A novel method for preparing ultra-high performance concrete
By using irregularly shaped steel fiber units composed of open rings and extensions in ultra-high strength concrete, and combining them with a specific mixing process, the problem of uneven strength caused by uneven steel fiber mixing was solved, thereby improving the uniformity of concrete strength and load-bearing capacity.
Patent Information
- Application Number
- CN202211429976.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-15
AI Technical Summary
The problem of uneven strength caused by uneven mixing of steel fibers in existing ultra-high strength concrete is that there are large strength differences between different locations.
The steel fiber unit, consisting of an open ring and an extension, is used to ensure that the steel fiber forms a continuous structure in three-dimensional space by uniformly dispersing it in concrete and controlling the gas flow and vacuum exhaust during the mixing process.
It improves the uniformity of concrete strength and load-bearing capacity, reduces the problem of excessively high or low local strength, and enhances the overall performance of concrete.
Smart Images

Figure CN115847605B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete preparation, and in particular to a method for preparing a novel ultra-high performance concrete. Background Art
[0002] Concrete with strength grade above C100 is called ultra-high strength concrete. It is made of cement, sand, stone raw materials, water reducing agent or fly ash, F ore powder, slag, silica powder and other mixed materials, and produced by conventional process to obtain high-strength concrete.
[0003] In the prior art, fibers are usually added to ultra-high-strength concrete, among which steel fibers are a commonly used type of fiber. Steel fibers themselves have high toughness and strength, which can improve the strength performance of concrete. However, steel fibers are straight, curved or wavy. This type of fiber can only improve continuity in the direction of the fiber length, and multiple fibers are required to form a loose three-dimensional reinforcement structure in different directions to achieve effective reinforcement. This makes the reinforcement effect of steel fibers very dependent on the dispersed structural state in concrete, but this dispersed structural state is random and the effect stability is poor, especially for ultra-high-strength concrete. The proportions of each component are required to be very precise. When the steel fibers are unevenly dispersed, it is easy to cause a very large strength difference between different positions.
[0004] The Chinese patent with publication number CN 109912272 A discloses an ultra-high strength concrete and a thin-walled pole made of the ultra-high strength concrete. The concrete is prepared by the method of Example 1. 1000 kg of PO 52.5 ordinary Portland cement with a SiO2 content of 95% and a specific surface area of 20000 m 2 / kg silica fume 200kg, 4 mesh quartz sand 1200kg, wavy 30mm steel fiber 218kg are fully mixed in a concrete mixer; then add 223kg water and stir thoroughly for 30min; then add 18kg polycarboxylic acid water reducer with a water reduction rate of 40%, stir thoroughly until the mixture is uniform, and then get ultra-high strength concrete out of the tank. The test blocks made are 100 cubic millimeter test blocks, and the 28-day compressive strength reaches more than 122MPa. After trial production, 10 150 cubic millimeter test blocks were prepared, and the lowest 28-day compressive strength was only 79.8MPa, and the highest was 135.2MPa, and the strength was not uniform. Summary of the invention
[0005] Technical problem to be solved: In view of the problem of uneven strength caused by uneven mixing of steel fibers in the prior art, the present invention provides a novel method for preparing ultra-high performance concrete, which can achieve more uniform strength of ultra-high strength concrete.
[0006] Technical solution: A new method for preparing ultra-high performance concrete, including mixing cement, silica fume, aggregate, water, water reducing agent and steel fiber.
[0007] The steel fiber accounts for 1-2.5% of the total volume of the concrete by volume;
[0008] The steel fiber is composed of a plurality of steel fiber units, each of which includes an open ring and an extension portion connected thereto, wherein the extension portion extends from an open end of the open ring in a direction away from the open ring, and the extension length is not less than the inner diameter of the open ring;
[0009] Several steel fiber units are evenly dispersed in the new ultra-high performance concrete.
[0010] Preferably, each steel fiber unit comprises an open ring and one or two extensions connected thereto; when there is one extension, it is connected to any open end of the open ring; when there are two extensions, the two extensions extend in opposite directions.
[0011] Preferably, the open ring is a single ring formed by a steel wire or a spiral structure formed by at least two turns.
[0012] Preferably, when the open ring is a spiral structure formed by at least two turns of a steel wire, the diameters of the outermost circle and the innermost circle are different, and the diameter of the large diameter end is 1.5-3 times the diameter of the small diameter end.
[0013] Preferably, a ceramic tube is surrounded by the open ring, and the inner diameter of the ceramic tube is the average of the maximum diameter and the minimum diameter of the aggregate X±1mm.
[0014] Preferably, the surrounding method of the ceramic pipe is as follows:
[0015] Step 1. Heat the steel wire to 120-150℃;
[0016] Step 2. Fix the ceramic tube vertically, and wrap the steel wire obtained in step 1 around the ceramic tube. The portion of the steel wire around the ceramic tube forms an open ring, and the remaining portion is trimmed into an extension portion;
[0017] Step 3. Wait for the steel wire to cool and shrink naturally.
[0018] Preferably, when cement, silica fume, aggregate, water, water reducing agent and steel fiber are mixed, the specific steps are as follows:
[0019] Step 1. Pour the solid material into the mixing tank;
[0020] Step 2. Add water and other liquid components into the mixing tank;
[0021] Step 3. Seal the mixing tank and add air to the material while stirring. The amount of air added is 3%-9% of the total volume of cement, silica fume, aggregate, water, water reducer and steel fiber. Stir for 30 minutes.
[0022] Step 4. Evacuate the mixing tank to expel the internal gas from the mixed material in the mixing tank in step 3.
[0023] Preferably, the mixing tank is provided with a first air cylinder, an air injection pipe and a second air cylinder. The first air cylinder is connected to the mixing tank through the air injection pipe. The air outlet end of the first air cylinder is connected to the air inlet end of the air injection pipe. The air injection pipe extends into the bottom of the mixing tank to inflate the mixture. The second air cylinder is connected to the top of the mixing tank to extract the air in the mixing tank. The mixing tank is provided with a top cover, and the top cover is detachably sealed and connected to the tank body.
[0024] Preferably, the first gas cylinder has a scale, and the gas injection volume can be identified by the scale; the second gas cylinder has a scale, and the gas extraction volume can be identified by the scale.
[0025] Preferably, both the first gas cylinder and the second gas cylinder complete the movement of gas by moving the piston. In the step three, after sealing the mixing tank, push the piston of the first gas cylinder to inject a certain amount of air into the mixture, and the piston of the second gas cylinder will move outward under pressure. In the step four, pull the piston of the second gas cylinder until the air extraction volume of the second gas cylinder is not less than the air injection volume of the first gas cylinder, fix the piston position, maintain it for 3-5 minutes, and then pour out the fresh concrete.
[0026] Beneficial effects: The present invention, by adding special-shaped steel fibers and utilizing open rings and extensions, can improve the steel fibers' ability to bear and transfer stress on concrete, thereby improving the strength performance of concrete, while also improving the problem of uneven strength caused by uneven fiber mixing, thereby making the strength of concrete more balanced in various locations. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the steel fiber unit structure;
[0028] Figure 2 for Figure 1 Schematic diagram of the back structure of the steel fiber unit
[0029] Figure 3 It is a schematic diagram of the front view of a steel fiber unit structure with two extensions;
[0030] Figure 4 for Figure 3 A top view of
[0031] Figure 5 for Figure 1 Schematic diagram of the dispersion of steel fiber units in concrete;
[0032] Figure 6 for Figure 3 Schematic diagram of the dispersion of steel fiber units in concrete;
[0033] Figure 7 It is a schematic diagram when the steel fiber unit open ring is a multi-layer spiral structure;
[0034] Figure 8 This is a schematic diagram of the structure when preparing a ceramic tube surrounded by steel fibers;
[0035] Fig. 9 This is a schematic diagram of the structure when the steel wire is wrapped around the ceramic tube;
[0036] Fig.10 It is a schematic diagram of the structure when the multi-layer spiral structured open ring surrounds the ceramic tube;
[0037] Fig.11 It is a structural schematic diagram of the connection relationship between the mixing tank and the gas cylinder.
[0038] The numbers in the figure represent the following: 100. steel fiber; 110. open ring; 120. extension part; 130. ceramic tube; 200. mixing tank; 300. first air cylinder; 400. second air cylinder. DETAILED DESCRIPTION
[0039] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0040] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0042] Example 1
[0043] A method for preparing a novel ultra-high performance concrete comprises the steps of mixing cement, silica fume, aggregate, water, a water reducing agent and steel fibers, wherein the steel fibers account for 1-2.5% of the total volume of the concrete by volume; the steel fibers are composed of a plurality of steel fiber units 100, each of which comprises an open ring 110 and an extension portion 120 connected thereto; the extension portion 120 extends from an open end of the open ring in a direction away from the open ring, and the extension length is not less than the inner diameter of the open ring; and the plurality of steel fiber units 100 are uniformly dispersed in the novel ultra-high performance concrete.
[0044] like Figure 1 and 2 As shown, the open ring in this embodiment is a single ring formed by a wire, and the distance between the two open ends of the open ring in the axial direction of the ring is no more than 3 mm.
[0045] The specific steps of the preparation method of the novel ultra-high performance concrete are as follows: 1000 kg of PO 52.5 ordinary Portland cement with a SiO2 content of 95% and a specific surface area of 20,000 m 2 200kg of silica fume (about 0.04475 kg), 1200kg of 4-mesh quartz sand, and 218kg of steel fiber are fully mixed in a concrete mixer; then 223kg of water is added and stirred for 30 minutes; then 18kg of polycarboxylic acid water reducer with a water reduction rate of 40% is added and stirred until the mixture is uniform. The 10 prepared test blocks of 150 cubic millimeters have a 28-day compressive strength of 101.1MPa at the lowest and 141.2MPa at the highest, and the difference between the minimum and maximum strengths is significantly reduced. Because the steel fiber can form an anchor area in three-dimensional space not only in the length direction, it is easier to form a continuous spatial structure between areas. On the one hand, this kind of steel fiber with an open ring is not easy to form uneven dispersion problems, because due to its shape, multiple steel fibers are not easy to bond, unlike ordinary steel fibers, which are easy to bond in the presence of liquid. On the other hand, Figure 1-2 The steel fibers shown, even if they are unevenly dispersed like ordinary steel fibers, refer to Figure 5 This type of fiber will also have a stress relationship with concrete in three-dimensional space, and can bear the load of concrete in three-dimensional directions, with better reinforcement effect and less prone to problems of excessive or low local strength.
[0046] Example 2
[0047] Same as Example 1, except that, see Figure 3 , 4 and 6, there are two extending portions 120, and the two extending portions extend in opposite directions.
[0048] Using the same mix ratio and preparation method, and using this steel fiber, 10 test blocks of 150 cubic millimeters were made in the same way as in Example 1. The 28-day compressive strength was as low as 112.1 MPa and as high as 145.5 MPa. It can be seen that with the action of the two extensions extending in opposite directions and the open ring, the strength range of the concrete is narrower and more uniform.
[0049] Example 3
[0050] A single split ring can hold a small amount of hardened concrete, but the load it carries and the reinforcement effect are limited. Therefore, the split ring is further improved. Figure 7 As shown, the open ring 120 is formed by a steel wire wrapped around a plurality of spiral structures arranged up and down. The axial length of the spiral is not greater than the length of the extension portion. The diameters of the outermost circle and the innermost circle of the spiral are different, and the diameter of the large diameter end is 1.5-3 times the diameter of the small diameter end.
[0051] Use as Figure 7 The steel fiber shown is used to prepare concrete using the method of Example 1. The 28-day compressive strength of 10 test blocks is 121.3-148.9Mpa. This steel fiber has a stronger ability to combine with concrete, a stronger bearing capacity, and better concrete continuity. The steel fiber itself is also less likely to agglomerate, has better dispersion, a narrower strength range, and better strength stability.
[0052] Example 4
[0053] The bond strength between steel fiber and concrete is reduced, or the presence of chloride ions and other substances in the concrete that make the steel fiber easily corrode will cause the bond between steel fiber and concrete to fail. This will lead to a significant decrease in concrete strength. Therefore, in order to make the bond between steel fiber and concrete stronger and to make the steel fiber form a more stable strength bearing area in the concrete, further improvements are made to the steel fiber, such as Figure 8-10 shown.
[0054] A ceramic tube 130 is surrounded in the open ring 110, and the inner diameter of the ceramic tube 130 is the average number X±1mm of the maximum diameter and the minimum diameter of the aggregate.
[0055] The mortar is supplied to the ceramic tube, so that the steel fiber forms a load-bearing part with stronger load-bearing capacity and greater bonding strength with concrete. Combined with the hardened concrete, a more stable stress-bearing area is formed. Compared with simple steel fibers, this load-bearing area has a larger stress-bearing range and a stronger connection with concrete. It is easier for stress conduction to form between steel fibers, which greatly improves the overall mechanics of the concrete.
[0056] The 28-day compressive strength of 10 test blocks of concrete prepared by the method of Example 1 ranged from 132.4 to 151.1 MPa. It can be seen that the fiber of this structure can further improve the strength stability of concrete and greatly improve the strength of concrete.
[0057] The method of surrounding the ceramic tube 130 is as follows:
[0058] Step 1: Heat the steel wire to 120-150℃;
[0059] Step 2: fix the ceramic tube 130 vertically, and wrap the steel wire obtained in step 1 around the ceramic tube 130 to form an open ring 110 , and trim the remaining part to form an extension part 120 .
[0060] Step 3: Wait for the steel wire to cool and shrink naturally.
[0061] The purpose of cooling the steel wire after heating is to allow the steel wire to generate prestress on the ceramic pot. On the one hand, the bonding force between the steel wire and the ceramic pot is stronger and not easy to separate. On the other hand, when the concrete is compressed and the ceramic tube expands outward, the open ring 110 of the steel fiber can better bear the load, the strength stability is better, and the concrete is not easy to have micro cracks at the bonding interface.
[0062] Example 5
[0063] The steel fiber has an open ring, which creates a lot of obstacles during the mixing process. In order to further improve the uniformity of the steel fiber dispersion in concrete, the mixing process is further improved, such as Fig.11 shown.
[0064] The concrete mixing method comprises the following steps:
[0065] Step 1: Pour the solid material into the mixing tank 200;
[0066] Step 2: Add water and other liquid components into the stirring tank 200;
[0067] Step 3: Inflate the material while stirring. The amount of air added is 3%-9% of the total volume of cement, silica fume, aggregate, water, water reducer and steel fiber. Stir for 30 minutes.
[0068] Step 4: evacuate the mixing tank 200 to discharge the internal gas from the mixed material in the mixing tank 200 prepared in step 3.
[0069] It also includes a first gas cylinder 300, a gas injection pipe 310 and a second gas cylinder 400;
[0070] The first gas cylinder 300 is connected to the mixing tank 200 through the gas injection pipe 310. The gas outlet of the first gas cylinder 300 is connected to the gas inlet of the gas injection pipe 310. The gas injection pipe 310 extends into the bottom of the mixing tank 200 to inflate the mixture. The first gas cylinder 300 is provided with a scale, and the gas injection amount can be identified by the scale.
[0071] The second air cylinder 400 is connected to the top of the stirring tank 200 and is used to extract air from the stirring tank 200. The stirring tank 200 is provided with a top cover, and the top cover is detachably sealed and connected to the tank body;
[0072] The second gas cylinder 400 has a scale, and the amount of gas pumped can be identified by the scale;
[0073] The first gas cylinder 300 and the second gas cylinder 400 both achieve gas movement through piston movement.
[0074] In step three, after the mixing tank 200 is sealed, the piston of the first air cylinder 300 is pushed to inject a certain amount of air into the mixture, and at this time, the piston of the second air cylinder 400 is pressed to move outward;
[0075] Step four, pull the piston of the second air cylinder 400 until the air extraction volume of the second air cylinder 400 is not less than the air injection volume of the first air cylinder 300, fix the piston position, maintain for 3-5 minutes, and then pour out the freshly mixed concrete. After the first air cylinder is inflated, the piston of the second air cylinder will be compressed and move outward, but the air pressure will be stable. When it is necessary to maintain the vacuum state in the mixing tank, continue to pull the piston of the second air cylinder. When inflating, in order to make the materials in the concrete move more smoothly and the materials disperse more evenly, especially the steel fibers. When venting, in order to avoid air bubbles being retained in the concrete, stress concentration points will be formed after hardening, resulting in a decrease in strength.
[0076] Through testing, the concrete of Examples 1 to 4 were mixed using the above-mentioned equipment and method, and the strength range and quality range of the obtained test blocks were compared. Among them, ordinary mixing is the mixing method in the prior art, and special mixing is the method provided in this Example 5, as shown in the following table.
[0077]
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing ultra-high performance concrete, comprising mixing cement, silica fume, aggregate, water, a water reducing agent and steel fiber, characterized in that: The steel fiber accounts for 1-2.5% of the total volume of the concrete by volume; The steel fiber is composed of a plurality of steel fiber units (100), each of the steel fiber units (100) comprising an open ring (110) and an extension portion (120) connected thereto, wherein the extension portion (120) extends from an open end of the open ring (110) in a direction away from the open ring (110), and the extension length is not less than the inner diameter of the open ring (110); A plurality of steel fiber units (100) are uniformly dispersed in ultra-high performance concrete; a ceramic tube (130) is surrounded by the open ring (110), and the inner diameter of the ceramic tube (130) is an average of the maximum diameter and the minimum diameter of the aggregate X±1 mm.
2. The method for preparing ultra-high performance concrete according to claim 1, characterized in that: Each steel fiber unit (100) comprises an open ring (110) and one or two extension parts (120) connected thereto; when there is one extension part (120), it is connected to any open end of the open ring (110); when there are two extension parts (120), the two extension parts (120) extend in opposite directions.
3. The method for preparing ultra-high performance concrete according to claim 1, characterized in that: The open ring (110) is a single ring formed by a steel wire being wound around, or a spiral structure formed by at least two turns.
4. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: When the open ring (110) is a spiral structure formed by a steel wire being wound at least twice, the diameters of the outermost circle and the innermost circle are different, and the diameter of the large diameter end is 1.5 to 3 times the diameter of the small diameter end.
5. The method for preparing ultra-high performance concrete according to claim 1, characterized in that: The method of surrounding the ceramic tube (130) is as follows: Step 1. Heat the steel wire to 120-150℃; Step 2. Fix the ceramic tube (130) vertically, and wrap the steel wire obtained in step 1 around the ceramic tube (130), so that the portion of the steel wire wrapped around the ceramic tube (130) forms an open ring (110), and the remaining portion is trimmed to form an extension portion (120); Step 3. Wait for the steel wire to cool and shrink naturally.
6. The method for preparing ultra-high performance concrete according to any one of claims 1 to 5, characterized in that: When mixing cement, silica fume, aggregate, water, water reducing agent and steel fiber, the specific steps are as follows: Step 1. Pour the solid material into the mixing tank (200); Step 2. Add water and other liquid components into the stirring tank (200); Step 3. Seal the mixing tank (200), and add air to the materials while stirring. The amount of air added is 3% to 9% of the total volume of cement, silica fume, aggregate, water, water reducing agent and steel fiber, and stir for 30 minutes; Step 4. Evacuate the mixing tank (200) to expel the internal gas from the mixed material in the mixing tank (200) in step 3.
7. The method for preparing ultra-high performance concrete according to claim 6, characterized in that: The stirring tank (200) is provided with a first gas cylinder (300), a gas injection pipe (310) and a second gas cylinder (400); the first gas cylinder (300) is connected to the stirring tank (200) via the gas injection pipe (310); the gas outlet end of the first gas cylinder (300) is connected to the gas inlet end of the gas injection pipe (310); the gas injection pipe (310) extends into the bottom of the stirring tank (200) and is used to inflate the mixture; the second gas cylinder (400) is connected to the top of the stirring tank (200) and is used to extract air from the stirring tank (200); the stirring tank (200) is provided with a top cover, and the top cover is detachably sealed and connected to the tank body.
8. The method for preparing ultra-high performance concrete according to claim 7, characterized in that: The first gas cylinder (300) is provided with a scale, and the gas injection volume can be identified by the scale; the second gas cylinder (400) is provided with a scale, and the gas extraction volume can be identified by the scale.
9. The method for preparing ultra-high performance concrete according to claim 7, characterized in that: The first gas cylinder (300) and the second gas cylinder (400) both complete the movement of gas by moving the piston. In the step three, after the mixing tank (200) is sealed, the piston of the first gas cylinder (300) is pushed to inject a certain amount of air into the mixture, and the piston of the second gas cylinder (400) is pressed to move outward. In the step four, the piston of the second gas cylinder (400) is pulled until the air volume extracted by the second gas cylinder (400) is not less than the air volume injected by the first gas cylinder (300), and then the piston position is fixed and maintained for 3-5 minutes before pouring out the freshly mixed concrete.