Aluminum suction tube resistant to aluminum liquid corrosion and its manufacturing method and application

By forming a high-entropy alloy coating on the steel substrate of the aluminum suction pipe and performing MIG welding, the problems of short life and high scrap rate caused by corrosion of aluminum suction pipes in electrolytic aluminum production are solved, and higher corrosion resistance is achieved. and service life, simplifying the process and reducing costs.

CN115922244BActive Publication Date: 2024-10-15QIANJIANG JIANGHAN DRILLING TOOLS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211512434.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-10-15
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

During the electrolytic aluminum production process, the existing aluminum suction pipes have a short service life and a high scrap rate due to corrosion by high-temperature aluminum liquid. Moreover, the existing improvement methods are complex in process and high in cost, making it difficult to meet the needs of electrolytic aluminum production.

Method used

Plasma deposition technology is used to form a high-entropy alloy coating on the surface of the steel substrate, and the pipes are tightly connected through MIG welding to form an aluminum-absorbing pipe that is resistant to corrosion by aluminum liquid, improving the bonding strength and electric shock resistance of the coating and the substrate.

Benefits of technology

It significantly extends the service life of the aluminum suction tube, reduces the scrap rate, improves the efficiency and safety of electrolytic aluminum production, simplifies the process flow, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115922244B_ABST
    Figure CN115922244B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing an aluminum absorption tube resistant to aluminum liquid corrosion, comprising the following steps: first, grinding and polishing, degreasing, derusting and sandblasting the surface of a steel substrate; second, forming a high entropy alloy coating on the treated steel substrate surface by plasma deposition of a high entropy alloy composite powder; third, cooling the product with the furnace to obtain a composite material resistant to aluminum liquid corrosion; finally, rolling the composite material resistant to aluminum liquid corrosion to form a tube, and closely connecting the joints of the tube by MIG welding to obtain an aluminum absorption tube resistant to aluminum liquid corrosion. The present invention also provides an aluminum absorption tube obtained by the above-mentioned manufacturing method, and a lifting bag provided with the aluminum absorption tube. The aluminum absorption tube has excellent aluminum liquid corrosion resistance, a longer service life, and a lower scrap rate, which is of great significance for improving the quality of aluminum liquid, reducing the efficiency of disassembly and cleaning of the aluminum absorption tube, reducing labor intensity, achieving energy conservation and emission reduction, and ensuring safe production of electrolytic series.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metallurgy, and in particular relates to an aluminum absorbing tube resistant to aluminum liquid corrosion and a manufacturing method thereof, and also relates to a lifting bag comprising the aluminum absorbing tube resistant to aluminum liquid corrosion. Background Art

[0002] The ladle is an important equipment in the production process of electrolytic aluminum. It is mainly responsible for sucking out the high-temperature aluminum liquid from the electrolytic cell and transporting it. The aluminum suction tube is an indispensable and important structure of various types of ladle (including open ladle and vacuum ladle). It is generally composed of three sections: a curved tube (also called a spherical tube, A tube) at the top connected to the ladle body, a horseshoe-shaped straight tube (C tube) inserted into the aluminum liquid during aluminum suction, and a straight tube with flanges at both ends (B tube). The aluminum suction tubes currently used are basically all made of integral casting, which is relatively expensive and has high requirements for materials.

[0003] During operation, the C tube of the aluminum suction tube is inserted into the aluminum liquid in the electrolytic aluminum tank. Using the siphon principle, the aluminum liquid is sucked into the lifting bag along the B tube and the A tube. Since the temperature of the aluminum liquid is as high as 660-950°C and there are electrolyte fluorides, the aluminum suction tube will be continuously eroded and corroded by the high-temperature aluminum liquid during the above working process, which can easily lead to thinning of the tube wall or even perforation. Generally, the aluminum suction tube will be scrapped after 20-30 bags of aluminum are produced. It has a short service life, consumes a lot of materials, and has a high replacement frequency, which not only reduces the production efficiency of the electrolytic cell, but also increases the cost of aluminum production.

[0004] Based on the above background, researchers have been exploring new methods for preparing aluminum absorption tubes; however, most of these methods also have shortcomings. For example, the patent with publication number CN 104894465 A discloses a high-chromium cast iron aluminum absorption tube and its preparation method, which prepares a high-chromium cast iron aluminum absorption tube through smelting, deterioration treatment, calming treatment, heat treatment and other process flows. Compared with the existing aluminum absorption tube, its high-temperature stability has been improved to a certain extent, but the process of this method is relatively complicated, the production efficiency is low, and the economic benefits are insufficient.

[0005] The patent with the publication number CN2821346 discloses a high-strength composite aluminum suction tube, which adopts a structure of an outer metal sleeve and an inner graphite fiber to solve the problem that the inner wall of the pipe is blocked by electrolytic aluminum and filter residue during use and cannot be used any longer. However, the aluminum suction tube has the problems of complex process flow and high production cost. At the same time, the connection strength between the outer metal sleeve and the inner graphite is difficult to meet, and the outer metal tube still cannot prevent electric shock loss.

[0006] Based on this, it is a technical problem that urgently needs to be solved to provide an aluminum absorption tube with excellent resistance to aluminum liquid corrosion, and to improve the connection strength between the composite material and the matrix, so that it has a longer service life and a lower scrap rate, thereby increasing the manufacturing and use costs of the aluminum absorption tube in the electrolytic aluminum production industry, and achieving energy conservation, emission reduction and safe production. Summary of the invention

[0007] One of the purposes of the present invention is to provide a method for manufacturing an aluminum suction tube which is resistant to aluminum liquid corrosion and has good corrosion resistance and high connection strength between the coating material and the substrate.

[0008] The second object of the present invention is to provide an aluminum suction tube which is resistant to aluminum liquid corrosion and has good corrosion resistance and high connection strength between the coating material and the substrate.

[0009] The third object of the present invention is to provide a lifting bag with a long service life, a low scrap rate and a reduced replacement frequency of the aluminum suction tube.

[0010] The technical solution adopted by the present invention to achieve one of the purposes is: to provide a method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion, comprising the following steps:

[0011] S1. Grinding, polishing, degreasing, rust removal and sandblasting the surface of the steel substrate to obtain a treated steel substrate;

[0012] S2. Forming a high entropy alloy coating on the surface of the treated steel substrate by plasma deposition of a high entropy alloy composite powder; the high entropy alloy composite powder comprises an alloy powder and a ceramic phase powder, the alloy powder is selected from FeCrCoMnNi alloy and / or FeCuCoMnNi alloy, and the ceramic phase powder is selected from a combination of one or more of ZrC powder, WC powder or MoC powder;

[0013] S3, cooling the product obtained in step S2 along with the furnace temperature to obtain a composite material resistant to aluminum liquid corrosion;

[0014] S4, rolling the composite material resistant to aluminum liquid corrosion into a tube with a diameter of 130-150 mm, and connecting the seams of the tube tightly by MIG welding to obtain an aluminum liquid corrosion resistant aluminum absorption tube.

[0015] In the above manufacturing method, first, the steel substrate is fully pretreated to improve the bonding between the high entropy alloy coating and the steel substrate; secondly, a high entropy alloy composite powder with good bonding performance with the steel substrate and resistance to aluminum liquid corrosion is selected as a raw material by plasma cladding, and a high entropy alloy coating of a certain thickness is formed on the surface of the steel substrate, thereby further improving the resistance of the steel substrate surface to aluminum liquid corrosion; thirdly, the residual thermal stress in the cladding process is eliminated by furnace cooling, and the cracking of the coating is effectively prevented, thereby obtaining a composite material with good bonding performance and high connection strength; finally, the joints of the coiled tube are tightly connected by MIG welding to obtain an aluminum absorption tube with excellent resistance to aluminum liquid corrosion.

[0016] In the present invention, the selection of high entropy alloy composite powder is a necessary condition to ensure good and stable bonding performance between the coating and the steel substrate and to ensure that the obtained aluminum absorption tube has good resistance to aluminum liquid corrosion. After a large number of studies, it was found that when the alloy powder is selected from FeCrCoMnNi alloy and / or FeCuCoMnNi alloy, and is combined with ceramic phase powder formed by ZrC powder, WC powder or MoC powder, the high entropy coating formed by plasma deposition has the best bonding performance with the steel substrate, which can ensure the production of high-quality aluminum absorption tubes.

[0017] Preferably, the alloy powder is selected from FeCrCoMnNi alloy, and the ceramic phase powder is selected from ZrC powder. The composite material prepared by combining the above raw materials has good strength and toughness matching and relatively excellent impact resistance. In addition, after adding ZrC ceramic powder, the resistance is reduced, and the anti-electric shock performance of the aluminum absorption tube in the electrolytic cell can be improved. Thereby, the wear caused by scouring and the damage caused by electric shock of the aluminum absorption tube in the electrolytic aluminum preparation process can be better avoided.

[0018] Preferably, the high entropy alloy powder is placed in a box-type heat preservation furnace and stored at a constant temperature of 70 to 120° C. before use. This operation can dry the high entropy alloy powder and avoid defects such as pores in the coating.

[0019] Furthermore, in step S1, the thickness of the steel substrate is 10-15 mm, and the steel substrate is selected from Q235 steel or 304 stainless steel. Preferably, the steel substrate is Q235 steel, because Q235 steel is low in cost, and because Q235 steel contains fewer alloy elements, the welding performance after rolling is better. Optionally, in step S1, sandblasting is used to increase the roughness of the steel substrate surface.

[0020] Furthermore, in step S2, the high entropy alloy powder is spherical, with a particle size of 100 to 200 meshes, and the plasma deposition process is stable and reliable.

[0021] Furthermore, the thickness of the high entropy alloy coating is 2 to 4 mm. Under this thickness condition, a layer of metal can be deposited by optimizing the process. The wall thickness of the overall aluminum absorption tube can be controlled within 12 to 25 mm, and has good matching performance with other existing equipment.

[0022] Furthermore, in the plasma deposition, the temperature of the high entropy alloy composite powder is 70-80°C, the deposition current is 160-180A, the powder feeding gas flow rate is 3.5-6.5L / min, the powder feeding rate is 40-60g / min, and the deposition speed is 300-400mm / min. Preferably, the plasma deposition is performed in a double-sided deposition manner, that is, the corresponding high entropy alloy coating is formed on both sides of the steel substrate by plasma deposition.

[0023] In the present invention, plasma deposition is selected to prepare the high entropy coating because the plasma deposition technology can ensure the compactness of the high entropy alloy coating and increase the bonding strength between the steel substrate and the high entropy alloy coating; wherein, the argon atmosphere can prevent oxidation of the steel substrate and the high entropy alloy deposited powder. The present invention optimizes and adjusts the process parameters during the plasma deposition process, and the aluminum absorption tube prepared has good resistance to aluminum liquid corrosion, thermal stability, impact resistance and wear ratio.

[0024] Furthermore, in step S3, the initial temperature of the furnace cooling is 400-500°C, and the cooling rate is 30-50°C / h. Under the above cooling conditions, the residual thermal stress in the deposition process can be effectively eliminated, and the coating can be prevented from cracking, which provides a guarantee for the preparation of a composite material with good bonding performance and high connection strength.

[0025] Furthermore, in step S4, the diameter of the pipe is 130-150 mm; the welding atmosphere of the MIG welding is argon, the welding wire of the MIG welding is selected from ER309L welding wire with a diameter of 1.2 mm or 1.6 mm, and the welding speed is 200-300 mm / min. Among them, the advantages of using MIG welding are high welding quality and high production efficiency. The welding wire is ER309L, which has smooth wire feeding, stable arc, beautiful forming, and very little spatter; the deposited metal contains an appropriate amount of ferrite and has good crack resistance. Due to the high content of the alloy, it has good high temperature resistance; the carbon content is low and the corrosion resistance is excellent. The most important thing is that this welding wire can not only be used to weld Q235 carbon steel, but also can be used to weld high entropy alloys, thereby avoiding the replacement of welding materials during the welding of the substrate and the coating.

[0026] The technical solution adopted by the present invention to achieve the third purpose is: to provide an aluminum absorption tube, which is made of the composite material resistant to aluminum liquid corrosion as described in one of the purposes of the present invention. In the present invention, in addition to the winding manufacturing method, when preparing a smaller size of aluminum absorption tube, a stamping method can be used for processing.

[0027] Furthermore, the inner and outer sides of the C tube portion of the aluminum absorption tube are both provided with a high entropy alloy coating.

[0028] Preferably, before the MIG welding, the joints on both sides of the pipe are laser cleaned to remove surface oil and oxide layer and increase the surface roughness.

[0029] Preferably, during the MIG welding process, the weld formed by welding is tapped. In the present invention, during the MIG welding process, the weld is tapped with a tool (such as a small hammer, etc.), which can eliminate the residual thermal stress of the weld and effectively avoid cracking at the weld.

[0030] The technical solution adopted by the present invention to achieve the third purpose is: to provide a lifting bag, the lifting bag includes the aluminum absorption tube described in the second purpose of the present invention.

[0031] When the above-mentioned lifting ladle is used in the electrolytic aluminum production process, the C tube of the lifting ladle aluminum suction tube is inserted into the high-temperature aluminum liquid to absorb the aluminum liquid. Since the C tube of the aluminum suction tube is provided with a high-entropy alloy coating on both the inner and outer sides, it can effectively avoid the corrosion of the aluminum suction tube caused by the high-temperature aluminum liquid, thereby extending the service life of the aluminum suction tube; at the same time, the high-entropy alloy coating has a high connection strength with the steel substrate and is not easy to fall off and be damaged. The high-entropy alloy coating rich in ceramics is not easily damaged by electric shock, which can reduce material consumption and replacement frequency, thereby comprehensively improving the production efficiency of the electrolytic cell and reducing the cost of aluminum output.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention provides a method for manufacturing an aluminum absorption tube that is resistant to aluminum liquid corrosion, which includes forming a high entropy alloy coating on the surface of a steel substrate by plasma deposition. Among them, suitable high entropy alloy composite powder enables the coating to form a good and stable bonding performance with the steel substrate, ensuring that the obtained aluminum absorption tube has good resistance to aluminum liquid corrosion and electric shock. The manufacturing process of plasma deposition improves the density of the high entropy alloy coating and the bonding strength between the steel substrate and the high entropy alloy coating. The obtained composite material has excellent resistance to aluminum liquid corrosion and good overall performance. The coating is not easy to crack or peel off, which prolongs the service life of the composite material under high-temperature aluminum liquid conditions, reduces the scrap rate, and avoids the occurrence of safety accidents.

[0034] (2) The aluminum absorption tube provided by the present invention has a high entropy alloy coating on its surface, which has excellent resistance to aluminum liquid corrosion and electric shock, longer service life, and lower scrap rate. It is of great significance for improving the quality of aluminum liquid, reducing the efficiency of disassembly and cleaning of the aluminum absorption tube, reducing labor intensity, achieving energy conservation and emission reduction, and ensuring safe production of the electrolytic series.

[0035] (3) Compared with the aluminum absorption tube prepared by the traditional method, the aluminum absorption tube provided by the present invention can significantly reduce the iron content in the aluminum liquid, which is of great significance to improving the quality of the aluminum liquid produced by electrolytic aluminum. In addition, the aluminum absorption tube of the present invention is made by winding. Compared with the integral casting method, the process flow of the present invention is simple, less polluting, low in time cost, and high in economic benefit. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The electron microscope images of the high entropy alloy powder and the ZrC powder used in Example 1 of the present invention; wherein (a) is a high-magnification SEM image of the high-entropy alloy powder; (b) is a low-magnification SEM image of the high-entropy alloy powder; (c) is a high-magnification SEM image of the ZrC powder; (d) is a low-magnification SEM image of the ZrC powder;

[0037] Figure 2 This is a schematic diagram of the structure of the plasma cladding equipment used in Example 1 of the present invention;

[0038] Figure 3 This is a schematic diagram of the structure of the composite material prepared in Example 1 of the present invention;

[0039] Figure 4 This is an EDS line scan distribution diagram near the fusion line of the composite material prepared in Example 1 of the present invention;

[0040] Figure 5 This is an EDS surface scanning distribution diagram near the fusion line of the composite material prepared in Example 1 of the present invention;

[0041] Figure 6 This is a comparison chart of the mass loss of the aluminum absorption tube material prepared in Example 1 of the present invention and the conventional aluminum absorption tube material in aluminum liquid;

[0042] Figure 7 It is a schematic structural diagram of a lifting bag including the aluminum suction tube prepared in Example 1 of the present invention.

[0043] Among them, 10-workpiece; 11-electrode; 12-ion gas; 13-ceramic tube; 141-water inlet; 142-water outlet; 15-powder feeding gas; 16-shielding gas; 17-nozzle; 18-plasma arc; 19-molten pool; 21-steel substrate; 22-high entropy alloy coating; 30-aluminum suction tube; 31 aluminum suction tube C tube; 32-ejector; 33-crossbeam; 34-jib; 35-manhole; 36-package cover; 37-speed reduction mechanism; 38-package body; 39-lining. DETAILED DESCRIPTION

[0044] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0046] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0047] Example 1

[0048] A method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion comprises the following steps:

[0049] Step 1: Use Q235 steel as the steel substrate, grind and polish, degrease and rust, and sandblast its surface to obtain the treated steel substrate, and place it in a drying furnace to keep it warm at 80°C;

[0050] Step 2: Using FeCrCoMnNi high entropy alloy powder with a purity higher than 99.9% and a particle size of 160 mesh as the alloy phase and ZrC powder as the ceramic phase, a high entropy alloy composite powder raw material is prepared, and the powder is placed in a drying furnace for drying for 1.5 hours at a drying temperature of 100°C; a high entropy alloy coating with a thickness of 3 mm is formed on the surface of the treated steel substrate by plasma deposition; the parameters of the plasma deposition are as follows: the temperature of the high entropy alloy composite powder is 80°C, the deposition current is 170A, the powder feeding gas flow rate is 5L / min, the powder feeding rate is 50g / min, and the deposition speed is 350mm / min.

[0051] Step 3: Cooling the workpiece obtained in step 2 at 450° C. at a cooling rate of 40° C. / h to obtain a composite material resistant to aluminum liquid corrosion;

[0052] Step 4: The composite material resistant to aluminum liquid corrosion is rolled into a tube with a diameter of 140 mm, and the joints of the tubes are tightly connected by MIG welding (the welding atmosphere is argon, an ER309L welding wire with a diameter of 1.2 mm is selected, and the welding speed is 200 mm / min) to form a metallurgical bond, thereby obtaining an aluminum absorption tube resistant to aluminum liquid corrosion.

[0053] Figure 4 This is an EDS line scan distribution diagram near the fusion line of the composite material prepared in Example 1 of the present invention; Figure 5 This is an EDS surface scanning distribution diagram near the fusion line of the composite material obtained in Example 1 of the present invention. It can be seen from the figure that the dilution rate of the main elements of the high entropy alloy and the Q235 steel matrix is ​​relatively low. This is because the hysteresis diffusion effect of the high entropy alloy coating makes it difficult for the matrix elements to diffuse into the coating. The above characteristics can effectively avoid corrosion and damage caused by high-temperature Al liquid scouring during the operation of the aluminum suction tube.

[0054] Figure 6 The figure is a comparison of the mass loss of the aluminum absorption tube material prepared in Example 1 of the present invention and the conventional aluminum absorption tube material in aluminum liquid. It can be seen from the figure that in the same time, the weight loss of the aluminum absorption tube prepared in Example 1 of the present invention is much lower than that of the conventional aluminum absorption tube.

[0055] Figure 7 A schematic diagram of a lifting bag is provided, which has an aluminum absorption tube made in Example 1 of the present invention, and a high-entropy alloy coating is provided on both the inner and outer sides of the C tube of the aluminum absorption tube, which can effectively avoid corrosion of the aluminum absorption tube caused by high-temperature aluminum liquid, thereby extending the service life of the aluminum absorption tube; at the same time, the high-entropy alloy coating has a high connection strength with the steel substrate and is not easy to fall off and be damaged, which can reduce material consumption and replacement frequency, thereby comprehensively improving the production efficiency of the electrolytic cell and reducing the aluminum output cost.

[0056] Example 2

[0057] A method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion comprises the following steps:

[0058] Step 1: Use Q235 steel as the steel substrate, grind and polish, degrease and rust, and sandblast its surface to obtain the treated steel substrate, and place it in a drying furnace to keep it warm to 90°C;

[0059] Step 2: Using FeCrCoMnNi high entropy alloy powder with a purity higher than 99.9% and a particle size of 100-200 mesh as the alloy phase and WC powder as the ceramic phase, a high entropy alloy composite powder raw material is prepared, and the powder is placed in a drying furnace and dried for 1 hour at a drying temperature of 120°C; a high entropy alloy coating with a thickness of 4 cm is formed on the surface of the treated steel substrate by plasma deposition; the parameters of plasma deposition are as follows: the temperature of the high entropy alloy composite powder is 75°C, the deposition current is 180A, the powder feeding gas flow rate is 3.5L / min, the powder feeding rate is 60g / min, and the deposition speed is 300mm / min.

[0060] Step 3: Cooling the product obtained in step 2 at 400° C. at a cooling rate of 30° C. / h in a furnace to obtain a composite material resistant to aluminum liquid corrosion;

[0061] Step 4: The composite material resistant to aluminum liquid corrosion is rolled into a tube with a diameter of 130 mm, and the joints of the tubes are tightly connected by MIG welding (the welding atmosphere is argon, an ER309L welding wire with a diameter of 1.2 mm is selected, and the welding speed is 300 mm / min) to form a metallurgical bond, thereby obtaining an aluminum absorption tube resistant to aluminum liquid corrosion.

[0062] Example 3

[0063] A method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion comprises the following steps:

[0064] Step 1: Use Q235 steel as the steel substrate, grind and polish, degrease and rust, and sandblast its surface to obtain the treated steel substrate, and place it in a drying furnace to keep it warm at 80°C;

[0065] Step 2: Using FeCrCoMnNi high entropy alloy powder with a purity higher than 99.9% and a particle size of 100-200 mesh as the alloy phase and MoC powder as the ceramic phase, a high entropy alloy composite powder raw material is prepared, and the powder is placed in a drying furnace and dried for 2 hours at a drying temperature of 70°C; a high entropy alloy coating with a thickness of 2 cm is formed on the surface of the treated steel substrate by plasma deposition; the parameters of plasma deposition are as follows: the temperature of the high entropy alloy composite powder is 70°C, the deposition current is 160A, the powder feeding gas flow rate is 6.5L / min, the powder feeding rate is 60g / min, and the deposition speed is 400mm / min.

[0066] Step 3: Cooling the product obtained in step 2 at 500° C. at a cooling rate of 50° C. / h in a furnace to obtain a composite material resistant to aluminum liquid corrosion;

[0067] Step 4: Roll the composite material resistant to aluminum liquid corrosion into a tube with a diameter of 150 mm, and use MIG welding (the welding atmosphere is argon, the ER309L welding wire with a diameter of 1.6 mm is selected, and the welding speed is 250 mm / min) to tightly connect the joints of the tube to form a metallurgical bond, thereby obtaining an aluminum liquid corrosion-resistant aluminum absorption tube.

[0068] Example 4

[0069] A method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion comprises the following steps:

[0070] Step 1: Use Q235 steel as the steel substrate, grind and polish, degrease and rust, and sandblast its surface to obtain the treated steel substrate, and place it in a drying furnace to keep it warm to 90°C;

[0071] Step 2: Using FeCuCoMnNi high entropy alloy powder with a purity higher than 99.9% and a particle size of 100-200 mesh as the alloy phase and ZrC powder as the ceramic phase, a high entropy alloy composite powder raw material is prepared, and the powder is placed in a drying furnace for drying for 1.5 hours at a drying temperature of 90°C; a high entropy alloy coating with a thickness of 3 cm is formed on the surface of the treated steel substrate by plasma deposition; the parameters of plasma deposition are as follows: the temperature of the high entropy alloy composite powder is 75°C, the deposition current is 170A, the powder feeding gas flow rate is 4.5L / min, the powder feeding rate is 55g / min, and the deposition speed is 350mm / min.

[0072] Step 3: Cooling the product obtained in step 2 at 450° C. at a cooling rate of 40° C. / h to obtain a composite material resistant to aluminum liquid corrosion;

[0073] Step 4: The composite material resistant to aluminum liquid corrosion is rolled into a tube with a diameter of 150 mm, and the joints of the tubes are tightly connected by MIG welding (the welding atmosphere is argon, an ER309L welding wire with a diameter of 1.2 mm is selected, and the welding speed is 220 mm / min) to form a metallurgical bond, thereby obtaining an aluminum absorption tube resistant to aluminum liquid corrosion.

[0074] Example 5

[0075] A method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion comprises the following steps:

[0076] Step 1: Use 304 as the steel substrate, grind and polish, degrease and rust, and sandblast its surface to obtain the treated steel substrate, and place it in a drying furnace to keep it at 100°C;

[0077] Step 2: Using FeCrCoMnNi high entropy alloy powder with a purity higher than 99.9% and a particle size of 100-200 mesh as the alloy phase and ZrC powder as the ceramic phase, a high entropy alloy composite powder raw material is prepared, and the powder is placed in a drying furnace for drying for 1.5 hours at a drying temperature of 100°C; a high entropy alloy coating with a thickness of 3 cm is formed on the surface of the treated steel substrate by plasma deposition; the parameters of plasma deposition are as follows: the temperature of the high entropy alloy composite powder is 80°C, the deposition current is 180A, the powder feeding gas flow rate is 6.5L / min, the powder feeding rate is 60g / min, and the deposition speed is 400mm / min.

[0078] Step 3: Cooling the product obtained in step 2 at 400° C. at a cooling rate of 40° C. / h in a furnace to obtain a composite material resistant to aluminum liquid corrosion;

[0079] Step 4: The composite material resistant to aluminum liquid corrosion is rolled into a tube with a diameter of 150 mm, and the joints of the tubes are tightly connected by MIG welding (the welding atmosphere is argon, an ER309L welding wire with a diameter of 1.6 mm is selected, and the welding speed is 280 mm / min) to form a metallurgical bond, thereby obtaining an aluminum absorption tube resistant to aluminum liquid corrosion.

[0080] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing an aluminum suction tube resistant to aluminum liquid corrosion, The following steps are involved: S1. Grinding, polishing, degreasing, rust removal and sandblasting the surface of the steel substrate to obtain a treated steel substrate; the thickness of the steel substrate is 10-15 mm, and the steel substrate is selected from Q235 steel or 304 stainless steel; S2, forming a high entropy alloy coating on the surface of the treated steel substrate by plasma cladding of high entropy alloy composite powder; the high entropy alloy composite powder comprises alloy powder and ceramic phase powder, the alloy powder is selected from FeCrCoMnNi alloy, and the ceramic phase powder is ZrC powder; in the plasma cladding, the cladding current is 160-180A, the powder feeding gas flow rate is 3.5-6.5L / min, the powder feeding rate is 40-60g / min, and the cladding speed is 300-400mm / min; the plasma cladding is performed in a double-sided cladding manner; S3, cooling the product obtained in step S2 with the furnace to obtain a composite material resistant to aluminum liquid corrosion; the initial temperature of the furnace cooling is 400-500°C, and the cooling rate is 30-50°C / h; S4. The composite material resistant to aluminum liquid corrosion is rolled into a tube with a diameter of 130-150 mm, and the joints of the tube are tightly connected by MIG welding. The welding atmosphere of the MIG welding is argon gas, and the welding wire of the MIG welding is selected from ER309L welding wire with a diameter of 1.2 mm or 1.6 mm. The welding speed is 200-300 mm / min, so as to obtain an aluminum absorption tube resistant to aluminum liquid corrosion.

2. The manufacturing method according to claim 1, It is characterized in that In step S2, the high entropy alloy composite powder is spherical and has a particle size of 100-200 meshes.

3. The manufacturing method according to claim 2, It is characterized in that In step S2, the thickness of the high entropy alloy coating is 2-4 mm.

4. A suction aluminum tube, It is characterized in that The method is prepared according to any one of claims 1 to 3.

5. A lifting bag, It is characterized in that It comprises the aluminum suction tube as claimed in claim 4.

Citation Information

Cited By

  • Low interface defect control method using plasma deposition

    CN122061144A