a volume ratio of HF:HNO3=1:5 to corrode and clean the chip, then rinse with deionized water, dehydrate with alcohol and dry.
[0020] Step 6: Mold loading and sintering: stack the electrode sheet, tube core, and electrode sheet from bottom to top in the sintering mold, send the sintering mold into a vacuum sintering furnace for fusion welding and bonding. The fusion welding and bonding temperature is 660~700℃, and the constant temperature time is 2~5min. Cool to below 100℃ and take out the diode.
[0021] Step 7: Countertop corrosion: Use a KOH solution with a concentration of 2-12% and a temperature of 80-100°C to corrode the diode after fusion welding for 2-25 minutes. Rinse the corroded diode with hot deionized water and boil the diode in hot deionized water for 5 times. Then put the diode in a passivation solution at 55-60°C for 1-10 minutes.
[0022] Step 8, encapsulating glass powder: add high-purity paraffin wax to the glass powder, prepare glass powder slurry according to the ratio of glass powder: water = 3g: 1ml, and stir evenly when the paraffin wax is molten, put the diode into the casting mold, inject the glass powder slurry into the casting mold, scrape off the excess glass powder slurry, demould after the glass powder slurry cools down and solidifies, and then put the diode encapsulated with glass powder slurry into a vacuum sintering furnace for dewaxing;
[0023] Step 9, high temperature molding: put the diode encapsulated with glass powder slurry into a high temperature molding furnace for glass powder vitrification, the heating time is 45~65 minutes, the highest sintering temperature is 660℃, and it is maintained for 2~15 minutes;
[0024] Step 10: Shaping: Shape the electrode sheet outside the passivation glass into a desired shape to obtain a glass passivated surface mount diode.
[0025] In the step eight, 10% to 20% of high-purity paraffin is added to the glass powder.
[0026] In the step eight, dewaxing is performed at 150° C. for 1 to 2 hours, and then dewaxing is performed at 500° C. for 0.2 to 0.5 hours.
[0027] The beneficial effects of the present invention are:
[0028] 1. The lead-out electrode of the diode is a molybdenum sheet with a thickness of 0.1mm~0.2mm, and the lead-out electrode size is smaller.
[0029] 2. The lead-out electrode of the diode extends radially along the tube core. When the size of the tube core increases, only the pad size of the molybdenum sheet needs to be increased, and the thickness of the diode will not increase. A surface-mount device with small size and very thin thickness can be manufactured.
[0030] 3. Place the diode after the mesa is etched into a casting mold, and then inject glass powder slurry into the casting mold to coat the glass slurry. Different packaging shapes can be manufactured as needed.
[0031] 4. The lead-out electrode of the diode is only a molybdenum sheet, which eliminates the welding process between the molybdenum column and the copper lead and reduces the manufacturing cost of the diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic structural diagram of a diode of the present invention;
[0033] Figure 2 It is a schematic diagram of the structure of the diode before shaping of the present invention;
[0034] Figure 3 It is a structural schematic diagram of the upper mold of the injection mold of the present invention;
[0035] Figure 4 for Figure 3 Schematic diagram of the cross-sectional structure along AA;
[0036] Figure 5 It is a structural schematic diagram of the lower mold of the injection mold of the present invention;
[0037] Figure 6 for Figure 5 Schematic diagram of the cross-sectional structure along BB;
[0038] Figure 7 It is a schematic diagram of the assembly structure of the diode and the injection mold when encapsulating the glass powder in the present invention.
[0039] In the figure: 1-tube core, 2-electrode sheet, 3-evaporated aluminum layer, 4-passivation glass. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0041] like Figures 1 to 7 As shown, a glass passivated surface-mount diode described in the present invention includes a tube core 1 and two electrode sheets 2, wherein the tube core 1 is located between the two electrode sheets 2, and the electrode sheet 2 is connected to the tube core 1 through a vaporized aluminum layer 3. The tube core 1, the two electrode sheets 2 and the vaporized aluminum layer 3 are all encapsulated in a passivation glass 4, and an end of the electrode sheet 2 away from the tube core 1 extends radially along the tube core 1 to the outside of the passivation glass 4.
[0042] The tube core 1 is made of an N-type single crystal silicon wafer with a thickness of 200-350 μm, and the tube core 1 is located at the center of the passivation glass 4 .
[0043] The thickness of the evaporated aluminum layer 3 is 6-16 μm.
[0044] The electrode sheet 2 is a molybdenum sheet.
[0045] One end of the two electrode sheets 2 away from the tube core 1 passes through the left and right sides of the passivation glass 4 respectively.
[0046] The middle part of the electrode sheet 2 is bent toward the direction close to the tube core 1, and after being flush with the tube core 1, it passes through the passivation glass 4 along the radial direction of the tube core 1. The end of the electrode sheet 2 located outside the passivation glass 4 is first bent downward, then bent toward the center of the passivation glass 4, and rests against the bottom of the passivation glass 4.
[0047] The upper and lower parts of the passivation glass 4 are both in a trapezoidal structure.
[0048] A method for manufacturing a glass passivated surface mount diode comprises the following steps:
[0049] Step 1: Single crystal wafer: Select an N-type single crystal silicon wafer with a resistivity of 0.003Ω·cm~500Ω·cm.
[0050] Step 2, phosphorus-boron diffusion: Phosphorus and boron are diffused on N-type single crystal silicon wafers to form a P+NN+ chip structure. The diffusion temperature is 1100~1280℃, the diffusion time is 5~50h, the phosphorus junction depth is 10~80μm, the sheet resistance is ≤3Ω / □, the boron junction depth is 10~80μm, and the sheet resistance is ≤5Ω / □.
[0051] Step 3: Sandblasting: Use compressed air to carry corundum to remove the borosilicate glass layer formed on the boron diffusion surface. When using, the specifications of corundum are 302# or 303#, and the compressed air pressure is ≤5 × 10 5 pa.
[0052] Step 4: Aluminum evaporation: Aluminum is evaporated on the phosphorus and boron diffusion surfaces of the chip to form an aluminum vapor layer 3, and then the chip is placed in a vacuum sintering furnace to weld and bond the chip and the aluminum vapor layer 3. The welding bonding temperature is 450-550°C and the constant temperature time is 5-20 minutes. When in use, the aluminum vapor layer 3 is formed on the phosphorus and boron diffusion surfaces of the chip by electron beam evaporation.
[0053] Step 5, splitting: Use ultrasonic cutting to split the chip into the required tube core 1 size, use a solution with a volume ratio of HF:HNO3=1:5 to corrode and clean the chip, then rinse with deionized water, dehydrate with alcohol and dry.
[0054] Step 6, molding and sintering: stack the electrode sheet 2, tube core 1, and electrode sheet 2 from bottom to top in the sintering mold, send the sintering mold into a vacuum sintering furnace for fusion welding and bonding, the fusion welding and bonding temperature is 660~700℃, the constant temperature time is 2~5min, and cool to below 100℃ to take out the diode.
[0055] Step 7: Countertop corrosion: Use a KOH solution with a concentration of 2-12% and a temperature of 80-100°C to corrode the fusion-bonded diode for 2-25 minutes. Rinse the corroded diode with hot deionized water and boil it in hot deionized water for 5 times. Then place the diode in a passivation solution at 55-60°C for 1-10 minutes.
[0056] Step 8, encapsulating glass powder: add high-purity paraffin wax to the glass powder, prepare glass powder slurry according to the ratio of glass powder: water = 3g: 1ml, and stir evenly when the paraffin wax is molten, put the diode into the casting mold, inject the glass powder slurry into the casting mold, scrape off the excess glass powder slurry, demould after the glass powder slurry cools down and solidifies, and then put the diode encapsulated with glass powder slurry into a vacuum sintering furnace for dewaxing;
[0057] Step 9, high temperature molding: put the diode encapsulated with glass powder slurry into a high temperature molding furnace for glass powder vitrification, the heating time is 45~65 minutes, the highest sintering temperature is 660℃, and it is maintained for 2~15 minutes;
[0058] Step 10: Shaping: Shaping the electrode sheet 2 outside the passivation glass 4 into a desired shape, thereby obtaining a glass-passivated surface-mount diode.
[0059] In the step eight, 10% to 20% of high-purity paraffin is added to the glass powder.
[0060] In the step eight, dewaxing is performed at 150° C. for 1 to 2 hours, and then dewaxing is performed at 500° C. for 0.2 to 0.5 hours.
[0061] The glass passivated surface mount diode provided by the present invention has the following effects compared with the traditional glass passivated solid package surface mount diode: 1. The lead-out electrode of the traditional glass passivated solid package surface mount diode is a molybdenum column, and the diameter of the molybdenum column is generally 1.5mm~5mm. The lead-out electrode of the diode provided by the present invention is a molybdenum sheet, and the thickness of the molybdenum sheet is 0.1mm~0.2mm, and the lead-out electrode size is smaller.
[0062] 2. The lead-out electrode of the traditional glass-passivated solid-package surface-mount diode extends along the axial direction of the tube core 1. The larger the tube core 1, the larger the thickness and diameter of the diode. The lead-out electrode of the diode provided by the present invention extends along the radial direction of the tube core 1 (the diameter is 0.15mm~0.3mm). When the size of the tube core 1 increases, it is only necessary to increase the pad size of the molybdenum sheet, and the thickness of the diode will not increase. Therefore, a surface-mount device with a small size and very thin thickness can be manufactured.
[0063] 3. In the conventional glass passivated solid package surface mount diode, the passivated glass is coated by mixing glass powder into glass paste and then coating it on the rotating tube core 1 and drying it. The glass paste shrinks into an ellipsoidal shape. After high temperature molding, only an ellipsoidal shape can be obtained, and the required external dimensions cannot be manufactured as required. The present invention adopts the method of placing the diode after the mesa is etched into a casting mold, and then injecting glass powder paste into the casting mold to coat the glass paste, so that different packaging external shapes can be manufactured as required.
[0064] 4. The lead-out electrode of the traditional glass passivated solid package surface-mount diode is a molybdenum column + copper lead. The lead-out electrode of the diode provided by the present invention only has a molybdenum sheet, which eliminates the welding process of the molybdenum column and the copper lead, thereby reducing the manufacturing cost of the diode.
[0065] The diode provided by the present invention can replace the DO-214 plastic surface mount package diode.
Claims
1. A method for manufacturing a glass passivated surface mount diode, Features: The glass passivated surface-mount diode comprises a tube core (1) and two electrode sheets (2), the tube core (1) is located between the two electrode sheets (2), the electrode sheet (2) is connected to the tube core (1) via a vaporized aluminum layer (3), the tube core (1), the two electrode sheets (2) and the vaporized aluminum layer (3) are all encapsulated in a passivation glass (4), and an end of the electrode sheet (2) away from the tube core (1) extends radially along the tube core (1) to the outside of the passivation glass (4); The manufacturing method of the glass passivated surface mount diode comprises the following steps: Step 1: Single crystal wafer: Select N-type single crystal silicon wafer with resistivity of 0.003Ω·cm ~500Ω·cm; Step 2, phosphorus-boron diffusion: Phosphorus and boron are diffused on N-type single crystal silicon wafers to form a P+NN+ chip structure. The diffusion temperature is 1100~1280℃, the diffusion time is 5~50h, the phosphorus junction depth is 10~80μm, the sheet resistance is ≤3Ω / □, and the boron junction depth is 10~80μm, the sheet resistance is ≤5Ω / □; Step 3: Sandblasting: Use compressed air to carry diamond sand to remove the borosilicate glass layer formed on the boron diffusion surface; Step 4, aluminum vaporization: Aluminum is vaporized on the phosphorus and boron diffusion surfaces of the chip to form an aluminum vaporization layer (3), and then the chip is placed in a vacuum sintering furnace to weld and bond the chip and the aluminum vaporization layer (3). The welding bonding temperature is 450-550° C. and the constant temperature time is 5-20 minutes. Step 5, chip splitting: Use ultrasonic cutting to split the chip into the required tube core (1) size, use a solution with a volume ratio of HF:HNO3=1:5 to corrode and clean the chip, then rinse with deionized water, dehydrate with alcohol and dry; Step 6: mold assembly and sintering: stack the electrode sheet (2), the tube core (1), and the electrode sheet (2) from bottom to top in a sintering mold, and send the sintering mold into a vacuum sintering furnace for fusion welding and bonding. The fusion welding and bonding temperature is 660-700°C, and the constant temperature time is 2-5 minutes. Cool to below 100°C and take out the diode; Step 7: Countertop corrosion: Use a KOH solution with a concentration of 2-12% and a temperature of 80-100°C to corrode the diode after fusion welding for 2-25 minutes, rinse the corroded diode with hot deionized water, boil the diode in hot deionized water for 5 times, and then put the diode in a passivation solution at 55-60°C for 1-10 minutes; Step 8, encapsulating glass powder: add high-purity paraffin wax to the glass powder, prepare glass powder slurry according to the ratio of glass powder: water = 3g: 1ml, and stir evenly when the paraffin wax is molten, put the diode into the casting mold, inject the glass powder slurry into the casting mold, scrape off the excess glass powder slurry, demould after the glass powder slurry cools down and solidifies, and then put the diode encapsulated with glass powder slurry into a vacuum sintering furnace for dewaxing; Step 9, high temperature molding: put the diode encapsulated with glass powder slurry into a high temperature molding furnace for glass powder vitrification, the heating time is 45~65 minutes, the highest sintering temperature is 660℃, and it is maintained for 2~15 minutes; Step 10: Shaping: Shaping the electrode sheet (2) outside the passivation glass (4) into a desired shape, thereby obtaining a glass passivation surface mount diode.
2. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: The tube core (1) is made of an N-type single crystal silicon wafer with a thickness of 200-350 μm; the tube core (1) is located at the center of the passivation glass (4).
3. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: The thickness of the evaporated aluminum layer (3) is 6 to 16 μm.
4. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: The electrode sheet (2) is a molybdenum sheet.
5. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: The ends of the two electrode sheets (2) that are away from the tube core (1) respectively pass through the left and right sides of the passivation glass (4).
6. The method for manufacturing a glass passivated surface mount diode according to claim 5, Features: The middle portion of the electrode sheet (2) is bent in a direction close to the tube core (1), and after being flush with the tube core (1), it passes through the passivation glass (4) in the radial direction of the tube core (1); the end of the electrode sheet (2) located outside the passivation glass (4) is first bent downward, then bent in a direction towards the center of the passivation glass (4), and abuts against the bottom of the passivation glass (4).
7. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: The upper part and the lower part of the passivation glass (4) both have a trapezoidal structure.
8. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: In the step eight, 10% to 20% of high-purity paraffin is added to the glass powder.
9. The method for manufacturing a glass passivated surface mount diode according to claim 1, Features: In the step eight, dewaxing is performed at 150° C. for 1 to 2 hours, and then dewaxing is performed at 500° C. for 0.2 to 0.5 hours.