A kind of extended chain crystalline nonwoven fabric and its manufacturing method and application
By adding small molecule crystal channel structure to the spinning liquid, the conformation of polymer crystals is regulated, and the problems of poor thermal stability and low mechanical properties of nonwovens are solved, and high-performance linear crystalline nonwovens are realized. Preparation and application.
Patent Information
- Application Number
- CN202310008787.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-01-04
AI Technical Summary
The existing nonwoven fabrics have poor thermal stability and low mechanical properties, especially folded chain crystalline polymer nonwoven fabrics cannot form high-performance straight-chain crystal structures.
Small molecules with pore structure are added to the spinning liquid of traditional flash spinning, and the polymer crystal conformation is regulated through the small molecule crystal channel to prepare composite fibers containing small molecules and polymers, and then a straightening process is made by hot pressing. Chain crystal non-woven fabric.
It significantly improves the temperature resistance and mechanical properties of non-woven fabrics, forming high-performance straight-chain crystal non-woven fabrics, suitable for medical protection, printing, construction and other fields.
Smart Images

Figure CN115976738B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an extended chain crystalline nonwoven fabric and a manufacturing method and application thereof, belonging to the technical field of nonwoven fabrics. Background Art
[0002] Non-woven fabrics are moisture-proof, breathable, flexible, lightweight, non-toxic and odorless, inexpensive, and recyclable. They can be used in different industries such as sound insulation, heat insulation, electric heaters, masks, clothing, medical treatment, filling materials, etc.
[0003] The crystal structure of non-woven fabrics prepared by traditional spunlace, spunbond, meltblown, flash evaporation and other methods is composed of folded chain lamellae, and there are a large number of amorphous regions between the lamellae, which makes the modulus, strength and thermal stability of non-woven fabrics much lower than other materials. In the straight chain crystal, the molecular chains are unfolded and stacked in parallel, and the thickness of the lamellae is basically equal to the length of the straightened molecular chain. This highly regular internal structure makes the polymer have the characteristics of high crystallinity, high strength, good mechanical properties and excellent thermal properties.
[0004] Chinese patent CN102224282A can prepare ultra-high molecular weight polyethylene fibers with extended chain crystals through sol-gel spinning and high-multiple drawing, but medium and low molecular weight polymers cannot form a gel system and extended chain crystals cannot be prepared by this method. Currently, there is no method to prepare non-woven fabrics with extended chain crystals.
[0005] Chinese patent CN106519261A regulates the crystal structure of the polymer by using urea inclusion compound and prepares polymer extended chain crystals under low pressure. However, this method can only prepare polymer extended chain crystals under low pressure. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides an extended chain crystalline non-woven fabric and a method for manufacturing the same and an application thereof; small molecules having a pore structure in the crystal are added to the spinning solution of traditional flash spinning to obtain polymer / small molecule fibers containing small molecules and polymers; the pores of the small molecule crystals are used to regulate the crystal conformation of the polymer to obtain a non-woven fabric of extended chain crystals, thereby improving the temperature resistance and mechanical properties of the non-woven fabric and solving the problems of poor thermal stability and low mechanical properties of the folded chain crystalline polymer non-woven fabric.
[0007] The technical solution of the present invention to solve the above technical problem is as follows: a method for manufacturing an extended chain crystalline non-woven fabric, the manufacturing method comprising the following steps:
[0008] S1. Preparation of spinning solution: dissolving polymer and small molecules in a solvent under high temperature and high pressure to obtain a uniform spinning solution; after the small molecules are crystallized, a hollow channel structure can be formed inside the crystal, and the pore size of the hollow small molecule crystal is less than 10 angstroms, which can accommodate a single polymer molecular chain;
[0009] S2, preparation of polymer / small molecule fibers: the spinning solution obtained in step S1 is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret, the solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers;
[0010] S3, preparation of composite non-woven fabric: the polymer / small molecule fiber obtained in step S2 is composed of a polymer guest and a small molecule host, wherein a single molecular chain of the polymer is confined in the pores of the small molecule crystal, and the polymer / small molecule fiber is divided into filaments, laid out, and subjected to primary hot pressing to obtain a composite non-woven fabric;
[0011] S4. Preparation of extended chain crystalline nonwoven fabric: removing small molecules from the composite nonwoven fabric obtained in step S3, and obtaining a high-performance nonwoven fabric of extended chain crystalline form through secondary hot pressing.
[0012] Furthermore, in step S1, the polymer is one or a combination of polyethylene, polypropylene, halogenated polyethylene, halogenated polypropylene, polyamide, polyester, polyoxymethylene, polyketone, and polyether.
[0013] Furthermore, in step S1, after the small molecule is crystallized, the crystal has a narrow pore structure inside. The small molecule is selected from one or a combination of urea, cyclodextrin, thiourea, methyl urea, dimethyl urea, trimethyl urea, tetramethyl urea, and p-nitrophenol. After the small molecule is crystallized, a narrow pore with a pore size of less than 10 angstroms can be formed inside the crystal to accommodate a single polymer molecular chain.
[0014] Furthermore, in step S1, the solvent is one or more of water, alcohol, acid, amine, ester, ether, ketone, nitrile, amide, halogenated hydrocarbon, aliphatic hydrocarbon, alicyclic hydrocarbon, aromatic hydrocarbon, and unsaturated hydrocarbon.
[0015] Preferably, the solvent is any one or a combination of aniline, xylene, dichloromethane, cyclopentane, DMF, chloroform, dodecafluoropentane, pentafluorobutane, hexafluoroisopropanol, and carbon tetrachloride.
[0016] Furthermore, in step S1, the weight ratio of the polymer to the small molecule is (100:1) to (1:500), and the mass content of the polymer in the spinning solution is 0.1-30wt%;
[0017] In step S1, the temperature of the spinning solution preparation process is 100-250°C and the pressure is 0.1-50Mpa.
[0018] Furthermore, in step S2, the diameter of the polymer / small molecule fiber is 0.01-100 um, the degree of irregularity of the polymer / small molecule fiber is ≥35%, and the strength of the polymer / small molecule fiber is 1-10 g / d.
[0019] Furthermore, in step S3, the temperature condition of the first-stage hot pressing is:
[0020] The glass transition temperature of the polymer is ≤ the temperature of the first-stage hot pressing ≤ the decomposition temperature of the polymer; during the first-stage hot pressing process, the line pressure is 0.1-10N / mm and the vehicle speed is 0.1-10m / min.
[0021] Furthermore, in step S4, the method for removing small molecules from the composite non-woven fabric includes soaking in a good solvent for small molecules or enzymatic hydrolysis; the temperature of the secondary hot pressing is greater than the glass transition temperature of the polymer and the temperature of the secondary hot pressing is lower than the thermal decomposition temperature of the polymer, the line pressure is 10-300N / mm, the vehicle speed is 70-150m / min, and the number of hot pressing times is 1-4 times.
[0022] Furthermore, step S1 is to prepare the spinning solution in a high temperature and high pressure device, which includes but is not limited to: a reactor, a screw extruder, and an internal mixer. During pressurization, a gas is introduced into the high temperature and high pressure device, which includes but is not limited to: one or a mixture of nitrogen, carbon dioxide, argon, neon, and helium.
[0023] In step S2, the flash spinning steps include feeding, dissolving, spinning, filament separation, web laying, hot pressing and solvent recovery, which are well-known technologies in the art. The specific process parameters are determined according to actual production needs.
[0024] The invention also discloses an extended chain crystalline non-woven fabric, and the non-woven fabric is prepared by the manufacturing method of the invention.
[0025] The invention also discloses an application of an extended chain crystalline non-woven fabric, wherein the non-woven fabric is applied to medical protection, printing, construction, insulation packaging, home textile barrier, sewage treatment, and composite material reinforcement.
[0026] The beneficial effects of the present invention are:
[0027] (1) The method for manufacturing the non-woven fabric of the present invention solves the problem of poor thermal stability and low mechanical properties of the folded chain crystal polymer non-woven fabric. The polymer crystal structure in the non-woven fabric obtained by the present invention is an extended chain crystal structure. The entire preparation process is simple, with high crystallinity, good mechanical properties, good operability, fast spinning speed, and high production efficiency. It has broad prospects in medical protection, printing, construction, insulation packaging, home textile barrier, sewage treatment, composite material reinforcement, etc.
[0028] (2) The present invention is the first to add small molecules with a pore structure in the crystal to the spinning solution of traditional flash spinning to obtain composite fibers containing small molecules and polymers. The small molecule pores are used to regulate the crystal conformation of the polymer. The small molecule pores are used to accommodate a single polymer molecular chain to prepare a composite of small molecules and polymers, which effectively restricts the conformation of the polymer molecular chain. The polymer is maintained in a condensed structure in the composite through the first hot pressing action. After the small molecules are removed, the polymer molecular chains are fully stretched and stacked in parallel to obtain a polymer with a straight chain crystal form, thereby improving the temperature resistance and mechanical properties of the non-woven fabric.
[0029] (3) The crystal structure of the non-woven fabric prepared by the present invention is essentially different from the crystal structure of the non-woven fabric prepared by conventional traditional methods such as spunlace, meltblowing, spunbonding, and flash spinning. The present invention is the first to prepare polymer / small molecule fibers composed of small molecules and polymers by flash spinning, and obtain a non-woven fabric with an extended chain crystal form after hot pressing and removal of small molecules. The method provided by the present invention gets rid of the limitation of room temperature solvents, has a simple method, high crystallinity, good mechanical properties, good operability, fast spinning speed, and high production efficiency. The non-woven fabric is composed of a polymer with an extended chain crystal form.
[0030] (4) In the preparation method of the present invention, the temperature of the first-stage hot pressing in step S3 is limited to not higher than the melting point of the small molecules, and the temperature of the first-stage hot pressing is not lower than the glass transition temperature of the polymer, because at this time the polymer can undergo chain segment movement in the narrow channels formed by the small molecules, making the molecular segments of the polymer more regular. Through the first-stage hot pressing effect, the polymer retains the condensed conformation in the composite structure, which is beneficial for the polymer to continue to maintain this pre-conformation after the small molecules are removed, thereby forming extended chain crystals.
[0031] (5) In the preparation method of the present invention, the pore size of the small molecule is less than 10 angstroms, and the small molecule can form a narrow and long channel structure for accommodating a single polymer molecular chain, and finally obtain a non-woven fabric of extended chain crystals. If the diameter of the channel formed by the small molecule is too large, the single polymer molecular chain cannot be confined in a narrow space, and the extended chain crystal non-woven fabric of the present invention cannot be obtained at all. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The process flow of the manufacturing method of the extended chain crystalline nonwoven fabric of the present invention is as follows;
[0033] Figure 2 is a scanning electron microscope photograph of the polymer / small molecule fiber obtained in Example 1;
[0034] Figure 3 This is a scanning electron microscope photograph of the composite nonwoven fabric after removing the urea small molecules in Example 1. DETAILED DESCRIPTION
[0035] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0037] like Figure 1 As shown, a method for manufacturing an extended chain crystalline nonwoven fabric comprises the following steps:
[0038] S1. Preparation of spinning solution: dissolving polymer and small molecules in a solvent under heating and pressurizing conditions to obtain a uniform spinning solution; after the small molecules are crystallized, a hollow channel structure can be formed inside the crystal, and the pore size of the hollow small molecule crystal is less than 10 angstroms, which can accommodate a single polymer molecular chain;
[0039] S2, preparation of polymer / small molecule fibers: the spinning solution obtained in step S1 is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret, the solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers;
[0040] S3, preparation of composite non-woven fabric: the polymer / small molecule fiber obtained in step S2 is composed of a polymer guest and a small molecule host, wherein a single molecular chain of the polymer is confined in the pores of the small molecule crystal, and the polymer / small molecule fiber is divided into filaments, laid out, and subjected to primary hot pressing to obtain a composite non-woven fabric;
[0041] S4. Preparation of extended chain crystalline nonwoven fabric: removing small molecules from the composite nonwoven fabric obtained in step S3, and obtaining a high-performance nonwoven fabric of extended chain crystalline form through secondary hot pressing.
[0042] In step S1, the polymer is one or a combination of polyethylene, polypropylene, halogenated polyethylene, halogenated polypropylene, polyamide, polyester, polyoxymethylene, polyketone, and polyether.
[0043] In step S1, the small molecule is selected from one or a combination of urea, cyclodextrin, thiourea, methyl urea, dimethyl urea, trimethyl urea, tetramethyl urea, and p-nitrophenol.
[0044] In step S1, the solvent is one or more of water, alcohol, acid, amine, ester, ether, ketone, nitrile, amide, halogenated hydrocarbon, aliphatic hydrocarbon, alicyclic hydrocarbon, aromatic hydrocarbon, and unsaturated hydrocarbon.
[0045] In step S1, the weight ratio of the polymer to the small molecule is (100:1) to (1:500), and the mass content of the polymer in the spinning solution is 0.1-30wt%;
[0046] In step S1, the temperature of the spinning solution preparation process is 100-250°C and the pressure is 0.1-50Mpa.
[0047] In step S2, the diameter of the polymer / small molecule fiber is 0.01-100 um, the degree of irregularity of the polymer / small molecule fiber is ≥35%, and the strength of the polymer / small molecule fiber is 1-10 g / d.
[0048] In step S3, the temperature condition of the first-stage hot pressing is:
[0049] The glass transition temperature of the polymer is ≤ the temperature of the first-stage hot pressing ≤ the decomposition temperature of the polymer;
[0050] During the first-stage hot pressing process, the line pressure is 0.1-10 N / mm and the vehicle speed is 0.1-10 m / min.
[0051] In step S4, the method for removing small molecules from the composite non-woven fabric includes soaking with a good solvent for small molecules or enzymatic hydrolysis; the temperature of the secondary hot pressing is greater than the glass transition temperature of the polymer and the temperature of the secondary hot pressing is lower than the thermal decomposition temperature of the polymer, the line pressure is 10-300N / mm, the vehicle speed is 70-150m / min, and the number of hot pressing times is 1-4 times.
[0052] Testing method: After the non-woven fabric is subjected to constant temperature and humidity treatment, the thickness is measured using the PTI thickness tester of the German FRANK company, TAPPI standard T411om-97; the tensile strength and elongation are measured using the PTI horizontal tensile machine of the German FRANK company, TAPPI standard T410om-01; the tear degree is measured using the PTI tear tester of the German FRANK company, TAPPI standard T410om-04; the air permeability is measured using the 121D density meter of the Lorentzen & Wettre company, TAPPI standard T4600M-88.
[0053] Example 1
[0054] (1) Preparation of spinning solution: HDPE (Yangzi Petrochemical 5000S), urea, nitrogen, aniline and dichloromethane were added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 145°C and a pressure of 20 MPa, wherein the polymer content in the spinning solution was 10 wt%, the aniline content was 4% of the weight of the dichloromethane, and the weight ratio of the polymer to the small molecule was 1:10;
[0055] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 0.01-10 μm, the degree of irregularity of the polymer / small molecule fibers is 55%, and the strength of the polymer / small molecule fibers is 4.3 g / d. The scanning electron microscopy of the polymer / small molecule fibers is as follows: Figure 2 As shown;
[0056] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 90° C., a line pressure of 0.1 N / mm, and a speed of 10 m / min;
[0057] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in sufficient methanol for 5 times to completely remove urea. Scanning electron microscopy showed that Figure 3 As shown, the temperature of the secondary hot pressing is 142°C, the line pressure is 10N / mm, the vehicle speed is 150m / min, the number of hot pressing times is 4, and a high-performance non-woven fabric with an extended chain crystal form is obtained after the secondary hot pressing.
[0058] Using DSC test, the melting point of the non-woven fabric was 145°C, the melting enthalpy was 291 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 84.93N / cm, CD is 81.26N / cm, elongation MD is 30.12%, CD is 33.78%, tear strength MD is 11.43N, CD is 15.35N, and gurley porosity is 20s.
[0059] Example 2
[0060] (1) Preparation of spinning solution: ultra-high molecular weight polyethylene (Celanese 4118, USA), thiourea, carbon dioxide, dichloromethane and cyclopentane are added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 190°C and a pressure of 15 MPa, wherein the polymer content in the spinning solution is 0.1 wt%, the cyclopentane content is 10% of the weight of the dichloromethane, and the weight ratio of the polymer to the small molecule is 1:500;
[0061] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 0.1-20 μm, the degree of irregularity of the polymer / small molecule fibers is 35%, and the strength of the polymer / small molecule fibers is 7.6 g / d.
[0062] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) was separated into filaments and laid into a web, and a composite non-woven fabric was obtained by first-stage hot pressing at a temperature of 110° C., a line pressure of 2.5 N / mm, and a speed of 3 m / min;
[0063] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in sufficient ethanol for 8 times to completely remove thiourea. The temperature of the secondary hot pressing was 145°C, the line pressure was 200N / mm, the vehicle speed was 80m / min, and the number of hot pressing times was 1. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0064] Using DSC test, the melting point of the non-woven fabric was 149°C, the melting enthalpy was 272 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 290.25N / cm, CD is 412.89N / cm, elongation MD is 90.52%, CD is 92.74%, tear strength MD is 13.38N, CD is 18.78N, and gurley porosity is 28s.
[0065] Example 3
[0066] (1) Preparation of spinning solution: polyvinylidene fluoride (JHR-600, Juhua, Zhejiang), thiourea, nitrogen and carbon dioxide, cyclopentane and DMF were added into a screw extruder and stirred to obtain a spinning solution at a temperature of 220°C and a pressure of 15 MPa, wherein the polymer content in the spinning solution was 10 wt%, the DMF was 20% by weight of the cyclopentane, and the weight ratio of the polymer to the small molecule was 100:1;
[0067] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 0.1-20 μm, the degree of irregularity of the polymer / small molecule fibers is 71%, and the strength of the polymer / small molecule fibers is 14 g / d.
[0068] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 170° C., a linear pressure of 10 N / mm, and a speed of 5 m / min;
[0069] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in sufficient ethanol for 5 times to completely remove thiourea. The temperature of the secondary hot pressing was 205°C, the line pressure was 300N / mm, the vehicle speed was 100m / min, and the number of hot pressing times was 1. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0070] Using DSC test, the melting point of the non-woven fabric was 210°C, the melting enthalpy was 219 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 162.92N / cm, CD is 174.88N / cm, elongation MD is 25.75%, CD is 38.09%, tear strength MD is 19.04N, CD is 19.85N, and gurley porosity is 30s.
[0071] Example 4
[0072] (1) Preparation of spinning solution: polypropylene (Tianjin United 504PT), p-nitrophenol, carbon dioxide, chloroform and dichloromethane are added into a screw extruder and stirred to obtain a spinning solution at a temperature of 180° C. and a pressure of 50 MPa, wherein the polymer content in the spinning solution is 20 wt %, the chloroform is 5% of the weight of the dichloromethane, and the weight ratio of the polymer to the small molecule is 10:1;
[0073] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 0.01-40 μm, the degree of irregularity of the polymer / small molecule fibers is 49%, and the strength of the polymer / small molecule fibers is 8.7 g / d.
[0074] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 110° C., a linear pressure of 6 N / mm, and a speed of 1 m / min;
[0075] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in sufficient ethanol for 5 times to completely remove p-nitrophenol. The temperature of the secondary hot pressing was 183°C, the line pressure was 80N / mm, the vehicle speed was 130m / min, and the number of hot pressing times was 4. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0076] Using DSC test, the melting point of the non-woven fabric was 185°C, the melting enthalpy was 207 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 128.25N / cm, CD is 117.84N / cm, elongation MD is 64.68%, CD is 61.39%, tear strength MD is 12.77N, CD is 14.35N, and gurley porosity is 25s.
[0077] Example 5
[0078] (1) Preparation of spinning solution: LLDPE (Dow M3368 DFDA-1375RD, USA), urea, carbon dioxide, dichloromethane and dodecafluoropentane are added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 145°C and a pressure of 20 MPa, wherein the polymer content in the spinning solution is 15 wt%, the dodecafluoropentane is 10% by weight of the dichloromethane, and the weight ratio of the polymer to the small molecule is 1:20;
[0079] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 1-50 μm, the degree of irregularity of the polymer / small molecule fibers is 62%, and the strength of the polymer / small molecule fibers is 4.8 g / d.
[0080] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 120° C., a linear pressure of 1 N / mm, and a speed of 5 m / min;
[0081] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in sufficient deionized water for 5 times to completely remove urea. The temperature of the secondary hot pressing was 144°C, the line pressure was 50N / mm, the vehicle speed was 70m / min, and the number of hot pressing times was 3. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0082] Using DSC test, the melting point of the non-woven fabric was 145°C, the melting enthalpy was 291 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 71.93N / cm, CD is 89.26N / cm, elongation MD is 50.12%, CD is 50.78%, tear strength MD is 12.43N, CD is 15.35N, and gurley porosity is 32s.
[0083] Example 6
[0084] (1) Preparation of spinning solution: polybutylene succinate (Hengli Petrochemical KHB22BP11), urea, nitrogen, pentafluorobutane and hexafluoroisopropanol were added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 130°C and a pressure of 0.1 MPa, wherein the polymer content in the spinning solution was 30 wt%, the hexafluoroisopropanol was 5% of the weight of pentafluorobutane, and the weight ratio of the polymer to the small molecule was 10:1;
[0085] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 10-100 μm, the degree of irregularity of the polymer / small molecule fibers is 65%, and the strength of the polymer / small molecule fibers is 5.7 g / d.
[0086] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 120° C., a line pressure of 5.5 N / mm, and a speed of 4 m / min;
[0087] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in methanol for 5 times to completely remove urea. The temperature of the secondary hot pressing was 134°C, the line pressure was 10N / mm, the vehicle speed was 150m / min, and the number of hot pressing times was 2 times. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0088] Using DSC test, the melting point of the non-woven fabric was 136°C, the melting enthalpy was 106 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 51.37N / cm, CD is 60.85N / cm, elongation MD is 18.74%, CD is 22.76%, tear strength MD is 7.13N, CD is 8.80N, and gurley porosity is 18s.
[0089] Example 7
[0090] (1) Preparation of spinning solution: polycaprolactone (CAPA6500 of Polyren Chemical), cyclodextrin, argon, hexafluoroisopropanol and dodecafluoropentane were added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 100°C and a pressure of 10 MPa, wherein the polymer content in the spinning solution was 25 wt%, the hexafluoroisopropanol was 20% of the weight of dodecafluoropentane, and the weight ratio of the polymer to the small molecule was 50:1;
[0091] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 1-100 μm, the degree of irregularity of the polymer / small molecule fibers is 39%, and the strength of the polymer / small molecule fibers is 4.7 g / d.
[0092] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 50° C., a line pressure of 0.1 N / mm, and a speed of 10 m / min;
[0093] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in an aqueous solution of α-amylase for 10 times to completely remove cyclodextrin. The temperature of the secondary hot pressing was 74°C, the line pressure was 50 N / mm, the vehicle speed was 100 m / min, and the number of hot pressing times was 1. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0094] Using DSC test, the melting point of the non-woven fabric was 79°C, the melting enthalpy was 112 J / g, and the basis weight of the non-woven fabric was 39 g / m 2 , tensile strength MD is 35.32N / cm, CD is 37.43N / cm, elongation MD is 25.04%, CD is 28.23%, tear strength MD is 11.93N, CD is 8.68N, and gurley porosity is 35s.
[0095] Example 8
[0096] (1) Preparation of spinning solution: polyketone (Hyosung M330A, Korea), p-nitrophenol, nitrogen and carbon dioxide, carbon tetrachloride and hexafluoroisopropanol are added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 230°C and a pressure of 40 MPa, wherein the polymer content in the spinning solution is 5 wt%, the hexafluoroisopropanol is 10% of the weight of the carbon tetrachloride, and the weight ratio of the polymer to the small molecule is 1:200;
[0097] (2) Preparation of polymer / small molecule fibers: The spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret. The solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers. The diameter of the polymer / small molecule fibers is 1-50 μm, the degree of irregularity of the polymer / small molecule fibers is 43%, and the strength of the polymer / small molecule fibers is 8.9 g / d.
[0098] (3) Preparation of composite non-woven fabric: The polymer / small molecule fiber obtained in step (2) is separated into filaments and laid into a web, and a composite non-woven fabric is obtained by first-stage hot pressing at a temperature of 110° C., a linear pressure of 1 N / mm, and a speed of 2 m / min;
[0099] (4) Preparation of high-performance nonwoven fabric with extended chain crystal form: The composite nonwoven fabric obtained in step (3) was soaked and washed in ethanol for 6 times to completely remove p-nitrophenol. The temperature of the secondary hot pressing was 248°C, the line pressure was 300 N / mm, the vehicle speed was 90 m / min, and the number of hot pressing times was 2 times. After the secondary hot pressing, a high-performance nonwoven fabric with extended chain crystal form was obtained.
[0100] Using DSC test, the melting point of the non-woven fabric was 251°C, the melting enthalpy was 225 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 291.92N / cm, CD is 277.55N / cm, elongation MD is 35.39%, CD is 42.76%, tear strength MD is 19.77N, CD is 17.13N, and gurley porosity is 30s.
[0101] Comparative Example 1
[0102] (1) Preparation of spinning solution: HDPE (Yangzi Petrochemical 5000S), nitrogen and dichloromethane were added into a reaction kettle and stirred to obtain a spinning solution at a temperature of 145° C. and a pressure of 20 MPa, wherein the polymer content in the spinning solution was 10 wt %;
[0103] (2) Preparation of fibers: the spinning solution obtained in step (1) is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret, and the solvent in the spinning solution evaporates rapidly to obtain fibers;
[0104] (3) Preparation of non-woven fabric: the fibers obtained in step (2) are separated into strands, laid into a web, and hot-pressed to obtain a polyethylene non-woven fabric;
[0105] Using DSC test, the melting point of the non-woven fabric was 129°C, the melting enthalpy was 110 J / g, and the basis weight of the non-woven fabric was 42 g / m 2 , tensile strength MD is 34.26N / cm, CD is 40.85N / cm, elongation MD is 25.09%, CD is 20.11%, tear strength MD is 6.02N, CD is 4.35N, gurley porosity is 20s.
[0106] Comparing Example 1 with Comparative Example 1, the extended chain crystalline non-woven fabric prepared by the method of the present invention has significantly improved heat resistance and mechanical properties compared with the folded chain crystalline non-woven fabric prepared by the traditional flash evaporation method in Comparative Example 1; the extended chain crystalline non-woven fabric prepared by the method of the present invention has a high melting point, close to the equilibrium melting point, and has high tensile strength and tear resistance, indicating that the method of preparing a small molecule and polymer composite by using a small molecule pore structure to accommodate a single polymer molecular chain effectively regulates the condensed structure of the polymer molecular chain, so that the polymer molecular chain is fully stretched and stacked in parallel to obtain extended chain crystals, thereby greatly improving the heat resistance and mechanical properties of the non-woven fabric.
[0107] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0108] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for producing an extended chain crystalline nonwoven fabric, characterized in that: The manufacturing method comprises the following steps: S1. Preparation of spinning solution: dissolving polymer and small molecules in a solvent under heating and pressurizing conditions to obtain a uniform spinning solution; after the small molecules are crystallized, a hollow channel structure can be formed inside the crystal, and the pore size of the hollow small molecule crystal is less than 10 angstroms, which can accommodate a single polymer molecular chain; S2, preparation of polymer / small molecule fibers: the spinning solution obtained in step S1 is decompressed by a decompression device of a flash spinning device and then ejected from a spinneret, the solvent in the spinning solution evaporates rapidly, and the polymer and small molecules are assembled to obtain polymer / small molecule fibers; S3, preparation of composite non-woven fabric: the polymer / small molecule fiber obtained in step S2 is composed of a polymer guest and a small molecule host, wherein a single molecular chain of the polymer is confined in the pores of the small molecule crystal, and the polymer / small molecule fiber is divided into filaments, laid out, and subjected to a first-stage hot pressing to obtain a composite non-woven fabric; the temperature conditions of the first-stage hot pressing are: the glass transition temperature of the polymer ≤ the temperature of the first-stage hot pressing ≤ the decomposition temperature of the polymer, the line pressure is 0.1-10N / mm, and the vehicle speed is 0.1-10m / min; S4, preparation of extended chain crystalline non-woven fabric: removing small molecules from the composite non-woven fabric obtained in step S3, and obtaining a high-performance non-woven fabric of extended chain crystalline form through secondary hot pressing; The method for removing small molecules from the composite non-woven fabric includes soaking with a good solvent for small molecules or enzymatic hydrolysis; the temperature of the secondary hot pressing is greater than the glass transition temperature of the polymer and the temperature of the secondary hot pressing is lower than the thermal decomposition temperature of the polymer, the line pressure is 10-300N / mm, the vehicle speed is 70-150m / min, and the number of hot pressing times is 1-4 times.
2. The method for manufacturing an extended chain crystalline nonwoven fabric according to claim 1, characterized in that: In step S1, the polymer is one or a combination of polyethylene, polypropylene, halogenated polyethylene, halogenated polypropylene, polyamide, polyester, polyoxymethylene, polyketone, and polyether.
3. The method for manufacturing an extended chain crystalline nonwoven fabric according to claim 1, characterized in that: In step S1, the small molecule is selected from one or a combination of urea, cyclodextrin, thiourea, methyl urea, dimethyl urea, trimethyl urea, tetramethyl urea, and p-nitrophenol.
4. The method for manufacturing an extended chain crystalline nonwoven fabric according to claim 1, characterized in that: In step S1, the solvent is one or more of water, alcohol, acid, amine, ester, ether, ketone, nitrile, amide, halogenated hydrocarbon, aliphatic hydrocarbon, alicyclic hydrocarbon, aromatic hydrocarbon, and unsaturated hydrocarbon.
5. The method for manufacturing an extended chain crystalline nonwoven fabric according to claim 1, characterized in that: In step S1, the weight ratio of polymer to small molecule is (100:1) to (1:500), and the mass content of polymer in the spinning solution is 0.1-30wt%; In step S1, the temperature of the spinning solution preparation process is 100-250°C and the pressure is 0.1-50Mpa.
6. The method for manufacturing an extended chain crystalline nonwoven fabric according to claim 1, characterized in that: In step S2, the diameter of the polymer / small molecule fiber is 0.01-100 um, the degree of irregularity of the polymer / small molecule fiber is ≥35%, and the strength of the polymer / small molecule fiber is 1-10 g / d.
7. A straight chain crystalline nonwoven fabric, characterized in that: The nonwoven fabric is made by the manufacturing method described in any one of claims 1 to 6.
8. An application of the extended chain crystalline nonwoven fabric according to claim 7, characterized in that: The non-woven fabric is used in medical protection, printing, construction, insulation packaging, home textile barrier, sewage treatment, and composite material reinforcement.