A method for preparing a lost model shell and a casting by using a layered combustion method, and a mold shell
The layered combustion method promotes the slow combustion of foam patterns and prepares hollow shells, which solves the problems of carbon increase and hydrogen embrittlement caused by the gasification of foam patterns in the disappearing mold casting, and achieves the improvement of the quality of the castings and the improvement of production efficiency.
Patent Information
- Application Number
- CN202211484899.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-11-24
AI Technical Summary
In the disappearing mold casting technology, environmental pollution caused by bubble pattern gasification and casting pore defects, especially sensitive to non-ferrous metals and low-carbon alloy steel materials, which can easily lead to defects such as carbon increase and hydrogen embrittlement.
The layered combustion method is used to promote the slow combustion and decomposition of foam patterns by using small-molecular radius organic combustion aids, and prepare hollow shells to avoid the complete combustion of foam patterns before pouring, reducing the generation of gasification products.
Effectively eliminates the defects of carbon enhancement and hydrogen embrittlement of castings, improves the microstructure and mechanical properties of castings, is simple to operate, short cycle, is suitable for mass production, has low energy consumption, and is suitable for the preparation of castings with smaller wall thickness.
Smart Images

Figure CN115740364B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lost foam casting, and more specifically, relates to a method for preparing lost foam shells and castings by using a layered combustion method, and a mold shell. Background Art
[0002] The lost foam casting technology invented in 1971 is widely used by many foundries for its advantages of smooth casting surface, high dimensional accuracy, good formability of thin-walled complex castings, and almost no need for subsequent machining. However, there are still some urgent problems to be solved in the lost foam casting technology today: the pouring process is accompanied by the gasification of the foam pattern, which will cause environmental pollution; the probability of gas production during pouring will greatly increase the probability of porosity defects in castings; the lost foam foam pattern mainly gasifies and cracks to generate hydrocarbons, and non-ferrous metals, low-carbon alloy steels and other materials are very sensitive to them, which can easily lead to defects such as carbon increase and hydrogen embrittlement in castings, deteriorating the microstructure and mechanical properties of castings.
[0003] For example, the carbon increase effect caused by lost foam casting has been clearly mentioned in non-patent literatures such as "Research Status of Carbon Increase Defects in Lost Foam Casting Steel Parts", "Preliminary Study on the Surface Carbon Increase Law of Medium and Low Carbon Lost Foam Casting Steel Parts", and "Surface Carbon Increase of Lost Foam Casting Steel Parts". Therefore, how to avoid defects such as carbon increase and hydrogen embrittlement in castings is a technical problem that needs to be solved urgently. Summary of the invention
[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a method and shell for preparing a lost model shell and a casting by using a layered combustion method, the purpose of which is to use a small molecular radius organic combustion aid to promote the combustion of the foam pattern, and to use layer-by-layer combustion to slowly burn and decompose the foam pattern to obtain a hollow shell, thereby solving the technical problems of defects such as carbon increase and hydrogen embrittlement in castings.
[0005] To achieve the above object, according to one aspect of the present invention, a method for preparing an evaporative mold shell by using a layered combustion method is provided, the method comprising the following steps:
[0006] (1) coating the surface of the foam mold with a coating and then drying the mold to completely dehydrate the mold to obtain a casting mold;
[0007] (2) fixing the mold along the axis and rotating it, and pouring an organic combustion improver onto the surface of the mold from the pouring port of the mold, so that the organic combustion improver penetrates the mold wall and adheres to the foam surface;
[0008] (3) The mold is ignited from the pouring port, and the gaseous products of the combustion and decomposition of the foam inside the mold are discharged toward the pouring port. After the combustion is completed and the foam is completely burned, a lost foam hollow shell composed of refractory material is obtained.
[0009] It should be noted that the preparation process of the foam mold in the present invention is an existing mature technology. For example, the foam beads such as expandable polystyrene (EPS), expandable methyl methacrylate-styrene copolymer (STMMA), expandable polymethyl methacrylate resin (EPMMA) can be selected to prepare the foam pattern through the process of "pre-foaming-aging-foaming molding-cooling demolding-combined model cluster", cutting or high-precision machine tool processing. Preferably, the molecular radius of the organic combustion aid is smaller than the pore size of the casting mold; preferably, the organic combustion aid is at least one of anhydrous ethanol, methanol, ether or carbon disulfide.
[0010] Preferably, the volume ratio of the organic combustion aid to the foam sample is (2-7): (98-93).
[0011] Preferably, the pouring in step (2) is performed in layers starting from the gate position, with each pouring length being 5-10 mm, until pouring to the bottom of the mold.
[0012] In addition, in the present invention, the casting mold can be ignited from the pouring gate by pouring the organic combustion aid in layers and then igniting it, or by layered combustion, that is, the organic combustion aid can be poured again after a certain length of foam is burned out. This can make the shell preparation process stable and controllable, so that the combustion situation can be observed in real time, and a judgment can be made based on the actual situation, such as whether the combustion preparation is successful, whether the shell is damaged during the combustion process, whether the combustion is insufficient and whether the amount of organic combustion aid needs to be increased, etc.
[0013] Preferably, the pouring in step (2) is performed by using a needle or a nozzle.
[0014] Preferably, in the step (3), after the casting mold is ignited, when the unburned length is less than 2 mm, an organic combustion aid is poured into the unburned area again until the foam is completely burned.
[0015] Preferably, in step (3), an air pump is provided at the gate.
[0016] Preferably, in step (1) of the present invention, the surface of the foam mold is coated with a coating and then dried to completely dehydrate the mold. Specifically, the surface of the foam mold is coated with a special coating for lost foam casting 2-4 times, the working temperature of the drying box is set to 60-90°C, and the dried mold is placed in the oven for baking for 12-24 hours to completely dehydrate it to obtain a casting mold.
[0017] Preferably, the coating used in step (1) of the present invention is a mixture of special coating for lost foam casting and water in a mass ratio of (1-2): (2-1); the configuration process is: water is poured into a stirring vessel, the stirrer is turned on and special sand is slowly added (addition speed is: 400-600g / min), and the stirrer speed is increased (speed increase rate is: 20-40r / s), until the speed reaches 1500-1700 rpm, the speed increase is stopped and the speed is maintained, and the addition of special sand is completed, and then the original speed is maintained for 20-30 minutes, and finally the speed is reduced to 1100-1300 rpm and stirred for 360-480 minutes until the coating is uniformly paste-like. Among them, the special coating for lost foam casting is GLD model, purchased from Zhengzhou Hongjin Casting Materials Co., Ltd.
[0018] According to another aspect of the present invention, a vanishing pattern shell is provided.
[0019] According to another aspect of the present invention, there is provided a method for lost foam casting, the method comprising:
[0020] A lost model shell is prepared, and then the lost model shell is placed in a sand box, buried in dry quartz sand for vibration molding, and a casting is obtained by pouring molten metal under negative pressure.
[0021] According to yet another aspect of the present invention, a casting is provided.
[0022] In general, compared with the prior art, the above technical solution conceived by the present invention can at least achieve the following beneficial effects.
[0023] (1) The present invention utilizes an organic combustion aid to pour a foam pattern to promote its combustion to quickly prepare a hollow lost foam mold shell. The operation is simple, the cycle is short, and the hollow mold shell is of high quality. The components of the foam mold for lost foam casting are usually expandable polystyrene, expandable methyl methacrylate-styrene copolymer, expandable polymethyl methacrylate resin, etc., all of which are hydrocarbon organic substances. The combustion products are mainly CO2, CO, H2O, etc., and the high-temperature thermal decomposition and gasification products are mainly short-chain hydrocarbons, hydrocarbons containing benzene rings, carbon black, hydrogen, etc. The lost foam casting used in the prior art is usually to prepare a mold containing foam inside, then directly put the mold containing foam inside into a sand box, and pour the molten metal. When the molten metal is poured, the foam pattern burns and gasifies, and a large amount of gas products are rapidly generated, which will enter the molten metal along the surface of the molten metal, thereby causing carbon and hydrogen addition to the casting. The present invention has achieved the elimination of the foam mold before pouring, and the above-mentioned problem of foam mold combustion and gasification will no longer occur during the pouring process.
[0024] It can effectively eliminate defects such as carbon increase, hydrogen increase, pores, slag inclusions and uneven casting surface caused by the decomposition of polystyrene in the molten metal during traditional lost foam casting.
[0025] (2) Different from the existing method of high-temperature baking of foamed molds to soften and gasify the mold, the high-temperature baking method takes a long time to prepare the shell, which is not convenient for mass production; the baking temperature is strict and the energy consumption is high; limited by the baking method, the baked mold should not be too large, and only small mold parts can be prepared. The combustion method of the present invention has a short production cycle, low energy consumption, and can prepare castings with relatively small wall thickness. After multiple combustions, large parts can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a structural diagram of a casting mold after a refractory coating is applied to the surface of a foam mold and dried according to an embodiment of the present invention;
[0027] Figure 2 is a front view of a hollow mold shell after the foam inside the mold is burned and vaporized according to an embodiment of the present invention;
[0028] Figure 3 It is a top view of the hollow shell after the foam inside the mold is partially burned and vaporized according to an embodiment of the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0030] Example:
[0031] This embodiment adopts the method for rapidly preparing the hollow shell of lost foam casting proposed by the present invention to prepare low carbon steel castings. Figure 1-3 , including the following steps:
[0032] Step 1, pattern preparation: polystyrene foam beads are selected to prepare a polystyrene foam pattern with a size of 35*35*100mm through "pre-foaming-aging-foaming molding-cooling and demolding-assembly model cluster";
[0033] Step 2, coating preparation: select the special coating for lost foam casting and mix it with pure water in a mass ratio of 1:1. The detailed process is as follows: Pour 500g of water into the stirring vessel, turn on the stirrer and slowly add the special sand (addition speed: 500g / min), and increase the stirrer speed (speed increase rate: 25r / s), until the speed reaches 1600 rpm, stop increasing the speed and maintain the speed, and the special sand addition is completed, then maintain the original speed for 30 minutes, and finally reduce the speed to 1200 rpm and stir for 480 minutes until the coating is uniform and paste-like;
[0034] Step 3, mold preparation: evenly apply the coating prepared in step 2 on the surface of the mold obtained in step 1 (except the gate position), the number of times of application is 3 times, and the mold should be dried or the surface coating should not fall off between each two applications, and then the working temperature of the drying box is set to 70°C, and the dried mold is placed in the oven for 12 hours to completely dehydrate it;
[0035] Step 4, combustion preparation: keep the mold obtained in step 3 rotating, and pour 10 ml of anhydrous ethanol from the mold gate to the bottom of the mold, with each pouring length of about 5-10 mm, so that the organic combustion aid penetrates into the mold shell wall and adheres to the polystyrene;
[0036] Step 5, burning mold: ignite the polystyrene attached with organic combustion aid to make it burn slowly, and the gas products of combustion decomposition are discharged to the gate through the interior of the shell. This process gradually advances to the interior of the shell, so that the internal polystyrene mold is completely eliminated, and finally only the hollow shell composed of refractory material remains.
[0037] Step 6, pouring: placing the hollow shell obtained in step 5 in a sand box, burying it in dry quartz sand for vibration molding, and pouring under negative pressure to obtain a casting.
[0038] Comparative Example:
[0039] This comparative example adopts the traditional lost foam casting method to prepare low carbon steel castings, including the following steps:
[0040] Step 1, pattern preparation: polystyrene foam beads are selected to prepare a polystyrene foam pattern with a size of 35*35*100mm through "pre-foaming - aging - foaming molding - cooling and demolding - combined model cluster";
[0041] Step 2, coating preparation: select the special coating for lost foam casting and mix it with pure water in a mass ratio of 1:1. The detailed process is as follows: Pour 500g of water into the stirring vessel, turn on the stirrer and slowly add the special sand (addition speed: 500g / min), and increase the stirrer speed (speed increase rate: 25r / s), until the speed reaches 1600 rpm, stop increasing the speed and maintain the speed, and the special sand addition is completed, then maintain the original speed for 30 minutes, and finally reduce the speed to 1200 rpm and stir for 480 minutes until the coating is uniform and paste-like;
[0042] Step 3, mold preparation: evenly apply the coating prepared in step 2 on the surface of the mold obtained in step 1 (except the gate position), the number of times of application is 3 times, and the mold should be dried or the surface coating should not fall off between each two applications, and then the working temperature of the drying box is set to 70°C, and the dried mold is placed in the oven for 12 hours to completely dehydrate it;
[0043] Step 4, pouring: placing the mold obtained in step 3 in a sand box, burying it in dry quartz sand for vibration molding, and pouring under negative pressure to obtain a casting.
[0044] The comparative example is a conventional lost foam casting method in the prior art. Since the casting mold containing foam inside is directly placed in a sand box for molten metal pouring, the foam mold burns and gasifies during the molten metal pouring, and a large amount of gas products are rapidly generated and enter the molten metal along the surface of the molten metal, thereby causing carbon and hydrogen addition to the casting. However, the present invention has eliminated the foam mold before pouring, and the problem of the above-mentioned foam mold burning and gasification will no longer occur during the pouring process. It can effectively eliminate the defects of carbon addition, hydrogen addition, pores, slag inclusions, and uneven casting surface caused by the decomposition of polystyrene and the like in the molten metal during traditional lost foam casting.
[0045] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an evaporative model shell by using a layered combustion method, characterized in that: The method comprises the following steps: (1) coating the surface of the foam mold and then drying it to completely dehydrate the mold to obtain a casting mold; (2) The mold is fixed along the axis and then rotated, and an organic combustion aid is poured onto the surface of the mold from the gate position, so that the organic combustion aid passes through the mold wall and adheres to the foam surface; the pouring is layered pouring from the gate position, and each pouring length is 5-10 mm until pouring to the bottom of the mold; the molecular radius of the organic combustion aid is smaller than the pore size of the mold; the volume ratio of the organic combustion aid to the foam pattern is (2 - 7): (98 - 93); (3) The mold is ignited from the pouring port, and the gaseous products of the foam combustion and decomposition inside the mold are discharged toward the pouring port. After the combustion is completed and the foam is completely burned, a lost foam hollow shell composed of refractory material is obtained.
2. The method according to claim 1, characterized in that The organic combustion improver is at least one of anhydrous ethanol, methanol, ether or carbon disulfide.
3. The method according to claim 1, characterized in that In the step (2), the pouring is performed by using a needle or a nozzle.
4. The method according to claim 1, characterized in that In the step (3), after the casting mold is ignited, when the unburned length is less than 2 mm, the organic combustion aid is poured onto the unburned area again until the foam is completely burned.
5. The method according to claim 1, characterized in that In the step (3), an air pump is provided at the gate.
6. A method for lost foam casting, characterized in that: The method comprises: The lost pattern shell is prepared by the method described in any one of claims 1 to 5, and then the lost pattern shell is placed in a sand box, buried in dry quartz sand for vibration molding, and molten metal is poured under negative pressure to obtain a casting.
Citation Information
Patent Citations
Method for preventing crush of lost foam casting product
CN101767186A
Molding method of casting mold
JP1995204779A