Carbon nanotube for adsorption and separation of furfurylamine in biocatalytic system and preparation method thereof
By acidizing and grafting the multi-wall carbon nanotubes and introducing carboxylic functional groups and magnetic modifications, the problems of low adsorption capacity and difficulty in recycling of furfuramine in the biocatalytic system are solved, and high-efficiency furfuramine is achieved Adsorption and separation.
Patent Information
- Application Number
- CN202211725637.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing multi-wall carbon nanotube materials are difficult to meet the separation requirements of furfurylamine in biocatalytic systems in terms of adsorption capacity, selectivity and recycling, especially the problems of low adsorption capacity, easy agglomeration and difficult recovery.
By ultrasonic stirring of multi-walled carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, and graft modification is carried out at room temperature, carboxylic functional groups and magnetic modification are introduced to improve its adsorption ability and recyclability to furfuramine amine .
It realizes efficient adsorption of furfuramine and easy separation and recovery, fills the gap in furfuramine separation materials in the biocatalytic system, and improves the adsorption capacity and selectivity of the material.
Smart Images

Figure CN116020414B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and in particular relates to a carbon nanotube for adsorbing and separating furfurylamine in a biocatalytic system and a preparation method thereof. Background Art
[0002] Furfurylamine is an important organic synthesis intermediate and chemical product, which is widely used in the pharmaceutical industry. For example, it is condensed with 2,4-dichloro-5-aminosulfonylbenzoic acid to prepare the potent diuretic "Furosemide". At present, the industry mainly reduces furfural, Raney nickel, ammonia and methanol solution under 9Mpa conditions, and obtains the finished furfural amine by normal pressure distillation and vacuum distillation respectively. There are problems such as high energy consumption, high temperature and high pressure, and cumbersome steps. In 2017, Alice et al. (Alice Dunbabin, et al., Furfurylamines from biomass: transaminase catalyzed upgrading offfurals, Green Chem., 2017, 19, 397.) first reported a method for using transaminase to catalyze furfural to generate furfural amine, which achieved efficient synthesis of furfural amine in biocatalytic system and avoided the harsh reaction conditions of chemical method. However, the separation of furfural amine in biocatalytic system is still blank, and relevant research is urgently needed to promote the green preparation of furfural amine.
[0003] Adsorption is a simple, efficient and sustainable separation method. It separates adsorbates by physical adsorption or chemical adsorption, and has application potential in the separation of furfurylamine in biocatalytic systems. The core of the adsorption method is the design and preparation of adsorption materials, but there is currently a lack of research on furfurylamine adsorption materials for this system. Multi-walled carbon nanotubes have a hollow layer structure and a large specific surface area. After modification, it is easy to introduce oxygen-containing functional groups (such as COOH, OH) on the surface, and they have an efficient adsorption effect on nitrogen-containing adsorbates. For example, Gong et al. (Gong, Ji-Lai, et al., Removal ofcationic dyes from aqueous solution using magnetic multi-wall carbon nanotube nanocomposite as adsorbent, J. Harzard. Mater., 2009, 164, 1517) synthesized a specific surface area of 61.74 m 2 / g magnetic multi-walled carbon nanotube composite material, and used it to adsorb cationic dye methylene blue in aqueous solution, with a maximum adsorption capacity of 15.87mg / g; Nadia et al. (Boukhalfa, Nadia, et al., Maghemite / alginate / functionalized multiwalled carbon nanotubes beads for methylene blue removal: Adsorption and desorption studies, J. Mol. liq., 2019, 275, 431) designed magnetic hematite / sodium alginate / functionalized multi-walled carbon nanotube materials and applied them to the adsorption of methylene blue, with an adsorption capacity of up to 905.5mg / g in a wide range of pH = 4 to 10 and a stable physical structure; Tayebeh et al. (Tayebeh Esfandiyari, et al., Characterization and absorption studies of cationic dye on multi walled carbon nanotube–carbonceramic composite, J. Int. Eng. Chem., 2017, 46, 35) used sol-gel technology to synthesize multi-walled carbon nanotube-carbon ceramic composites, which can remove basic dyes 28 from aqueous solutions, and the adsorption capacity is 15 mg / g at pH = 8. However, the current multi-walled carbon nanotube materials are still difficult to meet the separation requirements of furfurylamine in biocatalytic systems in terms of adsorption capacity and selectivity, dispersibility and recyclability, and must be further structurally modified to meet the requirements. Summary of the invention
[0004] The present invention aims at the technical problem that the existing multi-walled carbon nanotube materials are still difficult to meet the requirements of separation of furfurylamine in biocatalytic system in terms of adsorption capacity and selectivity, dispersibility and recyclability, and there is a lack of materials for separation of furfurylamine in biocatalytic system. The present invention focuses on solving the problems of low adsorption capacity, easy agglomeration and difficult recycling of multi-walled carbon nanotube materials, and provides a method for preparing carbon nanotubes for adsorption and separation of furfurylamine in biocatalytic system. The preparation method comprises the following steps:
[0005] S1, adding multi-walled carbon nanotubes to a mixed solution of concentrated sulfuric acid and concentrated nitric acid, stirring with ultrasound, washing with distilled water until the pH value is 7, and drying to obtain acidified multi-walled carbon nanotubes;
[0006] S2, adding an organic solvent to the acidified multi-walled carbon nanotubes obtained in S1, then adding a condensing agent and an acid binding agent, stirring for 0.5 h, then adding an amino donor, reacting at room temperature, and filtering to obtain grafted double-bond modified multi-walled carbon nanotubes;
[0007] S3, adding an organic solvent to the grafted double-bond modified multi-walled carbon nanotubes obtained in S2, dispersing by ultrasonication, replacing with an oxygen-free environment, raising the temperature, adding a functional group monomer and an initiator, and filtering after the reaction to obtain a grafted material;
[0008] S4. Mix the iron salt and ethylene glycol until they are completely dissolved, add ammonia water and stir to react for 30 minutes, then add the grafted material obtained in S3, heat to 160°C and react for 8 hours, cool, and wash to obtain the magnetic grafted material.
[0009] It is further defined that the inner diameter of the multi-walled carbon nanotubes in S1 is 3-15 nm, the outer diameter is 10-80 nm, and the length is 5-50 um; the concentration of concentrated sulfuric acid is 98%, and the solid-liquid ratio of multi-walled carbon nanotubes to concentrated sulfuric acid is 1 g: 10-50 mL; the concentration of concentrated nitric acid is 65-68%, and the solid-liquid ratio of multi-walled carbon nanotubes to concentrated nitric acid is 1 g: 10-30 mL; and the ultrasonic time is 5-120 min.
[0010] It is further defined that the organic solvent in S2 is any one of acetonitrile, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, 1,4-dioxane, and dichloromethane, or a mixture of two or more thereof; and the solid-liquid ratio of the acidified multi-walled carbon nanotubes to the organic solvent is 1 g:10-30 mL.
[0011] It is further defined that the condensing agent in S2 is any one of HATU, HOBT, PyBOP, TATU, DCC, CDI, EDCI, and DMT-MM, or a mixture of two or more thereof, and the ratio of the amount of the condensing agent to the mass of the acidified multi-walled carbon nanotubes is 1 to 20 mmol: 1 g; the acid binding agent is any one of sodium carbonate, potassium carbonate, pyridine, triethylamine, and 4-dimethylaminopyridine, or a mixture of two or more thereof, and the ratio of the amount of the acid binding agent to the mass of the acidified multi-walled carbon nanotubes is 1 to 20 mmol: 1 g.
[0012] It is further defined that the amino donor in S2 is any one of allylamine and allylamine hydrochloride or a mixture of the two, the ratio of the amount of the amino donor substance to the mass of the acidified multi-walled carbon nanotubes is 1-20 mmol: 1 g; and the reaction time is 0.5-8 h.
[0013] It is further defined that the organic solvent in S3 is any one of toluene, acetone, n-hexane, tetrahydrofuran, acetonitrile, methanol, and water, or a mixture of two or more thereof; the solid-liquid ratio of the grafted double-bond modified multi-walled carbon nanotubes to the organic solvent is 1 g:10-500 mL; the ultrasonic dispersion time is 0.5-1 h; and the elevated temperature refers to a temperature raised to 35-70°C.
[0014] It is further defined that the functional group monomer in S3 is any one of acrylic acid, methacrylic acid, trifluoromethylacrylic acid, 4-vinylbenzoic acid, itaconic acid, and maleic anhydride, or a mixture of two or more thereof; the ratio of the amount of the functional group monomer substance to the mass of the grafted double-bond modified multi-walled carbon nanotubes is 0.1 to 0.5 mol:1 g; the initiator is any one of azobisisobutyronitrile, azobisisobutylheptonitrile, azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, and benzoyl peroxide, or a mixture of two or more thereof; the mass ratio of the initiator to the functional group monomer is 0.005 to 0.03:1; and the reaction time is 1 to 10 h.
[0015] It is further defined that the iron salt in S4 is any one of FeSO4·7H2O, FeCl3, (NH4)2Fe(SO4)2, and NH4FeSO4(SO4)2; the mass ratio of the iron salt to the grafted material obtained in S3 is 1.5-3.0:1; and the ratio of the volume of ethylene glycol to the mass of the iron salt is 5-20 mL:1 g.
[0016] The present invention also provides carbon nanotubes prepared by the above preparation method.
[0017] The present invention also provides the use of the carbon nanotubes prepared by the preparation method in the adsorption and separation of furfurylamine in a biocatalytic system.
[0018] Beneficial effects of the present invention:
[0019] We used oxidation, surface in situ polymerization and other methods to introduce carboxyl functional groups to interact electrostatically with furfuralamine, and modified magnetic MWCNTs on the basis of achieving specific adsorption of furfuralamine to obtain a series of furfuralamine adsorption and separation materials with high adsorption capacity and easy separation and recovery.
[0020] The present invention focuses on solving the problems of low adsorption capacity, easy agglomeration, and difficult recycling of multi-walled carbon nanotube materials. Based on the π-π interaction between the furan nucleus of furfurylamine and the conjugated structure of MWCNTs, a carboxyl functional group is introduced by oxidation, surface in-situ polymerization, and the like to generate electrostatic interaction with furfurylamine. On the basis of achieving specific adsorption of furfurylamine, magnetic MWCNTs are modified. Multi-walled carbon nanotubes are used as a matrix, and the dispersion performance of the material is improved by oxidation. In-situ polymerization and magnetic modification are used to improve the selectivity of furfurylamine and the recyclability of the material. A series of high-efficiency furfurylamine adsorption and separation materials with high adsorption capacity and easy separation and recycling are obtained, which fills the gap in furfurylamine separation materials in biocatalytic systems. The specific advantages are as follows:
[0021] 1) Selecting multi-walled carbon nanotube skeleton materials with high specific surface area and rich conjugated structure to achieve π-π interaction with furfurylamine furan ring, further introducing oxygen-containing functional groups by oxidation modification, improving the dispersion performance of the material, and improving the adsorption force on furfurylamine and the hydrophilicity of the material itself from the perspective of the matrix;
[0022] 2) Carboxyl functional groups are grafted onto the surface of multi-walled carbon nanotubes by in situ polymerization reaction, and the selective adsorption of furfurylamine is improved through ionic bonds, electrostatic interactions, etc., and a magnetic modification strategy is further introduced to improve the recyclability of the material, thereby obtaining a highly efficient furfurylamine adsorption material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The infrared results of MWCNTs, MWCNTs-1 and MWCNTs-AA in Example 1;
[0024] Figure 2 This is a graph showing the comparison of the adsorption capacity of various multi-walled carbon nanotube materials on the biocatalytic system furfurylamine in Example 9;
[0025] Figure 3 This is the result of liquid phase determination of the fermentation broth obtained after the various multi-walled carbon nanotube materials adsorbed the biocatalytic system furfurylamine in Example 9. The retention time of furfurylamine is 3.532min;
[0026] Figure 4 This is a diagram showing the results of the adsorption and separation of furfurylamine in the biocatalytic system by MWCNTs-AA in Example 9, and the measurement of the liquid phase of the desorption liquid after desorption. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific implementation methods and the accompanying drawings of the specification. The experimental methods used in the following examples are conventional methods unless otherwise specified, and the materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained by those skilled in the art through commercial channels.
[0028] Embodiment 1:
[0029] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0030] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter >50 nm, length 10-30 um) into a mixed solution of concentrated sulfuric acid (5 mL) and concentrated nitric acid (15 mL), stir ultrasonically for 60 min, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0031] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (N,N-dimethylformamide) (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 6 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0032] Step 3: MWCNTs-N (0.5 g) was added toluene (50 mL), and ultrasonic dispersion was performed for 0.5 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 ° C, acrylic acid (2.0 mL) and AIBN (azobisisobutyronitrile) (50 mg) were added. After reacting for 6 h, the grafted material was filtered;
[0033] Step 4: Dissolve FeSO4·7H2O (5 g) in deionized water (50 mL), mix with polyethylene glycol (molecular weight 200000, 25 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material of step 3, stir and react for 30 min, heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-AA.
[0034] Embodiment 2:
[0035] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0036] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 5-15 nm, outer diameter >50 nm, length 10-30 um) to a mixed solution of concentrated sulfuric acid (5 mL) and concentrated nitric acid (15 mL), stir ultrasonically for 2 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0037] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 8 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0038] Step 3: MWCNTs-N (0.5 g) was added to methanol (50 mL), and ultrasonically dispersed for 1 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 °C, acrylic acid (2.0 mL) and AIBN (azobisisobutyronitrile) (10 mg) were added. After reacting for 6 h, the grafted material was filtered.
[0039] Step 4: Dissolve FeSO4·7H2O (5 g) in deionized water (50 mL), mix with polyethylene glycol (molecular weight 200000, 25 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material of step 3, stir and react for 30 min, heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-AA.
[0040] Embodiment 3:
[0041] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0042] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter >50 nm, length 10-30 um) into a mixed solution of concentrated sulfuric acid (15 mL) and concentrated nitric acid (10 mL), stir with ultrasound for 1 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0043] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, add allylamine (0.57 g, 10 mmol), react at room temperature for 0.5 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0044] Step 3: MWCNTs-N (0.5 g) was added to methanol (50 mL), and ultrasonically dispersed for 0.5 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 ° C, methacrylic acid (2.1 mL) and AIBN (20 mg) were added. After reacting for 6 h, the grafted material was filtered.
[0045] Step 4: Dissolve FeSO4·7H2O (5 g) in deionized water (50 mL), mix with polyethylene glycol (molecular weight 200000, 25 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material of step 3, stir and react for 30 min, heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-MA.
[0046] Embodiment 4:
[0047] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0048] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter >50 nm, length 10-30 um) to a mixed solution of concentrated sulfuric acid (7.5 mL) and concentrated nitric acid (7.5 mL), stir ultrasonically for 1 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0049] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 8 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0050] Step 3: MWCNTs-N (0.5 g) was added to methanol (50 mL), and ultrasonically dispersed for 0.5 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 ° C, 4-vinylbenzoic acid (2.0 mL) and AIBN (25 mg) were added. After reacting for 6 h, the grafted material was filtered.
[0051] Step 4: Dissolve FeSO4·7H2O (5 g) in deionized water (50 mL), mix with polyethylene glycol (molecular weight 200000, 25 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material of step 3, stir and react for 30 min, heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-PA.
[0052] Embodiment 5:
[0053] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0054] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter >50 nm, length 10-30 um) to a mixed solution of concentrated sulfuric acid (7.5 mL) and concentrated nitric acid (7.5 mL), stir ultrasonically for 1 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0055] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 4 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0056] Step 3: MWCNTs-N (0.5 g) was added to methanol (50 mL), and ultrasonically dispersed for 0.5 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 ° C, itaconic acid (2.3 mL) and AIBN (25 mg) were added. After reacting for 6 h, the grafted material was filtered;
[0057] Step 4: Dissolve FeSO4·7H2O (5 g) in deionized water (50 mL), mix with polyethylene glycol (molecular weight 200000, 25 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material of step 3, stir and react for 30 min, heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-CA.
[0058] Embodiment 6:
[0059] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0060] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter >50 nm, length 10-30 um) to a mixed solution of concentrated sulfuric acid (7.5 mL) and concentrated nitric acid (7.5 mL), stir ultrasonically for 1 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0061] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 6 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0062] Step 3: MWCNTs-N (0.5 g) was added to methanol (50 mL), and ultrasonic dispersion was performed for 0.5 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 ° C, maleic anhydride (1.5 mL) and AIBN (10 mg) were added. After reacting for 6 h, the grafted material was filtered.
[0063] Step 4: Dissolve FeSO4·7H2O (5 g) in deionized water (50 mL), mix with polyethylene glycol (molecular weight 200000, 25 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material of step 3, stir and react for 30 min, heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-GA-1.
[0064] Embodiment 7:
[0065] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0066] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter>50 nm, length 10-30 um) to a mixed solution of concentrated sulfuric acid (5 mL) and concentrated nitric acid (15 mL), stir ultrasonically for 0.5 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0067] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add HATU (3.0 g, 7.9 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 4 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0068] Step 3: MWCNTs-N (0.5 g) was added toluene (50 mL), and ultrasonically dispersed for 1 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 °C, maleic anhydride (1.5 mL) and AIBN (15 mg) were added. After reacting for 6 h, the grafted material was filtered.
[0069] Step 4: Dissolve (NH4)2Fe(SO4)2 (6.5 g) in deionized water (50 mL), mix with ethylene glycol (50 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material in step 3, stir and react for 30 min, then heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-GA-2.
[0070] Embodiment 8:
[0071] The method for preparing carbon nanotubes by adsorption and separation of furfurylamine in a biocatalytic system of this embodiment is carried out in the following steps:
[0072] Step 1: Add multi-walled carbon nanotubes (0.5 g, inner diameter 3-15 nm, outer diameter>50 nm, length 10-30 um) to a mixed solution of concentrated sulfuric acid (5 mL) and concentrated nitric acid (15 mL), stir ultrasonically for 0.5 h, wash with distilled water until pH = 7, and dry to obtain acidified multi-walled carbon nanotubes MWCNTs-1;
[0073] Step 2: Add the acidified multi-walled carbon nanotubes (0.5 g) to DMF (10 mL), add EDCI (1.6 g, 8.3 mmol), triethylamine (1.0 g, 10 mmol), stir for 0.5 h, then add allylamine (0.57 g, 10 mmol), react at room temperature for 4 h, and filter to obtain double-bond modified multi-walled carbon nanotubes MWCNTs-N;
[0074] Step 3: MWCNTs-N (0.5 g) was added toluene (50 mL), and ultrasonic dispersion was performed for 0.5 h. The mixture was replaced with an oxygen-free environment. After the reaction temperature was raised to 60 ° C, maleic anhydride (3.0 mL) and BPO (50 mg) were added. After reacting for 6 h, the grafted material was filtered;
[0075] Step 4: Dissolve (NH4)2Fe(SO4)2 (6.5 g) in deionized water (50 mL), mix with ethylene glycol (50 mL), slowly add 30% hydrogen peroxide solution (0.5 mL), ammonia water (2.5 wt%, 25 mL), and the grafted material in step 3, stir and react for 30 min, then heat to 160 ° C and react for 8 h, cool, and wash to obtain the magnetic grafted material MWCNTs-GA-3.
[0076] Embodiment 9:
[0077] This embodiment provides a method for adsorbing and separating furfurylamine in a biocatalytic system using carbon nanotube materials, which is specifically carried out in the following steps:
[0078] (1) In a 50 mL centrifuge tube, add 20 mL of fermentation broth from the biocatalytic system, with a furfurylamine concentration of 0.5 g / L;
[0079] (2) Weigh 20 mg each of multi-walled carbon nanotubes (MWCNTs), MWCNTs-1 (obtained in step 1 of Example 1), MWCNTs-AA (prepared in Example 1), MWCNTs-MA (prepared in Example 3), MWCNTs-PA (prepared in Example 4), MWCNTs-CA (prepared in Example 5), and MWCNTs-GA-1 (prepared in Example 6), add them to the above centrifuge tube, and adsorb them at 30°C and 180 rpm for 24 h. Determine the furfurylamine concentration before and after adsorption by HPLC and calculate the adsorption capacity (see Figure 2 );
[0080] (3) After solid-liquid separation by magnet, the above material is desorbed with 1 wt% ammonia water, and the purity of the desorbed furfurylamine is measured by liquid phase.
[0081] Result analysis:
[0082] The original multi-walled carbon nanotubes MWCNTs used in Example 1, the acidified multi-walled carbon nanotubes MWCNTs-1, and the finally prepared material MWCNTs-AA were characterized by infrared structure. The specific results are as follows Figure 1 As shown in the figure, compared with the original multi-walled carbon nanotube material without carboxyl groups, the MWCNTs-1 introduced with carboxyl groups after acidification has a higher -1 There is an obvious carboxyl characteristic peak at 1715 cm -1 The carboxyl characteristic peak is the strongest, indicating that MWCNTs-AA is loaded with a higher content of carboxyl functional groups and the modification strategy is successful.
[0083] Figure 2 The comparison results of the adsorption capacity of furfurylamine of various multi-walled carbon nanotube materials in the examples for the biocatalytic system are shown. According to the results, the adsorption capacities of the original multi-walled carbon nanotubes MWCNTs, the acidified material MWCNTs-1, the grafted acrylic acid material MWCNTs-AA, the grafted methacrylic acid material MWCNTs-MA, the grafted 4-vinylbenzoic acid material MWCNTs-PA, the grafted itaconic acid material MWCNTs-CA, and the grafted maleic anhydride material MWCNTs-GA-1 for furfurylamine are 0.09mmol / g, 0.79mmol / g, 1.10mmol / g, 1.16mmol / g, 0.97mmol / g, 0.91mmol / g, and 1.24mmol / g, respectively. The grafted materials show better furfurylamine adsorption performance.
[0084] Adsorption capacity calculation formula:
[0085] Before adsorption, the amount of furfural amine in 20 mL of fermentation broth was: n furfural amine 1 = (20 / 1000) × 0.5 / 97 = 0.103 mmol
[0086] After adsorption, the remaining furfural amine concentration in the fermentation broth was determined as C1. The amount of furfural amine in 20 mL of fermentation broth was: n furfural amine 2 = n furfural amine 1 - (20 / 1000) × C1
[0087] Add 20 mg of adsorption material, and calculate the adsorption capacity of the material after adsorption: Q = (n furfurylamine 1-n furfurylamine 2) / (20 / 1000)
[0088] Figure 3 This is the result of liquid phase determination of the fermentation broth of the biocatalytic system in Example 9. The retention time of furfuralamine is 3.532 min, and furfural impurity (7.595 min) is also present in the fermentation broth.
[0089] Figure 4In Example 9, MWCNTs-AA was used to adsorb and separate furfural in the biocatalytic system, and the desorption liquid phase was measured after desorption. It was found that the material effectively adsorbed furfural (3.512 min) but did not adsorb impurities such as furfural.
[0090] Although the present invention has been disclosed as above in the form of preferred embodiments, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing carbon nanotubes for adsorption and separation of furfurylamine in a biocatalytic system, characterized in that: The preparation method comprises the following steps: S1, adding multi-walled carbon nanotubes to a mixed solution of concentrated sulfuric acid and concentrated nitric acid, stirring with ultrasound, washing with distilled water until the pH value is 7, and drying to obtain acidified multi-walled carbon nanotubes; S2, adding an organic solvent to the acidified multi-walled carbon nanotubes obtained in S1, then adding a condensing agent and an acid binding agent, stirring for 0.5 h, then adding an amino donor, reacting at room temperature, filtering to obtain grafted double-bond modified multi-walled carbon nanotubes; the organic solvent is any one of acetonitrile, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, 1,4-dioxane, and dichloromethane, or a mixture of two or more thereof; the condensing agent is any one of HATU, HOBT, PyBOP, DCC, CDI, EDCI, and DMT-MM, or a mixture of two or more thereof; the acid binding agent is any one of sodium carbonate, potassium carbonate, pyridine, triethylamine, and 4-dimethylaminopyridine, or a mixture of two or more thereof; the amino donor is any one of allylamine and allylamine hydrochloride, or a mixture of two or more thereof; S3, adding an organic solvent to the grafted double-bond modified multi-walled carbon nanotubes obtained in S2, after ultrasonic dispersion, replacing with an oxygen-free environment, raising the temperature, adding a functional group monomer and an initiator, and filtering to obtain a grafted material after the reaction; the organic solvent is any one of toluene, acetone, n-hexane, tetrahydrofuran, acetonitrile, methanol, and water, or a mixture of two or more thereof; the functional group monomer is any one of acrylic acid, methacrylic acid, trifluoromethylacrylic acid, 4-vinylbenzoic acid, itaconic acid, and maleic anhydride, or a mixture of two or more thereof; the initiator is any one of azobisisobutyronitrile, azobisisobutylheptanitrile, azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, and benzoyl peroxide, or a mixture of two or more thereof; S4. Mix the iron salt and ethylene glycol until they are completely dissolved, add ammonia water and stir to react for 30 min, then add the grafted material obtained in S3, heat to 160°C and react for 8 h, cool, and wash to obtain the magnetic grafted material.
2. The preparation method according to claim 1, characterized in that: S1 The inner diameter of the multi-walled carbon nanotubes is 3~15 nm, the outer diameter is 10~80 nm, and the length is 5~50 um; the concentration of concentrated sulfuric acid is 98%, and the solid-liquid ratio of multi-walled carbon nanotubes to concentrated sulfuric acid is 1g:10~50 mL; the concentration of concentrated nitric acid is 65%~68%, and the solid-liquid ratio of multi-walled carbon nanotubes to concentrated nitric acid is 1 g:10~30mL; the ultrasonic time is 5~120 min.
3. The preparation method according to claim 1, characterized in that: The solid-liquid ratio of the acidified multi-walled carbon nanotubes and the organic solvent in S2 is 1 g: 10~30 mL.
4. The preparation method according to claim 1, characterized in that: S2: The ratio of the amount of the condensing agent substance to the mass of the acidified multi-walled carbon nanotubes is 1-20 mmol: 1 g; the ratio of the amount of the acid binding agent substance to the mass of the acidified multi-walled carbon nanotubes is 1-20 mmol: 1 g.
5. The preparation method according to claim 1, characterized in that: The ratio of the amount of the amino donor substance in S2 to the mass of the acidified multi-walled carbon nanotubes is 1-20 mmol:1 g; and the reaction time is 0.5-8 h.
6. The preparation method according to claim 1, characterized in that: S3: the solid-liquid ratio of the grafted double-bond modified multi-walled carbon nanotubes to the organic solvent is 1 g: 10~500 mL; the ultrasonic dispersion time is 0.5~1 h; the elevated temperature refers to the temperature being raised to 35~70°C.
7. The preparation method according to claim 1, characterized in that: S3: The mass ratio of the functional group monomer substance to the grafted double bond modified multi-walled carbon nanotubes is 0.1-0.5 mol: 1 g; the mass ratio of the initiator to the functional group monomer is 0.005-0.03: 1; and the reaction time is 1-10 h.
8. The preparation method according to claim 1, characterized in that: The iron salt in S4 is any one of FeSO4·7H2O, FeCl3, (NH4)2Fe(SO4)2, and NH4Fe(SO4)2; the mass ratio of the iron salt to the grafted material obtained in S3 is 1.5~3.0:1; the ratio of the volume of ethylene glycol to the mass of the iron salt is 5~20 mL:1 g.
9. The carbon nanotubes prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the carbon nanotubes prepared by the preparation method according to any one of claims 1 to 8 in the adsorption and separation of furfurylamine in a biocatalytic system.
Citation Information
Patent Citations
Preparation and application methods of carbon-nanotube-base magnetic bactericide molecularly-imprinted polymer
CN105693961A
Cited By
Composite modified multi-walled carbon nanotube material, preparation method thereof and application of composite modified multi-walled carbon nanotube material in furfuryl amine adsorption separation
CN116920797A
A composite modified multi-walled carbon nanotube material, its preparation method, and its application in the adsorption and separation of furfurylamine.
CN116920797B