A bimetallic carbon nanofiber catalyst and its preparation method and application
By dosing the catalyst with bimetallic nanoparticles such as copper and cobalt on the upper limit of carbon nanofibers, the problem of transition metal leakage and deactivation of the catalyst in water pollution treatment is solved, and an efficient, stable and reusable catalytic degradation effect is achieved.
Patent Information
- Application Number
- CN202211414847.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-11
AI Technical Summary
Existing catalysts have problems with transition metal leakage, deactivation and secondary pollution during the catalytic degradation process. Moreover, single-metal catalysts are easily deactivated. The catalytic effect is affected by the pH value of the system, making it difficult to achieve high efficiency, stability and repeatability in water pollution treatment. use.
Develop bimetal-loaded carbon nanofiber catalysts. Transition metal nanoparticles such as copper and cobalt are confined in the carbon nanofiber lattice through electrospinning methods to form a uniformly distributed catalyst, avoid metal agglomeration and leakage, and utilize bimetallic synergy. The effect improves catalytic efficiency.
It achieves efficient degradation of antibiotic pollutants. The catalyst has good stability and recyclability, avoiding metal leakage and deactivation. The catalytic effect is far better than that of a single metal catalyst, and it still maintains high degradation efficiency after multiple uses.
Smart Images

Figure CN116037122B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a bimetallic carbon nanofiber-based catalyst and a preparation method and application thereof. The catalyst generates highly active free radicals to degrade pollutants by activating persulfate and peroxycarbonate, and belongs to the field of environmental chemistry. Background Art
[0002] Advanced oxidation technology is to generate highly reactive free radicals in the reaction system under the conditions of catalyst or external energy, so as to remove refractory organic matter and decompose pollutants into CO2 and H2O. Advanced oxidation technology has mild reaction conditions, simple principle, convenient application, can quickly and efficiently treat organic pollutants in different concentrations and different media, and has a wide range of applications. It is easy to combine with other technologies and is considered to be one of the most effective means to solve organic pollution such as antibiotics. Among the advanced oxidation technologies, the advanced oxidation technology based on persulfate and peroxycarbonate has the advantages of high reaction efficiency, less pollution, low energy consumption, and thorough removal of pollutants. Persulfate causes the peroxy bond to break under the action of catalyst or external energy, forming highly active free radicals containing unpaired electrons. Advanced oxidation technology based on persulfate has received widespread attention in water pollution treatment due to the high stability of the oxidant in production and transportation, its persistence in the environment, and its high degradation efficiency of refractory pollutants. Peroxycarbonate ions are mainly generated from hydrogen peroxide and bicarbonate. When peroxycarbonate ions are activated, the peroxy bond breaks to generate a series of active substances, such as hydroxyl radicals and carbonate radicals. Peroxycarbonates and peroxycarbonate oxidation systems can efficiently degrade pollutants under alkaline and near-neutral conditions. The reaction system is simple, economical, environmentally friendly and non-corrosive.
[0003] The catalyst activates peroxysulfuric acid and peroxycarbonic acid to degrade organic pollutants. The conditions are mild and no external energy is required, which can effectively reduce the cost of use. According to whether the catalyst and the reactant are in the same phase, catalysis is divided into homogeneous catalysis and heterogeneous catalysis. Homogeneous catalysts are mainly various transition metal ions that can be dissolved in the water phase, while heterogeneous catalysts refer to various water-insoluble solid catalysts such as transition metal oxides. Homogeneous catalysis has a good catalytic effect because the reaction system is in the same phase and the contact is sufficient. However, since homogeneous catalytic reactions will cause the problem of heavy metal ion leakage, and most transition elements have certain toxicity, homogeneous catalysis will cause secondary pollution. Heterogeneous catalytic reactions can effectively reduce the problem of secondary pollution of transition metals and increase the reuse rate of catalysts. During the use of heterogeneous catalysts, problems such as difficulty in recovery, metal agglomeration, transition metal leakage and deactivation will occur.
[0004] The larger specific surface area of carbon nanofibers can increase the metal loading of carbon nanofibers, provide more reaction sites, and increase the dispersion of catalysts; the ultra-high aspect ratio can effectively combine the efficient catalysis and efficient separation efficiency of nanometer size; the higher surface activity can effectively combine the catalyst with the reactants, and improve the reaction rate of catalytic degradation; the better stability provides conditions for the reuse of the catalyst; at the same time, using non-magnetic carbon nanofibers as carriers to load heavy metals can effectively reduce the agglomeration of metals and reduce the magnetic effect of the material; the nanocatalyst can be confined to the carbon nanofiber lattice through a blending process, which can effectively avoid problems such as metal leakage and deactivation.
[0005] Single metal catalysts are easily deactivated during catalytic degradation, and the catalytic effect is affected by the pH value of the system. Compared with single metals, bimetallic catalysts have a significantly improved catalytic efficiency due to the synergistic effect of electron exchange between the loaded metals. When two metals are loaded on carbon nanofibers, the bimetallic can be evenly distributed in the carbon nanofibers, effectively avoiding the leakage of transition metals, and when the loading sites of the two nanometals in the carbon nanofibers are close, the metal ions are conducive to the synergistic effect. Therefore, carbon nanofiber-loaded transition metal catalysts have certain advantages in the application of activated peroxides to degrade environmental pollutants.
[0006] In order to solve the problems arising in homogeneous and heterogeneous catalytic reaction systems and make persulfate and peroxycarbonate advanced oxidation technologies adapt to actual engineering, bimetallic catalysts were combined with carbon nanofibers to develop a bimetallic-loaded carbon nanofiber catalyst. This catalyst can avoid secondary pollution, metal agglomeration and other problems, has good stability, recyclability and high catalytic efficiency, and has a good application prospect in water pollution treatment. Summary of the invention
[0007] To improve the above technical problems, the present invention provides a catalyst, which is a carbon nanofiber loaded with two transition metals, wherein the two transition metals are selected from any two of copper, cobalt, tungsten, vanadium, iron and manganese; for example, copper and cobalt.
[0008] In one embodiment, the catalyst is carbon nanofibers loaded with copper and cobalt.
[0009] Preferably, the transition metal is present in the form of nanoparticles thereof.
[0010] Preferably, the transition metal nanoparticles are uniformly distributed in the carbon nanofibers.
[0011] According to an embodiment of the present invention, the transition metal nanoparticles are confined and synthesized in the carbon nanofiber lattice.
[0012] According to an embodiment of the present invention, the loading amount of each transition metal nanoparticle is 0.005-0.05 wt%, for example, 0.01 wt%, 0.016 wt%, 0.02 wt%, 0.03 wt%.
[0013] According to an embodiment of the present invention, the loading amount of the cobalt nanoparticles is 0.005-0.05 wt %, for example, 0.01 wt %, 0.016 wt %, 0.02 wt %, 0.03 wt %.
[0014] According to an embodiment of the present invention, the loading amount of the copper nanoparticles is 0.005-0.05 wt %, for example, 0.01 wt %, 0.02 wt %, 0.03 wt %.
[0015] According to an embodiment of the present invention, the diameter of the carbon nanofiber is 100-500 nm, for example, 200 nm, 300 nm, 400 nm.
[0016] According to an embodiment of the present invention, the diameter of each transition metal nanoparticle is 10 to 80 nm, such as 30 to 50 nm.
[0017] According to an embodiment of the present invention, the diameter of the cobalt nanoparticles is 10 to 80 nm, preferably 30 to 50 nm.
[0018] According to an embodiment of the present invention, the diameter of the copper nanoparticles is 10 to 80 nm, preferably 30 to 50 nm.
[0019] According to an embodiment of the present invention, the two transition metal nanoparticles have no agglomeration phenomenon. In a preferred embodiment, the cobalt and copper nanoparticles have no agglomeration phenomenon.
[0020] According to an embodiment of the present invention, the distribution positions of the two transition metal nanoparticles in the carbon nanocellulose are close or the same. In a preferred embodiment, the distribution positions of the cobalt and copper nanoparticles in the carbon nanocellulose are close or the same.
[0021] According to an embodiment of the present invention, the catalyst contains carbon, oxygen, copper and cobalt elements.
[0022] According to an embodiment of the present invention, the Co nanoparticles include nano zero-valent cobalt particles; preferably, the nano zero-valent cobalt particles are dispersed inside the carbon nanofibers.
[0023] In some embodiments, the Co nanoparticles further include Co3O4 nanoparticles; preferably, the Co3O4 nanoparticles are located on the surface of the carbon nanofibers.
[0024] According to an embodiment of the present invention, the copper nanoparticles exist in the form of nano zero-valent copper.
[0025] According to an embodiment of the present invention, the catalyst has soft magnetic properties.
[0026] According to an embodiment of the present invention, the catalyst contains mesopores.
[0027] According to an embodiment of the present invention, the pore volume of the catalyst is 2 to 10 cm 3 / g, for example 4cm 3 / g, 5cm 3 / g, 6cm 3 / g, 6.4cm 3 / g, 7cm 3 / g, 8cm 3 / g.
[0028] The present invention also provides a method for preparing the above catalyst, comprising the following steps: electrostatically spinning an electrospinning precursor solution to form nano-polymer fibers containing transition metal salts, pre-oxidizing and carbonizing the nano-polymer fibers to synthesize the catalyst;
[0029] The electrospinning precursor solution comprises an organic solvent, a carbon source and two transition metal salts.
[0030] According to an embodiment of the present invention, the organic solvent is an organic solvent that can dissolve two transition metal salts, such as N,N-dimethylformamide.
[0031] According to an embodiment of the present invention, the carbon source may be selected from polymers, such as polyacrylonitrile.
[0032] According to an embodiment of the present invention, the two transition metal salts are selected from the corresponding acetates. According to an embodiment of the present invention, the cobalt salt and the copper salt can be selected from the corresponding acetates, such as cobalt acetate and copper acetate.
[0033] According to an embodiment of the present invention, the mass ratio of the cobalt element in the cobalt salt, the copper element in the copper salt and polyacrylonitrile is (1-2.5):1:(15-30), for example (1.2-2):1:(20-25), and exemplarily 1.7:1:24.
[0034] According to an embodiment of the present invention, the electrostatic blending method can encapsulate the prepared electrospinning precursor solution through a 50mL medical syringe, and the syringe is equipped with a 0.8mm stainless steel needle. As an example, the electrostatic blending method adopts the following parameters: the high voltage between the positive and negative electrodes is 20kV, the injection rate of the automatic injection pump is 1mL / min, and the distance between the syringe needle and the stainless steel receiving net is 15cm.
[0035] According to an embodiment of the present invention, the pre-oxidation temperature may be 250-350°C. The specific process may be, for example, heating to 250-300°C at a rate of 0.5-10°C / min, and maintaining the pre-oxidation temperature of 250-300°C for 0.5-5h; for example, heating to 300-350°C at a rate of 5-8°C / min, and then maintaining the temperature of 300-350°C for 1-5h. As an example, heating to 300°C at a rate of 5°C / min and maintaining for 1h stabilizes the pre-oxidation of the nanofibers.
[0036] According to an embodiment of the present invention, the carbonization temperature is 700-1100° C., for example, 800-900° C. The high temperature carbonization process can be, for example, heated to 700-1100° C. at a rate of 1-10° C. / min, and the carbonization temperature of 700-1100° C. is maintained for 0.5-5 h, for example, heated to 800-900° C. at a rate of 5° C. / min, and the carbonization temperature of 800-900° C. is maintained for 1 h; preferably, an inert atmosphere is maintained throughout the carbonization process, such as nitrogen, helium, argon atmosphere, or a mixed atmosphere of two or more thereof.
[0037] According to an embodiment of the present invention, the preparation method further comprises grinding the carbonized product.
[0038] Preferably, the method for preparing the catalyst comprises the following steps:
[0039] 1) adding polyacrylonitrile, cobalt salt and copper salt into an organic solvent to obtain a stable and uniform mixed solution;
[0040] 2) preparing nano polymer fibers containing cobalt salt and copper salt by electrostatically spinning the mixed solution of step 1);
[0041] 3) pre-oxidizing the nano polymer fiber of step 2), wherein the pre-oxidation temperature is 250-300° C.;
[0042] 4) carbonizing the pre-oxidized nano-polymer fibers obtained in step 3) in an inert atmosphere at a temperature of 700 to 1100° C.;
[0043] 5) Grinding the product obtained in step 4) to obtain the catalyst.
[0044] According to an embodiment of the present invention, in step 1), a stable and uniform mixed solution, such as a uniform colloidal solution, can be obtained by stirring. As an example, the stirring can be carried out using a medium or large magnetic stirring bar, such as a rotor with a diameter greater than 0.5 cm. There is no particular restriction on the rotation speed and stirring time of the rotor, as long as a stable and uniform mixed solution can be obtained. As an example, the rotation speed can be 200 to 2000 r / min, such as 500 to 1500 r / min, 1000 r / min, and the stirring time can be 1 to 10 h, such as 2 to 4 h.
[0045] According to an embodiment of the present invention, in step 3), the pre-oxidation can stabilize the nano polymer fiber. The pre-oxidation can be carried out in an air atmosphere in a tubular high temperature furnace to allow the nano polymer fiber to fully react, such as cyclization, dehydrogenation and oxidation.
[0046] According to an embodiment of the present invention, during the carbonization process, carbon-hydrogen, carbon-nitrogen, and nitrogen-hydrogen bonds inside the fiber undergo condensation reactions, the fibers are cross-linked with each other, and the carbon nanofibers finally formed present a certain spatial structure.
[0047] Preferably, the carbonized nano-polymer fibers are taken out after the furnace temperature drops to room temperature.
[0048] The present invention also provides the use of the above catalyst in degrading organic pollutants. Preferably, the organic pollutants are antibiotics, such as nitroimidazoles, sulfonamides, fluoroquinolones, tetracyclines, macrolides, chloramphenicols, β-lactams and other antibiotics, preferably nitroimidazole antibiotics. As an example, the antibiotics are one or more of metronidazole, tinidazole, ornidazole and the like.
[0049] In one embodiment, the catalyst is used to degrade metronidazole in an aqueous environment.
[0050] According to an embodiment of the present invention, the catalyst degrades organic pollutants in a persulfate and / or percarbonate oxidation system.
[0051] Beneficial effects of the present invention:
[0052] (1) The bimetallic carbon nanofiber catalyst degrades antibiotic pollutants by activating persulfate and peroxycarbonate to produce active free radicals, and its catalytic effect is much better than that of the monometallic carbon nanofiber catalyst.
[0053] (2) The transition metals in the catalyst are confined within the carbon nanofiber lattice, which effectively prevents metal leakage. The positions of the two transition metals in the catalyst are close or identical, which, combined with the conductivity of the carbon nanofibers, helps to produce a synergistic effect between the two transition metals and the metals.
[0054] (3) The catalyst has soft magnetic properties, and its hysteresis and coercive force are very small. It can be collected and recycled by a magnet after the reaction, and is environmentally friendly to a certain extent.
[0055] (4) The catalyst has catalytic effect in both persulfate and percarbonate oxidation systems. The product has high stability. In the persulfate oxidation system, it can maintain a degradation efficiency of more than 84% for antibiotics after multiple uses, and in the percarbonate oxidation system, it can maintain a degradation efficiency of more than 89% for antibiotics.
[0056] (5) Electrospun nanopolymer fibers (NFs) undergo low-temperature pre-oxidation to undergo fiber cross-linking, which greatly improves the spatial structure of the fibers. After high-temperature carbonization, carbon nanofibers are formed, which give the carbon nanofibers a larger specific surface area. The metal nanoparticles and carbon fibers are firmly connected, the nanometal particles have good crystallinity and crystalline structure, and the loading amount of transition metal nanoparticles.
[0057] In summary, the catalyst has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 It is a schematic diagram of the electrostatic blended fiber device;
[0059] Figure 2 The scanning electron microscope (SEM) images of Co / NFs and Co / CNFs in Example 1;
[0060] Figure 3 TEM images (ac) and element distribution diagrams of carbon (d), oxygen (e), cobalt (f), and copper (g) of the catalyst of Example 1;
[0061] Figure 4 is the X-ray diffraction (XRD) pattern of the catalyst of Example 1;
[0062] Figure 5 The concentration change curve of the target substance in the catalyst / persulfate system of Application Example 1;
[0063] Figure 6 This is the concentration change curve of the target substance in the catalyst / percarbonate system of Application Example 2. DETAILED DESCRIPTION
[0064] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0065] Some of the reagents and instruments used in the following examples are as follows:
[0066] Polyacrylonitrile (analytical grade), Sigma-Aldrich;
[0067] Cobalt acetate (analytical grade), Sinopharm Group;
[0068] Copper acetate (analytical grade), Anaiji Chemical;
[0069] Dimethylformamide (analytical grade), Sigma-Aldrich;
[0070] Syringe Farmingdale;
[0071] Magnetic stirrer, MS-M-S1 from Asone Co., Ltd., Japan;
[0072] Vacuum tube furnace, Hefei Kejing Material Technology Co., Ltd. VBF-1200X;
[0073] High voltage power supply, Dongwen high voltage power supply.
[0074] The methods are conventional methods unless otherwise specified. The raw materials can be obtained from public commercial channels unless otherwise specified.
[0075] Example 1
[0076] Weigh 41.4 g of N,N-dimethylformamide, 0.75 g of cobalt acetate, 0.474 g of copper acetate, and 3.6 g of polyacrylonitrile into a beaker, add a medium-sized magnetic stir bar, place on a magnetic stirrer, set the speed to 300 rpm, and stir for 2 h until all dissolved. The electrostatic blending fiber device used is as follows Figure 1 As shown, the prepared electrospinning precursor solution is encapsulated with a 50mL medical syringe, and a 0.8mm stainless steel needle is installed in the syringe. The high voltage between the positive and negative electrodes is set to 20kV, the injection rate of the automatic injection pump is 1mL / min, the distance between the syringe needle and the stainless steel receiving net is 15cm, and the electrospun nanopolymer fibers (NFs) on the stainless steel receiving net are collected every 2h. The electrospun fibers collected on the receiving net are folded and placed in a corundum crucible for pre-oxidation and carbonization. The crucible is placed in a tubular furnace, heated to 300℃ (heating rate 5℃ / min) in an air atmosphere for 60min, and maintained for 1h to complete the pre-oxidation stabilization of the nanofibers. The carbonization process is heated to 800℃ (heating rate 5℃ / min) in 250min, and maintained in a nitrogen atmosphere for 60min to complete the carbonization process. After the carbonization process is completed, nitrogen is continued to be introduced until the temperature of the entire system drops to room temperature. The crucible is taken out, and the carbon nanofibers obtained after pre-oxidation and carbonization are ground into powder using an agate mortar and sealed in a sample bottle to obtain the catalyst (abbreviated as Cu-Co / CNFs) for use.
[0077] Figure 2 The left picture shows the morphology of NFs, which have a smooth surface, no nodules, good spatial structure, and an average fiber diameter of about 300nm; the right picture shows the morphology of carbonized nanofibers (CNFs) in the catalyst. CNFs show good spatial structure, excellent fiber cross-linking ability and surface integrity, and the fiber diameter is about 300nm.
[0078] Figure 3 The results show that the diameter of cobalt and copper nanoparticles is about 30-50nm, and they are evenly distributed in the carbon nanofibers with good dispersion and no metal agglomeration. The two metals are distributed close to each other, which is conducive to the synergistic effect between the metals. The test and analysis results of crystal morphology and lattice structure show that the spacing between adjacent lattice planes of nano-metal elements in carbon nanofibers is 0.205 and 0.209nm, respectively, corresponding to the (111) plane of cobalt element and the (111) plane of copper element. This result is consistent with the test results of XRD.
[0079] Figure 4 It shows that the Cu-Co / CNFs catalyst has characteristic peaks of both elemental copper and elemental cobalt, among which the characteristic peak of copper is sharper than the characteristic diffraction peak of cobalt, indicating that the copper element has a relatively high crystallinity.
[0080] In the catalyst, the loading amount of the cobalt nanoparticles is 0.016 wt %, and the loading amount of the copper nanoparticles is 0.01 wt %.
[0081] Comparative Example 1
[0082] The preparation process of the carbon nanofiber catalyst (Cu / CNFs) loaded with only elemental copper is different from that of Example 1 in that cobalt acetate is not added to the electrospinning precursor solution.
[0083] Comparative Example 2
[0084] The preparation process of the carbon nanofiber catalyst (Co / CNFs) loaded with only elemental copper is different from that of Example 1 in that copper acetate is not added to the electrospinning precursor solution.
[0085] Application Example 1
[0086] Taking metronidazole as the target decomposition product, a catalytic degradation experiment was carried out in a persulfate system. The concentration of metronidazole was set to 0.12mM, the concentration of persulfate was set to 0.5mM, and the dosage of the catalyst was 0.1g / L. Comparative Example 1, a carbon nanofiber catalyst loaded with elemental copper, Comparative Example 2, a carbon nanofiber loaded with elemental cobalt, and Example 1 Cu-Co / CNFs were used as catalysts for oxidative decomposition comparison experiments. Figure 5The results show that the catalytic oxidation decomposition rate of the target substance of Cu-Co / CNFs within 60 minutes reaches 97.5%, while the degradation efficiency of carbon nanofibers loaded with only elemental cobalt and carbon nanofibers loaded with only elemental copper within 60 minutes is 5.5% and 3.4%, respectively. The embodiment proves that Cu-Co / CNFs has high catalytic efficiency.
[0087] Application Example 2
[0088] Taking metronidazole as the target decomposition product, a catalytic degradation experiment was carried out in a percarbonate system. The concentration of metronidazole was set to 0.12mM, the concentration of hydrogen peroxide was set to 500mM, the concentration of sodium bicarbonate was set to 25mM, and the dosage of the catalyst was 0.1g / L. Comparative Example 1, a carbon nanofiber loaded with elemental copper, Comparative Example 2, a carbon nanofiber loaded with elemental cobalt, and Example 1 Cu-Co / CNFs were used as catalysts for oxidative decomposition comparison experiments. Figure 6 The results showed that the catalytic oxidation decomposition rate of the target substance of Cu-Co / CNFs reached 97.4% within 60 minutes, while the degradation efficiency of carbon nanofibers loaded with only elemental cobalt and carbon nanofibers loaded with only elemental copper within 60 minutes was 8.6% and 30.6%, respectively, proving that Cu-Co / CNFs has high catalytic efficiency.
[0089] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. Use of a catalyst in the degradation of nitroimidazole antibiotics, wherein: The nitroimidazole antibiotic is one or more of metronidazole, tinidazole and ornidazole; The catalyst degrades the nitroimidazole antibiotic in a percarbonate oxidation system; The catalyst is a carbon nanofiber loaded with two transition metal nanoparticles, wherein the two transition metal nanoparticles are cobalt nanoparticles and copper nanoparticles, wherein the cobalt nanoparticles include nano zero-valent cobalt particles, and the copper nanoparticles exist in the form of nano zero-valent copper. The transition metal nanoparticles are confined and synthesized in the carbon nanofiber lattice.
2. The use according to claim 1, characterized in that: The transition metal nanoparticles are uniformly distributed in the carbon nanofibers; And / or, the loading amount of the cobalt nanoparticles is 0.005-0.05 wt %, and the loading amount of the copper nanoparticles is 0.005-0.05 wt %.
3. The use according to claim 1, characterized in that: The diameter of the carbon nanofiber is 100-500 nm; And / or, the diameter of the cobalt nanoparticles is 10-80 nm, and the diameter of the copper nanoparticles is 10-80 nm; And / or, the two transition metal nanoparticles have no agglomeration phenomenon; And / or, the distribution positions of the two transition metal nanoparticles in the carbon nanocellulose are close to or the same.
4. The use according to any one of claims 1 to 3, characterized in that: The catalyst also contains carbon and oxygen; And / or, the nano zero-valent cobalt particles are dispersed inside the carbon nanofibers; And / or, the cobalt nanoparticles further include Co3O4 nanoparticles, and the Co3O4 nanoparticles are located on the surface of the carbon nanofibers.
5. The use according to claim 1, characterized in that: The preparation method of the catalyst comprises the following steps: electrostatically blending an electrospinning precursor solution to form nano-polymer fibers containing two transition metal salts, pre-oxidizing and carbonizing the nano-polymer fibers to synthesize the catalyst; The electrospinning precursor solution includes an organic solvent, a carbon source and two transition metal salts; The organic solvent is an organic solvent that can dissolve a transition metal salt; The carbon source is selected from polymers; The two transition metal salts are selected from the corresponding acetates.
6. The use according to claim 5, characterized in that: The mass ratio of the cobalt element, the copper element and the polymer in the transition metal salt is (1-2.5):1:(15-30).
7. The use according to claim 5, characterized in that: The carbon source is polyacrylonitrile, and the two transition metal salts are selected from cobalt acetate and copper acetate.
8. The use according to claim 5, characterized in that The electrospinning method adopts the following parameters: the high voltage between the positive and negative electrodes is 20 kV, the injection rate of the automatic injection pump is 1 mL / min, and the distance between the syringe needle and the stainless steel receiving mesh is 15 cm; And / or, the pre-oxidation temperature is 250-350°C; And / or, the carbonization temperature is 700-1100°C.
9. The use according to claim 1, characterized in that: The preparation method of the catalyst comprises the following steps: 1) Adding polyacrylonitrile, cobalt salt and copper salt into an organic solvent to obtain a stable and uniform mixed solution; 2) preparing nano polymer fibers containing two transition metal salts by electrostatically spinning the mixed solution of step 1); 3) pre-oxidizing the nano polymer fiber in step 2) at a temperature of 250-300°C; 4) The pre-oxidized nano-polymer fibers obtained in step 3) are carbonized in an inert atmosphere at a temperature of 700-1100° C.; 5) Grinding the product obtained in step 4) to obtain the catalyst.
Citation Information
Patent Citations
Method for oxidation degradation of wastewater organic pollutant by activating hydrogen peroxide
CN101503241A
Method for treating organic wastewater by oxidation of bicarbonate activated load-type metal catalysts
CN102910724A
Method for in-situ preparing iron and copper dual-metal loaded carbon nano-fiber composite material
CN106835364A
Copper-cobalt bimetal / porous carbon nanofiber composite material, and preparation method and application thereof
CN108786814A
Preparation method and application for graphene multi-metal composite material
CN110015746A