A method for preparing lithium iron phosphate / graphene oxide composite material

Through the preparation method of lithium iron phosphate/graphene oxide composite material, the poor conductivity of lithium iron phosphate materials and slow lithium ion transport in lithium batteries are solved, the compaction density and conductive properties of the materials are improved, and the lithium battery is improved comprehensive performance.

CN115924899BActive Publication Date: 2024-11-15HEBEI MILSON TITANIUM DIOXIDE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211450345.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-19
Publication Date
2024-11-15
Estimated Expiration
2042-11-19

AI Technical Summary

Technical Problem

The application of lithium iron phosphate materials in lithium batteries is limited by the problems of poor conductivity and slow lithium ion transport, resulting in poor comprehensive performance in electrochemical energy storage.

Method used

The preparation method of lithium iron phosphate/graphene oxide composite material is adopted. By reacting the iron source with polyamine oxidized cellulose under acidic conditions, adding phosphorus source and graphene oxide solution, controlling the particle size and molar ratio of the lithium source, and combining it with Electrostatic adsorption technology prepares lithium iron phosphate/graphene oxide composite materials with small particle size and high conductivity.

Benefits of technology

The compaction density and conductivity of lithium iron phosphate material are improved, its comprehensive performance in lithium batteries is enhanced, and the rate capacity and cycling performance of electrode materials are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115924899B_ABST
    Figure CN115924899B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium iron phosphate materials, and proposes a preparation method of a lithium iron phosphate / graphene oxide composite material, comprising the following steps: S1, under acidic conditions, adding polyamine oxidized cellulose to an iron source for reaction to obtain a mixture A; S2, adding a phosphorus source to the mixture A and stirring to obtain a mixture B; S3, stirring the mixture B and a graphene oxide solution to obtain a mixture C; S4, adding a lithium source to the mixture C for reaction, and uniformly mixing the solid material obtained by the reaction with a carbon source, and drying; S5, sintering, crushing, screening, and demagnetizing the dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material. Through the above technical scheme, the iron source is mixed with polyamine oxidized cellulose; the ratio of lithium and iron elements and the particle size of the lithium source are limited, the comprehensive performance of the lithium iron phosphate material in the application of lithium batteries is improved, and the problem of poor comprehensive performance of the lithium iron phosphate material applied to batteries in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium iron phosphate materials, and in particular to a method for preparing a lithium iron phosphate / graphene oxide composite material. Background Art

[0002] Lithium-ion batteries are widely used in energy storage materials due to their high energy density and stable cycle life. Currently, LiCoO2, LiVPO4F, LiMn2O4, LiFePO4, Li2FeSiO4 and LiNi1 / 3Co1 / 3Mn1 / 3O2 have attracted widespread attention as ideal materials for electrochemical energy storage. Among these promising cathode materials, olivine-structured LiFePO4 has attracted the most attention due to its good stability, excellent safety and low cost. However, poor conductivity and slow lithium ion transport are bottlenecks that seriously limit the application of LiFePO4 in lithium energy storage.

[0003] In recent years, two-dimensional graphene sheets have been widely studied as carbon materials for improving the conductivity of electrode materials due to their superior conductivity. Literature reports have shown that the addition of graphene can significantly improve the rate capacity and cycle performance of LiFePO4. However, there is still a problem that the particle size of lithium iron phosphate is large, resulting in low conductivity and low compaction density after the composite of graphene and lithium iron phosphate. Summary of the invention

[0004] The present invention provides a method for preparing a lithium iron phosphate / graphene oxide composite material, which solves the problem of poor comprehensive performance of lithium iron phosphate materials applied to batteries in the related art.

[0005] The technical solution of the present invention is as follows:

[0006] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0007] S1. Under acidic conditions, adding polyamine oxidized cellulose to an iron source for reaction to obtain a mixture A;

[0008] S2, adding a phosphorus source to the mixture A and stirring to obtain a mixture B;

[0009] S3, stirring the mixture B and the graphene oxide solution to obtain a mixture C;

[0010] S4, adding a lithium source to the mixture C for reaction, mixing the solid material obtained by the reaction with the carbon source uniformly, and drying;

[0011] S5. Sintering, crushing, screening and demagnetizing the dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material.

[0012] As a further technical solution, the polyamine oxidized cellulose includes one or more of triethylenetetramine oxidized cellulose and hexamethylenediamine oxidized cellulose.

[0013] As a further technical solution, the phosphorus source includes one or more of phosphoric acid, diammonium phosphate, and sodium phosphate; the iron source includes one or more of ferrous sulfate and ferrous chloride; and the lithium source includes one or more of lithium carbonate and lithium hydroxide.

[0014] As a further technical solution, the particle size of the lithium source is 300-400nm.

[0015] By limiting the particle size of the lithium source, the particle size of lithium iron phosphate is reduced, the compaction density can be increased, and the comprehensive performance of lithium iron phosphate materials in lithium battery applications can be improved.

[0016] As a further technical solution, the molar ratio of the iron element in the iron source, the polyamine oxidized cellulose, the phosphorus element in the phosphorus source, and the lithium element in the lithium source is 1: (1.05-1.25): (1.1-1.3): (1.5-2.5).

[0017] The ratio of lithium and iron elements is limited. The molar amount of lithium is greater than that of iron. The lithium element is divided into two parts. One part reacts with iron phosphate to synthesize lithium iron phosphate, and the other part is adsorbed on the surface of the graphene oxide base through electrostatic action, increasing the conductivity of the lithium element during the charging and discharging process.

[0018] As a further technical solution, the carbon source is 0.7-2.5% of the mass of the lithium iron phosphate / graphene oxide composite material.

[0019] As a further technical solution, the sintering in step S5 is divided into two stages. In the first stage, the temperature is increased to 400-550°C at a heating rate of 3-5°C / min and maintained for 2-3 hours. In the second stage, the temperature is increased to 650-800°C at a heating rate of 3-5°C / min and maintained for 5-7 hours.

[0020] As a further technical solution, the drying in step S4 is spray drying, the air inlet temperature is 250-300°C, and the outlet temperature is 90-110°C.

[0021] As a further technical solution, the reaction temperature in step S4 is 190-230° C. and the reaction time is 5-7 h.

[0022] As a further technical solution, the method for preparing the graphene oxide solution in step S3 is:

[0023] A1. Add graphite powder and sodium nitrate into concentrated sulfuric acid to react and obtain a mixed solution A;

[0024] A2, adding potassium permanganate to the mixed solution A for reaction, and then adding water to obtain a mixed solution B;

[0025] A3, heating the mixed solution B to 95°C for 30 min, then adding hydrogen peroxide and reacting for 15 min to obtain a mixed solution C;

[0026] A4. Add 10% hydrochloric acid solution to the mixed solution C, centrifuge and wash, disperse the solid in an equal volume of water, and ultrasonicate to obtain a graphene oxide solution.

[0027] The working principle and beneficial effects of the present invention are:

[0028] 1. The present invention adopts graphene oxide and lithium iron phosphate composite, and the surface of graphene oxide has a large number of active groups such as hydroxyl, epoxy group, carbonyl and carboxyl, wherein hydroxyl and epoxy group are located on the basal plane of graphene oxide, carbonyl and carboxyl are located at the edge of graphene oxide, and due to the hybridization mode of graphene oxide, its overall surface is negatively charged, and the iron source is mixed with polyamine cellulose oxide and then complexed, and in the subsequent mixing process with graphene oxide solution, amino and hydroxyl and carboxyl and other active groups are connected by chemical bonds, thereby fixing the iron element on the surface and edge of graphene oxide, ensuring that the iron element is dispersed on the surface of graphene oxide, and finally controlling the distribution of lithium iron phosphate on the surface of graphene oxide, controlling the particle size of lithium iron phosphate, and ensuring that lithium iron phosphate particles do not agglomerate. In the present invention, the iron source compound is chemically combined with polyamine cellulose oxide and then electrostatically adsorbed with graphene oxide, thereby improving the comprehensive performance of lithium iron phosphate material.

[0029] 2. The lithium iron phosphate graphene oxide composite material prepared in the present invention has a small particle size, which can increase the compaction density and enhance the conductive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0031] Figure 1 The discharge specific capacity of Example 1 after 100 charge and discharge cycles at different rates. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The graphene oxide solutions in Examples 1-6 of the present invention are all prepared by the following steps:

[0034] Weigh 10g of graphite powder and 10g of sodium nitrate and add them to 250mL of concentrated sulfuric acid, stir slowly, add 30g of potassium permanganate after 1h, control the temperature ≤10℃, react for 2h, and obtain a mixed solution. Slowly add 500mL of deionized water to the obtained mixed solution, heat the mixed solution to maintain a temperature of 95℃ and react for 30min, then add 100mL of hydrogen peroxide, react for 15min, and then add 300mL of 10% hydrochloric acid solution. After low-speed centrifugal washing, disperse the solid in an equal volume of water, and ultrasonically exfoliate for 30min to obtain graphene oxide slurry.

[0035] The added amount of the graphene oxide solution in Examples 1-6 is 25%-50% of the molar amount of the polyamino compound.

[0036] Example 1

[0037] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0038] S1, mixing ferrous sulfate and dilute sulfuric acid solution, maintaining the solution pH at 2, then adding triethylenetetramine cellulose oxide and stirring evenly to obtain a mixture A;

[0039] S2, adding phosphoric acid to mixture A and stirring for 1 hour to obtain mixture B;

[0040] S3, mixing the mixture B and the graphene oxide solution in a reaction tank, and stirring for 0.5 h to obtain a mixture C;

[0041] S4, adding lithium hydroxide to the mixture C and heating to 190°C, reacting for 6 hours, cooling to room temperature for solid-liquid separation, mixing the solid material obtained by the reaction with glucose accounting for 0.7% of the weight of the composite material, and spray drying; the spray drying inlet temperature is 250°C, and the outlet temperature is 90°C; the particle size of the lithium hydroxide is 300-330nm;

[0042] S5, sintering, crushing, screening and demagnetizing the spray-dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; the sintering is divided into two stages, the first stage has a heating rate of 3°C / min, the temperature is raised to 400°C, and maintained for 2 hours, and the second stage has a heating rate of 3°C / min, the temperature is raised to 650°C, and maintained for 5 hours;

[0043] Among them, the molar ratio of iron in ferrous sulfate, triethylenetetramine cellulose oxide, phosphorus in phosphoric acid, and lithium in lithium hydroxide is 1:1.05:1.3:2.5.

[0044] Example 2

[0045] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0046] S1, mixing ferrous chloride and dilute sulfuric acid solution, maintaining the solution pH at 2, then adding hexamethylenediamine oxidized cellulose and stirring evenly to obtain a mixture A;

[0047] S2, adding ammonium dihydrogen phosphate to mixture A and stirring for 1 hour to obtain mixture B;

[0048] S3, mixing the mixture B and the graphene oxide solution in a reaction tank, and stirring for 0.5 h to obtain a mixture C;

[0049] S4, adding lithium carbonate to the mixture C and heating to 190°C, reacting for 7 hours, cooling to room temperature for solid-liquid separation, mixing the solid material obtained by the reaction with glucose accounting for 0.8% of the weight of the composite material, and spray drying; the spray drying inlet temperature is 270°C, and the outlet temperature is 100°C; the particle size of the lithium carbonate is 330-350nm;

[0050] S5, sintering, crushing, screening and demagnetizing the spray-dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; the sintering is divided into two stages, the first stage has a heating rate of 4°C / min, the temperature is raised to 500°C, and maintained for 3 hours, and the second stage has a heating rate of 4°C / min, the temperature is raised to 700°C, and maintained for 6 hours;

[0051] Among them, the molar ratio of iron in ferrous chloride, hexamethylenediamine oxidized cellulose, phosphorus in diammonium dihydrogen phosphate, and lithium in lithium carbonate is 1:1.05:1.1:1.5.

[0052] Example 3

[0053] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0054] S1, mixing ferrous chloride and dilute sulfuric acid solution, maintaining the solution pH at 2, then adding hexamethylenediamine oxidized cellulose and stirring evenly to obtain a mixture A;

[0055] S2, adding sodium phosphate to mixture A and stirring for 1 hour to obtain mixture B;

[0056] S3, mixing the mixture B and the graphene oxide solution in a reaction tank, and stirring for 0.5 h to obtain a mixture C;

[0057] S4, adding lithium carbonate to the mixture C and heating to 200°C, reacting for 5 hours, cooling to room temperature for solid-liquid separation, mixing the solid material obtained by the reaction with 2.5% glucose by weight of the composite material, and spray drying; the spray drying inlet temperature is 300°C, and the outlet temperature is 110°C; the particle size of the lithium carbonate is 350-400nm;

[0058] S5, sintering, crushing, screening and demagnetizing the spray-dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; the sintering is divided into two stages, the first stage has a heating rate of 5°C / min, the temperature is raised to 550°C, and maintained for 3 hours, and the second stage has a heating rate of 5°C / min, the temperature is raised to 800°C, and maintained for 7 hours;

[0059] Among them, the molar ratio of iron in ferrous chloride, hexamethylenediamine oxidized cellulose, phosphorus in sodium phosphate, and lithium in lithium carbonate is 1:1.15:1.2:1.7.

[0060] Example 4

[0061] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0062] S1, mixing ferrous sulfate and dilute sulfuric acid solution, maintaining the solution pH at 2, then adding hexamethylenediamine oxidized cellulose and stirring evenly to obtain a mixture A;

[0063] S2, adding sodium phosphate to mixture A and stirring for 1 hour to obtain mixture B;

[0064] S3, mixing the mixture B and the graphene oxide solution in a reaction tank, and stirring for 0.5 h to obtain a mixture C;

[0065] S4, adding lithium carbonate to the mixture C and heating to 230°C, reacting for 5 hours, cooling to room temperature for solid-liquid separation, mixing the solid material obtained by the reaction with 1.5% of glucose by weight of the composite material, and spray drying; the spray drying inlet temperature is 300°C, and the outlet temperature is 110°C; the particle size of the lithium carbonate is 370-350nm;

[0066] S5, sintering, crushing, screening and demagnetizing the spray-dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; the sintering is divided into two stages, the first stage has a heating rate of 5°C / min, the temperature is raised to 500°C, and maintained for 3 hours, and the second stage has a heating rate of 5°C / min, the temperature is raised to 760°C, and maintained for 7 hours;

[0067] Among them, the molar ratio of iron in ferrous chloride, hexamethylenediamine oxidized cellulose, phosphorus in sodium phosphate, and lithium in lithium carbonate is 1:1.25:1.3:2.5.

[0068] Example 5

[0069] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0070] S1, mixing ferrous chloride and dilute sulfuric acid solution, maintaining the solution pH at 2, then adding triethylenetetramine cellulose oxide and stirring evenly to obtain a mixture A;

[0071] S2, adding sodium phosphate to mixture A and stirring for 1 hour to obtain mixture B;

[0072] S3, mixing the mixture B and the graphene oxide solution in a reaction tank, and stirring for 0.5 h to obtain a mixture C;

[0073] S4, adding lithium carbonate to the mixture C and heating to 230°C, reacting for 5 hours, cooling to room temperature for solid-liquid separation, mixing the solid material obtained by the reaction with glucose accounting for 2.0% of the weight of the composite material, and spray drying; the spray drying inlet temperature is 280°C, and the outlet temperature is 105°C; the particle size of the lithium carbonate is 350-400nm;

[0074] S5, sintering, crushing, screening and demagnetizing the spray-dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; the sintering is divided into two stages, the first stage has a heating rate of 3°C / min, the temperature is raised to 500°C, and maintained for 3 hours, and the second stage has a heating rate of 5°C / min, the temperature is raised to 780°C, and maintained for 7 hours;

[0075] Among them, the molar ratio of iron in ferrous chloride, hexamethylenediamine oxidized cellulose, phosphorus in sodium phosphate, and lithium in lithium carbonate is 1:1.25:1.3:2.5.

[0076] Example 6

[0077] A method for preparing a lithium iron phosphate / graphene oxide composite material comprises the following steps:

[0078] S1, mixing ferrous chloride and dilute sulfuric acid solution, maintaining the solution pH at 2, then adding triethylenetetramine cellulose oxide and stirring evenly to obtain a mixture A;

[0079] S2, adding sodium phosphate to mixture A and stirring for 1 hour to obtain mixture B;

[0080] S3, mixing the mixture B and the graphene oxide solution in a reaction tank, and stirring for 0.5 h to obtain a mixture C;

[0081] S4, adding lithium carbonate to the mixture C and heating to 220°C, reacting for 5 hours, cooling to room temperature for solid-liquid separation, mixing the solid material obtained by the reaction with glucose accounting for 1.6% of the weight of the composite material, and spray drying; the spray drying inlet temperature is 280°C, and the outlet temperature is 105°C; the particle size of the lithium carbonate is 350-380nm;

[0082] S5, sintering, crushing, screening and demagnetizing the spray-dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; the sintering is divided into two stages, the first stage has a heating rate of 3°C / min, the temperature is raised to 500°C, and maintained for 3 hours, and the second stage has a heating rate of 5°C / min, the temperature is raised to 780°C, and maintained for 7 hours;

[0083] Among them, the molar ratio of iron in ferrous chloride, hexamethylenediamine oxidized cellulose, phosphorus in sodium phosphate, and lithium in lithium carbonate is 1:1.15:1.3:2.0.

[0084] Comparative Example 1

[0085] Compared with Example 1, Comparative Example 1 does not add graphene oxide, and the rest is the same as Example 1.

[0086] Comparative Example 2

[0087] Compared with Example 1, in Comparative Example 2, graphene oxide is replaced with an equal amount of graphene, and the rest is the same as Example 1.

[0088] Comparative Example 3

[0089] Compared with Example 1, Comparative Example 3 does not add triethylenetetramine oxidized cellulose, and the rest is the same as Example 1.

[0090] Comparative Example 4

[0091] Compared with Example 1, the molar ratio of the iron element in ferrous sulfate to the lithium element in lithium hydroxide in Comparative Example 4 is 1:1, and the others are the same as Example 1.

[0092] Comparative Example 5

[0093] Compared with Example 1, the molar ratio of the iron element in ferrous sulfate and the lithium element in lithium hydroxide in Comparative Example 5 is 1:3, and the others are the same as Example 1.

[0094] The lithium iron phosphate materials prepared in the above Examples 1-6 and Comparative Examples 1-5 were used as raw materials to prepare lithium iron phosphate positive electrode sheets, and their performance was measured. The measurement results are shown in Table 1.

[0095] Determination method: Add organic solvent NMP to lithium iron phosphate material, PVDF and acetylene black in a mass ratio of 90:5:5, mix and slurry, mix at a speed of 400 rpm, and evenly coat the electrode material on the aluminum foil current collector; vacuum dry at 80°C until the solvent evaporates, and finally press with a tablet press at a pressure of 15 MPa for 1 min to obtain a positive electrode sheet.

[0096] The above positive electrode sheet was used as the positive electrode, the metal lithium sheet was used as the negative electrode, the microporous polypropylene membrane was used as the separator, and 1M LiPF6

[0097] (using a mixture of EC and EMC in a volume ratio of 3:7 as solvent) as the electrolyte, the assembly was carried out in a glove box filled with inert gas to form a button half-cell.

[0098] The test temperature was 25.0℃, the charge and discharge voltage was 2.5V~4.5V, and the button battery was subjected to cyclic charge and discharge tests. The charge and discharge rates were 0.1C, 0.2C, 1C, 5C, 10C, 20C and 50C, and the charge and discharge test was performed 100 times at a rate of 1C.

[0099] Table 1 Measurement results

[0100]

[0101]

[0102] Compared with Example 1, the comparative example does not add graphene oxide, the comparative example 2 replaces the graphene oxide with an equal amount of graphene, and the comparative example 3 does not add polyamine oxidized cellulose. As can be seen from Table 1, the electrochemical performance of the button-type batteries assembled from the lithium iron phosphate materials prepared in Comparative Examples 1-3 is lower than that of Example 1. This indicates that the electrochemical performance of the button-type batteries assembled by selecting graphene oxide and lithium iron phosphate for compounding and adding polyamine oxidized cellulose can improve the electrochemical performance of the button-type batteries assembled. Comparative Examples 4 and 5 changed the molar ratio of iron to lithium, and the electrochemical performance of the button-type batteries assembled from the composite materials obtained decreased. Figure 1 The discharge specific capacity of Example 1 after 100 charge and discharge cycles at different rates.

[0103] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a lithium iron phosphate / graphene oxide composite material, characterized in that: The following steps are involved: S1. Under acidic conditions, adding polyamine oxidized cellulose to an iron source for reaction to obtain a mixture A; S2, adding a phosphorus source to the mixture A and stirring to obtain a mixture B; S3, stirring the mixture B and the graphene oxide solution to obtain a mixture C; S4, adding a lithium source to the mixture C for reaction, mixing the solid material obtained by the reaction with the carbon source uniformly, and drying; S5, sintering, crushing, screening and demagnetizing the dried material in S4 to obtain a lithium iron phosphate / graphene oxide composite material; The polyamine oxidized cellulose includes one or more of triethylenetetramine oxidized cellulose and hexamethylenediamine oxidized cellulose; The molar ratio of the iron element in the iron source, the polyamine oxidized cellulose, the phosphorus element in the phosphorus source, and the lithium element in the lithium source is 1: (1.05-1.25): (1.1-1.3): (1.5-2.5); The phosphorus source includes one or more of phosphoric acid, diammonium phosphate, and sodium phosphate; the iron source includes one or more of ferrous sulfate and ferrous chloride; the lithium source includes one or more of lithium carbonate and lithium hydroxide; The particle size of the lithium source is 300-400nm; The carbon source is 0.7-2.5% of the mass of the lithium iron phosphate / graphene oxide composite material; The sintering in step S5 is divided into two stages. In the first stage, the temperature is increased to 400-550°C at a heating rate of 3-5°C / min and maintained for 2-3 hours. In the second stage, the temperature is increased to 650-800°C at a heating rate of 3-5°C / min and maintained for 5-7 hours.

2. The method for preparing a lithium iron phosphate / graphene oxide composite material according to claim 1, characterized in that: The drying in step S4 is spray drying, the air inlet temperature is 250-300°C, and the outlet temperature is 90-110°C.

3. The method for preparing a lithium iron phosphate / graphene oxide composite material according to claim 1, characterized in that: In step S4, the reaction temperature is 190-230° C. and the reaction time is 5-7 h.

4. The method for preparing a lithium iron phosphate / graphene oxide composite material according to claim 1, characterized in that: The preparation method of the graphene oxide solution in step S3 is: A1. Add graphite powder and sodium nitrate into concentrated sulfuric acid to react and obtain a mixed solution A; A2, adding potassium permanganate to the mixed solution A for reaction, and then adding water to obtain a mixed solution B; A3, heating the mixed solution B to 95°C for 30 min, then adding hydrogen peroxide and reacting for 15 min to obtain a mixed solution C; A4. Add 10% hydrochloric acid solution to the mixed solution C, centrifuge and wash, disperse the solid in an equal volume of water, and ultrasonicate to obtain a graphene oxide solution.