Fluorine-free super-hydrophobic micro-nano structure SiO2 / TiN anti-icing and photo-thermal deicing coating
By combining TiN nanospheres and SiO2 microspheres in the photothermal superhydrophobic coating, a fluorine-free superhydrophobic micro-nanostructured SiO2/TiN coating was prepared, which solved the coating durability and environmental problems and achieved efficient Anti-ice and de-icing properties, suitable for applications under harsh conditions.
Patent Information
- Application Number
- CN202410596198.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The existing photothermal superhydrophobic coatings have poor durability, single functions, and environmental problems in use of fluorine-containing materials, making them difficult to actually apply under harsh conditions.
TiN nanospheres and SiO2 microspheres were mixed with materials such as 3-(isobutenyloxy)propyltrimethoxysilane through magnetic stirring, and the pH was adjusted by acetic acid and centrifuged purification, followed by octadecyl methacrylate and the other materials. Nitium bisisobutyronitrile was polymerized and a fluorine-free superhydrophobic micro-nanostructured SiO2/TiN coating was prepared using two-step spraying technology.
It achieves mechanical and chemical stability in harsh environments, extends the freezing time of water droplets, improves the photothermal deicing effect, maintains superhydrophobicity and self-cleaning effect, and is suitable for large-scale practical applications.
Smart Images

Figure CN118909515A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an anti-icing and photothermal deicing coating, and in particular to a fluorine-free super-hydrophobic micro-nanostructured SiO2 / TiN anti-icing and photothermal deicing coating. Background Art
[0002] Icing phenomena in nature bring great troubles to our daily lives. For example, driving on icy roads increases the risk of car accidents. Ice accumulation on aircraft wings can cause a decrease in flight speed or even a serious crash. Icing of power transmission lines can easily cause electrical short circuits. These icing phenomena not only increase energy consumption, but also pose a threat to personal safety. Traditional strategies to solve these problems mainly include mechanical vibration, chemical anti-icing agents, and electric thermal deicing, which are not only inefficient, costly, and harmful to the environment. Therefore, people have invested a lot of effort in developing new anti-icing / de-icing technologies to suppress ice accumulation while removing ice from the surface.
[0003] Superhydrophobic surfaces are an effective way to delay the freezing time. This is based on the presence of an air layer within the surface texture, which can greatly reduce the contact area between water droplets and solid substrates. Making photothermal materials into superhydrophobic coatings can effectively convert solar energy into heat and promote ice removal without the need for additional energy input. For example, a black superhydrophobic surface technology was prepared on carbon steel by combining multi-pulse laser ablation and hexadecyltrimethoxysilane chemical modification. Compared with the bare carbon steel substrate, the obtained coating with a water contact angle (WCA) of 156° had a longer freezing time and three times smaller deicing force. A fully water-based superhydrophobic coating was constructed using carbon nanotubes, polydopamine and silver particles as photothermal materials, and then mixed with a fluorinated polyacrylic acid emulsion. Under xenon lamp irradiation, the ice melting time of the coating was reduced by 982 seconds compared to the original surface. Although a variety of anti-icing and deicing strategies have been proposed in recent years, the poor durability, single function, use of fluorinated materials and complex preparation technology of photothermal superhydrophobic coatings have seriously hindered their practical application under harsh conditions. Summary of the invention
[0004] In order to make up for the deficiencies of the prior art, the present invention provides a fluorine-free super-hydrophobic micro-nanostructured SiO2 / TiN anti-icing and photothermal deicing coating.
[0005] The present invention is achieved through the following technical solutions:
[0006] A fluorine-free super-hydrophobic micro-nanostructured SiO2 / TiN anti-icing and photothermal deicing coating, wherein the coating is prepared by the following method:
[0007] Step 1: dispersing TiN nanospheres and SiO2 microspheres in a mixture of 3-(isobutyleneoxy)propyltrimethoxysilane KH-570, ethanol and H2O under magnetic stirring, and adjusting the pH to 4.0-5.0 with acetic acid to obtain a mixture;
[0008] Step 2: The mixture obtained in step 1 was reacted at 60° C. for 2.0 hours under stirring, and the solution was purified by centrifugation and washed with ethanol;
[0009] Step 3: The product obtained in step 2 is dispersed in ethanol, and then mixed with octadecyl methacrylate SMA and 2,2'-azobisisobutyronitrile AIBN, and the polymerization process is carried out at 60° C. with stirring for 2.0 h to obtain modified particles;
[0010] Step 4: The photothermal superhydrophobic coating was prepared by two-step spraying technology using different proportions of modified particles and E-51-based adhesive.
[0011] Furthermore, in step 1, the mass of TiN nanospheres is 3.0 g, the mass of SiO2 microspheres is 2.0 g, the volume of 3-(isobutyleneoxy)propyltrimethoxysilane KH-570 is 5.0 mL, the volume of ethanol is 22.0 mL, and the volume of H2O is 2.0 mL.
[0012] Furthermore, in step 3, the volume of ethanol is 20.0 mL, the volume of octadecyl methacrylate SMA is 3.0 mL, and the mass of 2,2'-azobisisobutyronitrile AIBN is 0.05 g.
[0013] Further, in step 4, the photothermal superhydrophobic coating preparation method is as follows: first, the modified particles, ethanol and E-51-based adhesive are mixed and stirred for 5 minutes to form a uniform solution; then the above solution is sprayed on a glass substrate and cured at 80°C for 3.0 minutes. Then, a uniform mixture of 0.066g of E-51-based adhesive and 3.0mL of modified particles is covered on the coating surface by secondary spraying and cured at 120°C for 6.0h.
[0014] Further, the modified particles were 0.9 mL, ethanol was 2.1 mL, and the E-51-based binder was 0.972 g.
[0015] Furthermore, the modified particles have a particle content of 15.1 wt%, m SiO2 / m TiN It is 3 / 2, and the superhydrophobic ability is the best.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] (1) A fluorine-free photothermal superhydrophobic SiO2 / TiN coating was successfully developed by a facile polymerization and spraying technique. After a series of durability tests such as etching and wear tests under harsh environments, the obtained coating can still maintain good superhydrophobicity due to its excellent mechanical and chemical stability. In addition, the coating also exhibits good anti-icing ability and excellent photothermal effect. Compared with ordinary sunlight irradiation conditions, the freezing time of water droplets can be extended by 3.6 times, while the surface temperature can be increased to 133.8℃ on the bare substrate. The coating can still maintain superhydrophobicity after 500 freezing / thawing cycles, and has good self-cleaning effect and corrosion resistance. The good anti-icing and de-icing ability is mainly attributed to the superhydrophobic surface produced by the micro-nano hierarchical structure and low surface energy chemical modification and the photothermal effect of TiN nanoparticles. Thanks to the strong mechanical and chemical stability, this study provides a promising anti-icing / de-icing coating for large-scale practical applications.
[0018] (2) The present invention effectively integrates passive deicing and active anti-icing capabilities into a fluorine-free photothermal superhydrophobic coating through a simple polymerization and two-step spraying process. The SiO2 / TiN mixture has a distinct micro-nanostructure and excellent superhydrophobic properties. Under simulated sunlight irradiation conditions, the coated aluminum plate can achieve more than 90% solar light absorption and produce a significant temperature rise of 105.5°C within 5 minutes. In addition, the synthesized superhydrophobic coating exhibits excellent resistance to tape peeling, Taber abrasion, solution immersion, and ice / thaw cycle tests. Self-cleaning and corrosion resistance further contribute to its long-term outdoor application. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The present invention will be further described below in conjunction with the accompanying drawings.
[0020] Figure 1 Schematic diagram of the preparation process of superhydrophobic photothermal SiO2 / TiN coating;
[0021] Figure 2 XPS measurement spectra and high-resolution C1s spectra of original particles, alkylated particles and modified particles; (a) XPS measurement spectra of original particles, alkylated particles and modified particles; (b) high-resolution C1s spectra of original particles, alkylated particles and modified particles;
[0022] Figure 3 High-resolution N1s, Si 2p, Ti 2p, and O1s spectra of modified particles;
[0023] Figure 4 SEM images at different magnifications and the corresponding Si and Ti element mapping images, cross-sectional SEM of the obtained superhydrophobic coating and the corresponding Ti element mapping images;
[0024] Figure 5WCA and WRA bar graphs and m of water droplets when the particle content is 3.4%, 9.7%, 15.1% and 20.0% respectively SiO2 / m TiN The WCA and WRA of the water droplet at 1 / 1, 6 / 5, 3 / 2, 2 / 1, and 3 / 1 respectively;
[0025] Figure 6 Superhydrophobicity of the coating; (a) WCA and WRA of various liquids, including HCl solution (pH = 1.0), NaOH solution (pH = 14.0), NaCl solution (0.1M), milk, tea and coffee on the coating surface; (b) The bouncing process of water droplets on the coating surface captured by a high-speed camera
[0026] Figure 7-15 Freezing process of water droplets on bare and coated aluminum plates at ℃;
[0027] Figure 8 The force required to remove a 1cm×1cm×1cm ice cube from the Al sheet and SiO2 / TiN coating surface versus time.
[0028] Fig. 9 Absorption spectra and light reflectance spectra of bare glass, original glass coated with SiO2 coating only, and SiO2 / TiN coating;
[0029] Fig.10 Photothermal effect of coatings; (a) Temperature change of bare aluminum plate and SiO2 / TiN coated aluminum plate under xenon lamp irradiation for 5 minutes; (b) Temperature change curve of bare glass and coated glass under xenon lamp irradiation for 6 minutes; (c) Temperature difference between coated glass with different TiN mass ratios and bare glass under xenon lamp irradiation for 5 minutes;
[0030] Fig.11 Actual deicing experiment on bare glass and coated glass at 0℃ outdoors in Jinan;
[0031] Fig.12 WCA of water droplets after the coating is immersed in different liquids for different time periods;
[0032] Fig.13 Changes in WCA and WRA of water droplets on the coating surface under different Taber abrasion test cycles under 250g load;
[0033] Fig.14 Adhesion test of coatings; (a) Comparison of optical photographs of the top coating (left) and double coating (right) after tape peeling test; (b) Adhesion of coatings to various substrates;
[0034] Fig.15 Changes in WCA and WRA of water droplets on coating surfaces during icing / deicing cycles;
[0035] Fig.16 Self-cleaning performance test using sand to simulate pollutants;
[0036] Fig.17 The anti-corrosion effect of the coating; (a) Surface morphology changes of the coated copper plate and the bare copper plate during 300 hours of salt spray corrosion; (b) Tafel polarization curves of the bare copper sheet and the coated copper sheet before and after corrosion at different times;
[0037] Fig.18 EIS of coated copper and bare copper before and after corrosion at different times. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with the embodiments.
[0039] Example 1
[0040] Experimental materials and instruments
[0041] Table 1 Main raw materials and reagents
[0042]
[0043]
[0044] Table 2 Main experimental instruments and equipment
[0045]
[0046] Example 2
[0047] Experimental preparation method
[0048] TiN nanospheres (3.0 g) and SiO2 microspheres (2.0 g) were dispersed in a mixture of 3-(isobutyleneoxy)propyltrimethoxysilane (KH-570) (5.0 mL), 22.0 mL ethanol and 2.0 mL H2O under magnetic stirring, and the pH was adjusted to 4.0-5.0 with acetic acid. The mixture was reacted at 60°C for 2.0 hours under stirring. The above solution was purified by centrifugation and washed with ethanol. Then, the product was dispersed in 20.0 mL ethanol and then mixed with 3.0 mL octadecyl methacrylate (SMA) and 0.05 g 2,2'-azobisisobutyronitrile (AIBN). The polymerization process was carried out at 60°C with stirring for 2.0 hours to obtain modified particles.
[0049] A photothermal superhydrophobic coating was prepared by two-step spraying technology using modified particles and E-51-based adhesive in different proportions. First, 0.9 mL of modified particles, 2.1 mL of ethanol and 0.972 g of E-51-based adhesive were mixed and stirred for 5 minutes to form a uniform solution. The above solution was then sprayed on a glass substrate (25 cm × 75 cm) and cured at 80 ° C for 3.0 min. Then, a uniform mixture of 0.066 g of E-51-based adhesive and 3.0 mL of modified particles was covered on the coating surface by secondary spraying and cured at 120 ° C for 6.0 h.
[0050] Example 3
[0051] Testing and Characterization
[0052] The surface morphology and element distribution were characterized by a Hitachi field emission scanning electron microscope (FE-SEM) Regulus 8220 equipped with an energy dispersive spectrometer (EDS). X-ray photoelectron spectroscopy (XPS) measurements were performed on a Thermo Fisher Scientific EscaLab Xi+ spectrometer with Al Kα X-rays as the light source. Fourier transform infrared (FTIR) spectra were collected on a Nicolet IS20 spectrometer (Thermo Fisher Scientific Inc., Waltham, MA, USA) in the range of 4000–400 cm -1 Optical absorption and reflectance spectra were collected on an Agilent Cary 7000 UV-Vis-NIR spectrophotometer.
[0053] Ice adhesion strength test
[0054] The adhesion strength of ice was analyzed by measuring the shear strength required to remove ice cubes from the coating using a dynamometer. Initially, water was placed in a 2.0 cm × 2.0 cm × 2.0 cm mold and frozen into ice cubes. The ice cubes were then placed on the coating surface and placed in a -15°C freezer for 12 hours.
[0055] Anti-icing performance test
[0056] The static anti-icing performance was evaluated by the freezing time of water droplets at an ambient humidity of 30 ± 2%. First, the bare and coated aluminum plates were placed on prefabricated ice blocks at -15 °C to simulate a cold environment. Then, 50 μL of water droplets were dropped on the coating surface and the crystallization process was studied by digital microscopy. The time it takes for the water droplet to transform from the liquid phase to the solid phase is defined as the freezing time.
[0057] Dynamic anti-icing tests were conducted in a high-low temperature / humidity test chamber under the condition of 30±2% ambient humidity. Initially, bare and coated aluminum sheets were placed at an inclination angle of 5° and a 1mL water droplet was formed on the surface. Subsequently, the chamber was cooled from 0°C every 10°C until the temperature reached -70°C and maintained for 30 minutes to ensure that the water droplets were completely transformed into ice cubes. The ice cubes at each temperature were weighed for comparison.
[0058] Photothermal deicing performance test
[0059] Under the conditions of ambient temperature 25±2℃ and relative humidity 30±2%, the photothermal deicing performance is evaluated by the time it takes for ice to slide off the surface under simulated sunlight 14cm above the substrate. 2 The simulated sunlight intensity is generated by a xenon lamp (PLS-SXE300 / 300UV). An infrared imaging thermometer is used to evaluate surface temperature changes.
[0060] Mechanical durability testing
[0061] The wear resistance of the coating was evaluated using a Taber abrasion tester under a load of 250 g. The sample was first sprayed on a glass substrate with a diameter of 10 cm and then fixed on a rotating platform. The rotation speed was set to 79 rpm / min. WCA and WRA were recorded after every 20 cycles.
[0062] The surface adhesion of the coating to various substrates was measured using an XH-M adhesion tester. In addition, the bonding strength was further measured by a tape test according to ASTM D3359. Prior to this, the samples were cut vertically into 1 mm squares using a grid knife. 2 100 squares of 3M tape were then compressed under a 2kg load and then peeled off to observe the peeling condition.
[0063] For the tape peel test, stick the 3M tape on the coating surface and press it with your thumb. After that, roll a 750-gram weight on the surface to ensure good contact with the coating, and then peel off the glue from one end. Repeat the above process, record the corresponding WCA and WRA after every 50 cycles of testing, and replace with new tape after every 10 cycles.
[0064] Chemical stability, self-cleaning and corrosion resistance testing
[0065] The coated glass plates were immersed in HCl solution (pH=1), NaOH solution (pH=14), NaCl solution (0.1 M) and various organic solvents (e.g. DMF, THF, DMSO, acetone, respectively). After every six days, the samples were taken out, cleaned and dried to measure WCA and WRA.
[0066] To examine the self-cleaning properties of the samples, sand was used to simulate contaminants. A glass substrate (25 mm x 75 mm) was tilted in a petri dish and covered with sand in a random pattern.
[0067] The corrosion resistance of the coating was evaluated by the copper accelerated acetic acid salt spray test (CASS) in a salt spray test chamber. Acetic acid was added to a 5wt% NaCl solution, the pH of the corrosion solution was adjusted to 2-3, and anhydrous CuCl2 was used to 2+ The concentration was adjusted to 0.26 g L -1 The temperature and humidity in the chamber were set to 35 °C and 95%, and the spray rate was maintained at 1.5 mL·h -1 cm -2 .
[0068] The electrochemical tests were carried out on an electrochemical analyzer (CHI 660E, Shanghai Chenhua) with a standard three-electrode system, including a platinum sheet as the counter electrode, a saturated calomel electrode (SCE) as the reference electrode, and a coated aluminum sheet (6 cm × 6 cm) as the working electrode. The electrochemical impedance spectroscopy (EIS) was performed in a 5.0 wt% NaCl solution at a frequency of 0.1 Hz to 10 6 The open circuit potential in the Hz range was measured with an amplitude of 20 mV. The Tafel curve was measured in 5.0 wt% NaCl solution at a scan rate of 10 mV / s.
[0069] Example 4
[0070] Coating preparation process
[0071] Figure 1The synthesis process of superhydrophobic photothermal coating is demonstrated. First, SiO2 microspheres and TiN nanoparticles are chemically modified by hydrolysis condensation reaction using KH-570. The hydrolysis product of KH-570 in acidic medium can react with the hydroxyl groups on the surface of SiO2 microspheres and TiN nanoparticles to form alkylated particles. Subsequently, AIBN is used as an initiator to graft the superhydrophobic alkyl chain of SMA to the particle surface through double bond polymerization reaction. Surface roughness and low surface energy are two key factors for superhydrophobicity. Generally speaking, larger surface roughness and lower surface energy are conducive to obtaining higher superhydrophobicity. By combining micron-sized particles with nano-sized particles, suitable roughness can be obtained to create a superhydrophobic surface. In this work, SiO2 microspheres and TiN nanoparticles can form a hierarchical rough structure to provide surface roughness, and chemical modification of SMA can reduce the surface energy of the particles. During the synthesis of the E-51-based adhesive, the amino groups of KH-550 can react with the epoxy groups of E-51 through the ring-opening reaction of E-51 with KH-550, thereby enhancing the adhesion between the E-51 layer and the modified particles. Subsequently, coatings with different ratios of modified particles and E-51-based adhesive were sprayed onto the glass substrate in sequence, wherein the upper and lower layers were composed mainly of modified particles and E-51-based adhesive, respectively.
[0072] Structural and compositional characterization of coatings
[0073] XPS spectroscopy was used to analyze the surface composition of the original particles, KH-570 alkylated particles, and KH-570 and SMA modified particles. All XPS spectra showed obvious C1s, O 1s, N 1s, Si 2p, and Ti 2p signals ( Figure 2 a) After hydrolysis and polycondensation with KH-570, the surface O atom ratio increased from 36.7% to 42.1%. At the same time, due to the long alkyl group of SMA, the C atom ratio increased significantly from 31.2% to 89.5%. Figure 2 b shows the high-resolution C1s spectra of the three samples. All C1s spectra were fitted to three peaks assigned to -CC-, -CO-, and -C=O bonds. The -CC- bond originates from the carbon chain or alkyl group in KH-570 and SMA, while the -CO- and -C=O bonds originate from the ester group in KH-570 and SMA. Compared with the original particles, the -C=O peak percentage in the alkylated particles increased slightly, while the -CC- peak percentage further increased from 64.3% to 88.4% after grafting SMA. The surface chemical state of the modified particles was further analyzed by XPS ( Figure 3). The high-resolution N1s XPS spectrum is decomposed into two peaks associated with N-Ti bonds (397.0 eV) and N-Ti-O bonds (395.8 eV), respectively. The high-resolution Si 2p spectrum is associated with Si-O bonds and Si-C bonds, respectively, indicating the presence of SiO2 microspheres and KH-570. The high-resolution Ti 2p XPS spectrum of the modified particles is divided into two doublets (Ti 2p 1 / 2 and Ti 2p 3 / 2 ). The peaks at 463.7eV and 458.2eV are attributed to Ti-O bonds, while the peaks at 462.0eV and 456.7eV are attributed to Ti-NO bonds, and the peaks at 460.4eV and 455.2eV are attributed to Ti-N bonds. In addition, O-Ti bonds and O-Si bonds appear in the high-resolution O1s XPS spectrum. The above results confirm the successful modification of TiN and SiO2 particles by KH-570 and SMA.
[0074] Figure 4 The SEM and element distribution images of the superhydrophobic coating are shown. The coating exhibits a rough feature with a hierarchical micro-nanostructure. Due to the aggregation of TiN nanoparticles, abundant grains are formed. In addition, there are a large number of gaps between SiO2 microspheres and TiN nanoscale aggregates, which can provide ample space for capturing air, thus giving the coating a high superhydrophobicity. From the high-magnification SEM image, it can be seen that the surface of the SiO2 microspheres is modified with some TiN nanoparticles. This structure further improves the surface roughness, resulting in superhydrophobicity. The element distribution images of Ti and Si prove the presence of SiO2 and TiN particles. The boundary between the two layers can be clearly seen from the cross-sectional SEM image, where the upper layer is rougher and is dominated by particle aggregates, while the flat bottom layer is mainly composed of E-51-based binder. From the Ti element distribution image, due to the high TiN content, the Ti element is mainly concentrated in the top layer, which is in sharp contrast to the bottom layer.
[0075] Optimization of particle content and ratio
[0076] The surface wettability of the coating was evaluated by measuring the WCA and WRA of the water droplet. In order to explore the effect of particle content on superhydrophobicity, the WCA and WRA were measured at particle contents of 3.4wt%, 9.7wt%, 15.1wt% and 20.0wt%, respectively. The results showed that WCA first increased, and when the particle percentage was 15.1wt%, WCA reached a maximum of 159.1°, and then WCA decreased with the increase of particle mass ratio, as shown in Figure 2. Figure 5As shown in the figure, when the particle content is less than 15.1wt%, water droplets easily adhere and cannot roll off the surface. When the particle percentage is 3.4wt%, the WCA of the coating is lower, which is 97°, indicating poor hydrophobicity due to the low surface roughness. When the particle content is 15.1wt%, the coating exhibits strong superhydrophobicity with a maximum WCA of 159.1° and a minimum WRA of 1.2°. Then, the effects of different SiO2 to TiN particle mass ratios (m SiO2 / m TiN ) of the coating. When m SiO2 / m TiN When the m / s ratio changes from 1 / 1 to 3 / 1, all coatings show strong hydrophobicity with WCA higher than 140°. SiO2 / m TiN When mSiO2 / mTiN is 3 / 2, the WCA reaches a maximum of 159.1° and a minimum of 1.2°, and water droplets can easily slide off the coating. When mSiO2 / mTiN is lower or higher than 3 / 2, WCA decreases and WRA increases. The differences in these coatings are mainly due to the changes in the surface micro-nano porous structure. The above results show that the particle content of 15.1wt% and m SiO2 / m TiN 3 / 2 is the best choice for super hydrophobicity.
[0077] Superhydrophobicity of coatings
[0078] In addition to water droplets, droplets of HCl solution (pH = 1.0), NaOH solution (pH = 14.0), NaCl solution (0.1 M), tea, coffee, and milk also showed almost perfect spheres. In addition, all liquids remained superhydrophobic with WCA above 150° and WRA below 5° ( Figure 6 a), indicating that the synthesized coating has excellent repellency to various liquids. As can be seen from the high-speed camera, water droplets can easily jump on the coated glass surface ( Figure 6 b).
[0079] Anti-icing properties of coatings
[0080] In order to evaluate the passive anti-icing performance of the coating, the freezing process of 50 μL water droplets on bare aluminum sheets and coated aluminum sheets at -15°C was studied using a digital magnifier. Figure 7As can be seen in the figure, when a water droplet falls on a bare aluminum sheet, the droplet spreads across the surface. Initially, the droplet is transparent, and ice grows from the bottom to the top after condensation. When the droplet begins to freeze, the surface becomes opaque due to the different reflectivity between water and ice. For the bare aluminum sheet, the droplet appears turbid at 20 seconds due to ice nucleation. Thereafter, the solid and liquid phases coexist until the droplet is completely frozen at 47 seconds. In contrast, the shape of the droplet on the coated aluminum sheet surface is close to spherical. The coated aluminum sheet begins to freeze at 40 seconds and does not freeze completely until 170 seconds. As expected, the freezing time of the droplet is effectively extended by 3.6 times, showing the good anti-icing ability of the coating. The relatively fast freezing time on the bare aluminum sheet surface is due to the direct freezing process from bottom to top at the solid-liquid contact line. For the aluminum sheet surface covered with the coating, the air layer can be trapped between the rough structure and the droplet, which reduces the solid-liquid contact area and hinders heat transfer, thereby delaying ice crystallization at the solid-liquid interface.
[0081] To judge the adhesion of the resulting coating, ice was preformed on an aluminum plate in a -15 °C refrigerator, and the adhesion strength of the ice was measured using a tensiometer at 5 °C ( Figure 8 ). The ice adhesion force on the bare aluminum sheet is as high as 660kPa, almost twice that of the coated aluminum sheet (355kPa). For the coated aluminum sheet, the required force drops to zero at 240 seconds, which means that the ice is completely detached. In contrast, the ice on the bare aluminum sheet is more difficult to remove due to its strong adhesion, and it takes about 300s to completely remove it. It is speculated that the air gap between the micro-nano structure and the water droplet significantly weakens the adhesion strength of the ice-solid interface.
[0082] De-icing properties of coatings The light-to-heat conversion effect is crucial to de-icing performance. Figure 4 As shown in the figure, compared with bare glass and glass coated with SiO2 microspheres only, the glass with superhydrophobic coating absorbs up to 90% of the light in the wavelength range of 300-2600 nm. Similarly, due to the addition of TiN nanoparticles, the light reflectivity is greatly reduced to 5% ( Fig. 9 ). Therefore, the addition of TiN nanoparticles can greatly suppress light reflectivity and increase light absorption. The high light absorption of TiN nanoparticles is conducive to improving the photothermal conversion efficiency and can quickly heat up, thereby promoting deicing. The photothermal effect of the synthetic coating was evaluated by surface temperature changes using an infrared imaging device ( Fig.10 a). It can be observed that under the irradiation of the xenon lamp, the surface temperature of the coated aluminum plate can reach 133.8℃ within 5 minutes, while the bare aluminum plate can only rise to 70.0℃. Using glass as the substrate, the surface temperature can reach 118℃ within 6.0 minutes, while the bare glass can only reach 92℃ ( Fig.10b). The above phenomenon confirms that the obtained coating has a high light-to-heat conversion efficiency. In order to clarify the key influencing factors of the photothermal effect, the temperature difference between the coated glass and the bare glass with different mass ratios of TiN nanoparticles ( Fig.10 c). As the TiN mass ratio increases from 0 to 33 wt%, the temperature rise of the glass substrate increases accordingly after 5.0 min, indicating that TiN plays a key role in maintaining the surface temperature rise. Under the irradiation of the xenon lamp, the coating heats up rapidly due to the photothermal effect of TiN. The ice adhesion is reduced, and the ice layer at the ice-solid interface will melt first, causing the ice block to slide off. As time goes on, the heat is transferred to the surrounding ice, thereby melting the entire block.
[0084] In order to simulate the photothermal deicing effect of the coating, an actual deicing experiment was carried out at an outdoor temperature of 0°C in Jinan, China. Prior to this, ice cubes of 2.0 cm × 2.0 cm × 2.0 cm were prepared using a template. Four ice cubes were frozen on the surface of the coated glass substrate and the bare glass substrate, respectively. The melting state of the ice cubes was studied and the melting time was recorded. Under solar irradiation, due to the excellent thermal conductivity of TiN nanoparticles, the ice cubes at the ice-solid interface on the coated glass began to melt at 6.5 min, and obvious sliding was observed at 6.67 min. Heat will be transferred from the photothermal zone to the surrounding coating, resulting in complete melting. In contrast, the ice cubes did not fall off from the bare glass until 10 min ( Fig.11 ).
[0085] Stability of coating
[0086] The chemical stability of superhydrophobic coatings plays a vital role in practical applications. Therefore, the chemical stability of the obtained coatings in various harsh environments was tested. Fig.12 As shown in the figure, after being immersed in strong acid / alkaline solutions (such as HCl solution (pH = 1.0), NaOH solution (pH = 14.0)), organic solvents (such as DMF, acetone, THF and DMSO) and NaCl solution (0.1M) for 30 days, the coating still maintains superhydrophobicity when WCA exceeds 150°, indicating that the coating has excellent chemical stability. The high chemical stability of this superhydrophobic coating may be due to the good chemical inertness and structural stability of the coating.
[0087] In addition to chemical stability, mechanical robustness also has a significant impact on coating life. Wear resistance tests were performed using a Taber abrasion tester under a load of 250 g. WCA and WRA were measured after every 20 cycles. Fig.13 As shown in Figure 2, after 180 wear cycles, the coating still maintains strong superhydrophobicity, with WCA higher than 150° and WRA lower than 10°. The above tests prove that the superhydrophobic coating has good mechanical strength.
[0088] To evaluate the adhesion and mechanical stability between the coating and the substrate, a tape peel test was performed. In this test, the coating was cut vertically into 100 1 mm 2 The squares were then compressed with 3 M tape under a 2 kg load and then peeled off to observe the peeling condition. Figure 5 Optical photographs of only the upper layer and two layers of coating after the tape peeling test are shown. It can be seen that the upper layer of coating suffered severe surface peeling due to weak adhesion, while no obvious structural damage was observed for the two layers of coating. In addition, the adhesion of the coating to different substrates (including copper plate, wood, aluminum plate and glass) was measured using an adhesion tester ( Fig.14 a), which is very important for broadening practical applications. In particular, the adhesion to glass substrates can reach 8.8MPa ( Fig.14 b), which means that the coating has a strong bond to the substrate.
[0089] This example further tests the durability of the superhydrophobic coating by freezing / thawing cycles. The water droplet (5 μL) is frozen in a -15°C refrigerator for 30 minutes, and then the coating with the frozen droplet is heated in a 120°C oven for 30 minutes to melt the frozen droplet. The above process is called a freeze / thaw cycle. Fig.15 As shown, WCA and WRA were recorded every 50 cycles, respectively. Even after 500 freezing / thawing cycles, the coating still exhibited strong superhydrophobicity with a WCA of 163.5° and a WRA of 3.7°, indicating that the coating has excellent anti-icing / de-icing performance.
[0090] Self-cleaning properties of coatings
[0091] Considering the practical application of the coating, the self-cleaning effect is an important feature of superhydrophobic materials to reduce contamination. The adhesion of contaminants to the coating surface is much weaker, and water flow can easily remove the dirt. During the test, sand was used to simulate contaminants. A glass substrate (25mm×75mm) was tilted in a petri dish and covered with sand. Fig.16 It can be seen in the figure that when a water droplet falls vertically on the coating surface, the water stream can easily roll off the glass surface with sand, indicating that the synthesized coating has significant self-cleaning properties.
[0092] Corrosion resistance of coating
[0093] Use salt spray test chamber to test Cu 2+ The accelerated acetic acid salt spray test was used to evaluate the anti-corrosion performance of the coating. The corrosion solution was 5.0 wt% CuCl2 and 0.26 g L -1NaCl mixture. After 300 h, the bare copper sheet was severely corroded and the surface structure was almost completely destroyed. For comparison, only a small amount of CuCl2 was deposited on the coated copper sheet ( Fig.17 a). Thanks to the protection of the super-hydrophobic coating, the copper sheet is well protected and almost not damaged. Fig.17 b shows the Tafel plots of bare copper and coated copper at different corrosion times. corr ) and corrosion current density (I corr ) can be determined by extrapolation. It is generally believed that a higher corrosion potential is associated with a lower corrosion probability and a smaller corrosion current density is associated with a slower corrosion rate. Obviously, with the increase of exposure time in the corrosive environment, the E of the bare copper plate and the coated copper plate increases. corr and I corr Compared with before exposure, the E corr The E of the coated copper plate shifted from -0.572V to -0.880V. corr is -0.162V. Therefore, the I corr The decrease was 1.52×10 -4 A and 6.28×10 -8 A. Superhydrophobic Surface I corr About four orders of magnitude smaller. corr The increase and I corr The decrease in indicates that the superhydrophobic coating can effectively enhance the corrosion resistance of the copper substrate. The excellent corrosion resistance of the synthesized coating mainly stems from the following factors. First, the air cushion trapped in the rough surface structure can prevent the coating from being penetrated by the corrosive solution. In addition, the air gap can repel the corrosive ions into the coating through the Laplace pressure. More importantly, the strong structure and composition stability of the coating can protect the copper plate substrate from corrosion.
[0094] In addition to the Tafel curve, the corrosion resistance of the coating was further analyzed by EIS. Fig.18 The evolution of the Nyquist plot of the bare copper plate and the coated copper plate under corrosion at different times is shown. Generally speaking, the larger the radius of the semicircle, the better the corrosion resistance. After 300h of corrosion test, the coated copper sheet still has the highest impedance value of 272.4Ωcm -2 , than bare copper sheet (0.25Ωcm -2 ) is two orders of magnitude higher, reflecting its excellent corrosion resistance.
Claims
1. A fluorine-free super-hydrophobic micro-nanostructured SiO 2 / TiN anti-icing and photothermal deicing coatings, It is characterized in that The coating is prepared by the following method: Step 1: Mix TiN nanospheres and SiO 2 The microspheres are dispersed in 3-(isobutyleneoxy)propyltrimethoxysilane KH-570, ethanol and H 2 O, and adjusting the pH to 4.0-5.0 with acetic acid to obtain a mixture; Step 2: The mixture obtained in step 1 was reacted at 60° C. for 2.0 hours under stirring, and the solution was purified by centrifugation and washed with ethanol; Step 3: The product obtained in step 2 is dispersed in ethanol, and then mixed with octadecyl methacrylate SMA and 2,2'-azobisisobutyronitrile AIBN, and the polymerization process is carried out at 60° C. with stirring for 2.0 h to obtain modified particles; Step 4: The photothermal superhydrophobic coating was prepared by two-step spraying technology using different proportions of modified particles and E-51-based adhesive.
2. The coating according to claim 1, It is characterized in that In step 1, the mass of TiN nanospheres is 3.0 g, and the mass of SiO 2 The mass of the microspheres was 2.0 g, the volume of 3-(isobutyleneoxy)propyltrimethoxysilane KH-570 was 5.0 mL, the volume of ethanol was 22.0 mL, and the volume of H 2 The volume of O is 2.0 mL.
3. The coating according to claim 1, It is characterized in that In step 3, the volume of ethanol is 20.0 mL, the volume of octadecyl methacrylate SMA is 3.0 mL, and the mass of 2,2'-azobisisobutyronitrile AIBN is 0.05 g.
4. The coating according to claim 1, It is characterized in that In step 4, the photothermal superhydrophobic coating preparation method is as follows: first, the modified particles, ethanol and E-51-based adhesive are mixed and stirred for 5 minutes to form a uniform solution; then the above solution is sprayed on the glass substrate and cured at 80°C for 3.0 minutes. Then, a uniform mixture of 0.066g of E-51-based adhesive and 3.0mL of modified particles is covered on the coating surface by secondary spraying and cured at 120°C for 6.0 hours.
5. The coating according to claim 4, It is characterized in that The modified particles were 0.9 mL, ethanol was 2.1 mL, and the E-51 based binder was 0.972 g.
6. The coating according to claim 4, It is characterized in that The modified particles have a particle content of 15.1wt%, m SiO2 / m TiN It is 3 / 2, and the superhydrophobic ability is the best.
Citation Information
Patent Citations
Preparation method of fluoride-free wear-resistant super-hydrophobic anti-icing coatinglayer with photothermal effect
CN114058227A
Anti-icing material with electrothermal photothermal conversion capability and wear-resistant and super-hydrophobic multiple properties as well as preparation method and application of anti-icing material
CN114656857A
Preparation method of super-hydrophobic anti-freezing polyurethane urea elastomer coating capable of being rapidly constructed in low-temperature environment
CN116535956A
Multi-scale super-hydrophobic surface with photo-thermal performance and stability and preparation method of multi-scale super-hydrophobic surface
CN117926256A
Coating composition hardly allowing icing and allowing easy deicing, coating method, and evaluation method thereof
JP2009263459A
Cited By
Fluorine-free super-hydrophobic silicon dioxide / titanium nitride coating, method and application thereof
CN121406212A
Multifunctional composite coating of OSB (oriented strand board) and preparation method of multifunctional composite coating
CN121537883A
A multifunctional composite coating for OSB substrate and its preparation method
CN121537883B