Electrocatalytic materials based on iron oxyhydroxide and metal-organic frameworks
By growing Ni-MOF nanosheet arrays on foam nickel and forming γ-FeOOH on its surface, forming γ-FeOOH/Ni-MOF heterostructure, the problem of low performance of MOF catalysts in the prior art is solved, and efficient Electrocatalytic oxygen evolution reaction, with simple process and low cost.
Patent Information
- Application Number
- CN202211097216.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-08
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-09-08
AI Technical Summary
The prior art is difficult to accurately control the conversion of ultra-thin MOF nanosheets into hydroxide/hydroxyoxide on the basis of solution, forming a heterostructure rich in active interfaces, while maintaining the integrity of MOF structure, resulting in insufficient performance of alkaline OER catalysts.
By growing a uniform array of Ni-MOF nanosheets on foam nickel and forming γ-FeOOH on its surface after treatment with ultraviolet ozone, γ-FeOOH/Ni-MOF heterostructure is formed, the process parameters are optimized to improve electrocatalytic performance.
It realizes that the electrocatalytic oxygen evolution reaction activity is significantly improved without destroying the internal structure of the nanosheet, and is low in cost and easy to mass production. When the current density is 10mA cm-2, the overpotential is only 199mV.
Smart Images

Figure HDA0003838671190000011 
Figure HDA0003838671190000012 
Figure HDA0003838671190000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy materials and is an electrocatalytic material based on iron oxyhydroxide and a metal organic framework. Technical Background
[0002] Metal-organic frameworks (MOFs) are crystalline materials composed of organic ligands and metal nodes. Due to their diversity in structure and composition, they can be used as a potential electrocatalyst precursor. In particular, ultrathin MOFs nanoarray materials can be directly used in alkaline electrocatalytic oxygen evolution reaction (OER). However, the research on this type of catalyst is still in its infancy. In order to further enhance its electrocatalytic performance, changing the intrinsic catalytic activity of the active metal center by forming a heterogeneous structure is an effective strategy to improve the performance of the material.
[0003] At present, common catalysts for alkaline OER reactions are based on hydroxides / oxyhydroxides of transition metals such as iron, cobalt, and nickel. Under appropriate reaction conditions, the above materials can be reversibly transformed with MOFs, thus providing the possibility of constructing their heterogeneous interface structures. However, the process of ultrathin MOF nanosheets converting into hydroxides / oxyhydroxides and forming abundant interfacial active metal sites is difficult to precisely control, because the degradation of the former and the formation of the latter inevitably occur simultaneously during the solution-based reaction process. Therefore, there are few reports on the construction of heterogeneous structures with rich active interfaces while maintaining the structural integrity of MOFs. Summary of the invention
[0004] The present invention provides an oxygen evolution electrocatalyst based on a heterojunction formed by iron oxyhydroxide (γ-FeOOH) and a metal organic framework (MOF) and a preparation method thereof. In the method, a high-efficiency OER electrocatalyst is prepared by further forming γ-FeOOH on the surface of MOF after ultraviolet ozone treatment, and the process parameters and raw material types in the preparation process are selected and optimized, thereby solving the problem of low catalytic efficiency of traditional noble metal catalysts.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] The present invention provides an electrocatalytic material based on a heterostructure of γ-FeOOH and MOF nanosheet arrays. A uniform and clearly morphological nickel-based MOF nanosheet array (Ni-MOFNA) is grown on nickel foam, because the introduction of iron has a significant effect on the improvement of catalytic performance. Therefore, by further treating Ni-MOFNA, it is hoped that iron oxyhydroxide can be grown on the surface without destroying the internal structure of the nanosheets. After synthesis, XRD, HRTEM and other characterizations show that γ-FeOOH is generated on the surface to form a γ-FeOOH / Ni-MOF heterostructure. Various electrochemical tests prove that the performance is significantly improved.
[0007] Specifically, an electrocatalytic material based on a heterostructure of γ-FeOOH and MOF nanosheet arrays, wherein the electrocatalytic material based on iron oxyhydroxide and a metal organic framework is prepared by the following method:
[0008] (1) Preparation of Ni-MOFNA: dripping an aqueous solution of nickel acetate into an anhydrous ethanol solution of 2,6-naphthalene dicarboxylic acid, after the dripping is completed, a mixed solution is obtained, and nickel foam is horizontally immersed in the mixed solution, and reacted at 60°C-100°C (preferably 80°C) for 16-24 hours (preferably 20 hours) under sealed conditions, and the obtained once-treated nickel foam is washed (with ultrapure water) and dried to obtain Ni-MOFNA (nickel foam supported by nickel-based metal organic framework nanosheet array); the molar ratio of nickel acetate contained in the aqueous solution of nickel acetate to 2,6-naphthalene dicarboxylic acid contained in the anhydrous ethanol solution of 2,6-naphthalene dicarboxylic acid is 2:2.5-3 (preferably 2:3); the concentration of the aqueous solution of nickel acetate is 7-9 mg / mL (preferably 8 mg / mL); the concentration of the anhydrous ethanol solution of 2,6-naphthalene dicarboxylic acid is 9-11 mg / mL (preferably 10 mg / mL);
[0009] Note: During the subsequent treatments, the nickel foam that has been treated once should be kept facing upwards, with the front side not touching the bottom of the reaction container, to protect the microstructure of the front side.
[0010] (2) Preparation of γ-FeOOH / Ni-MOFNA: The Ni-MOFNA described in step (1) is treated with a UV ozone generator for 20 min-6 h (preferably 0.5-3 h, particularly preferably 1 h), and then placed in a ferric chloride solution and reacted at 60-100° C. (preferably 80° C.) for 20 min-24 h (preferably 2 h). The secondary treated nickel foam is washed (with ultrapure water) and dried to obtain the electrocatalytic material based on iron oxyhydroxide and metal organic framework; the concentration of the ferric chloride solution is 0.2-0.3 M (preferably 0.25 M).
[0011] Furthermore, the nickel foam in step (1) is 1.5 mm thick and has a shape of 1.5×1.5 cm 2 square.
[0012] Furthermore, in order to wash away the oxides and grease on its surface and allow the Ni-MOF to grow evenly on the substrate, the nickel foam in step (1) is also pretreated before being immersed in the mixed solution: ultrasonic cleaning is performed using 0.1-10M (preferably 3M) hydrochloric acid, acetone, ultrapure water, and ethanol as washing solutions in sequence, and ultrapure water is used for rinsing each time before changing the washing solution.
[0013] Furthermore, the nickel foam in step (1) is pretreated before being immersed in the mixed solution: ultrasonic cleaning in 0.1-10M (preferably 3M) hydrochloric acid, acetone, ultrapure water, and ethanol for 15 minutes, and rinsing with ultrapure water three times before changing the washing solution each time.
[0014] Furthermore, the solvent of the ferric chloride solution in step (2) is 1-propanol, water, ethanol or acetonitrile, preferably 1-propanol.
[0015] Furthermore, the light intensity of the ultraviolet ozone generator used in step (2) is 14-20 mW / cm 2 (Preferably 16mW / cm 2 ).
[0016] Furthermore, the volume of the ferric chloride solution taken in step (2) is 4-6 mL (preferably 5 mL).
[0017] The present invention also provides an application of the electrocatalytic material based on iron oxyhydroxide and metal organic framework in an electrocatalytic reaction.
[0018] Specifically, the application is: the electrocatalytic reaction is an electrocatalytic oxygen evolution reaction.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The uniform and clear-shaped Ni-MOFNA is grown on the nickel foam, and the addition of iron has a significant effect on the improvement of catalytic performance. Then the Ni-MOFNA is further processed to generate γ-FeOOH on the surface without destroying the internal structure of the nanosheet, forming a γ-FeOOH / Ni-MOF heterojunction, thereby improving the electrocatalytic oxygen evolution reaction activity. The method of the present invention is simple, easy to operate, low-cost, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope image of the Ni-MOFNA of Example 1.
[0022] Figure 2 This is a transmission electron microscope image of the Ni-MOFNA of Example 2 after being treated in a UV ozone machine for 1 hour.
[0023] Figure 3 This is a scanning electron microscope image of the Ni-MOFNA of Example 3 after being treated in a UV ozone machine for 1 hour and placed in a 1-propanol solution of anhydrous ferric chloride to react at 80°C for 20 minutes.
[0024] Figure 4 This is a scanning electron microscope image of the Ni-MOFNA of Example 4 after being treated in a UV ozone machine for 1 hour and placed in a 1-propanol solution of anhydrous ferric chloride to react at 80°C for 1 hour.
[0025] Figure 5 This is a scanning electron microscope image of the Ni-MOFNA of Example 5 after being treated in a UV ozone machine for 1 hour and placed in a 1-propanol solution of anhydrous ferric chloride to react at 80°C for 2 hours.
[0026] Figure 6 This is a scanning electron microscope image of the Ni-MOFNA of Example 6 after being treated in a UV ozone machine for 1 hour and placed in a 1-propanol solution of anhydrous ferric chloride to react at 80°C for 6 hours.
[0027] Figure 7 It is a performance diagram of the electrocatalytic oxygen evolution reaction of Examples 1, 2, 3, 4, 5 and 6.
[0028] Figure 8 These are the electrochemical impedance spectra of Examples 1, 2, 3, 4, 5, and 6.
[0029] Fig. 9 These are the X-ray diffraction patterns of Example 1, Example 2, Example 3, Example 4, Example 5, and Example 6. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0031] Embodiment 1:
[0032] Take 1.5mm thick nickel foam (NF) and cut it into 1.5×1.5cm 2 In order to wash away the oxides and grease on the surface of NF and make Ni-MOF grow evenly on the substrate, ultrasonic cleaning was performed in 3M hydrochloric acid solution, acetone, ultrapure water, and ethanol for 15 min, and ultrapure water was used to rinse three times each time; 8.1 mg Ni(CH3COO)2·4H2O (0.034 mol) was taken in a centrifuge tube with a balance, 1 mL ultrapure water was added and ultrasonic mixing was performed; 10.3 mg 2,6-naphthalene dicarboxylic acid (0.046 mol) was added to a glass reaction bottle, 1 mL of anhydrous ethanol was added, and the solution was dispersed as evenly as possible by ultrasonication for 60 s. The obtained Ni(CH3COO)2·4H2O solution was dripped dropwise into the glass reaction bottle containing the ethanol solution of 2,6-naphthalene dicarboxylic acid using a pipette, and the cleaned NF was put into the bottle, sealed, and transferred to an oven for reaction at 80°C for 20 h. After the reaction was completed and cooled to room temperature, the obtained sample was washed with ultrapure water and ultrasonicated for 60 s, and dried at 60°C overnight to obtain the original MOF (Ni-MOFNA).
[0033] Embodiment 2:
[0034] The Ni-MOFNA prepared according to the method of Example 1 was placed in a clean glass culture dish and irradiated with an ultraviolet ozone machine (UV-ozone cleaning machine PSD-UV8 from Novascan, USA) at a light intensity of 16 mW / cm 2 After processing, seal and store.
[0035] Embodiment 3:
[0036] Use a balance to take 4.1 mg of anhydrous ferric chloride (0.025 mol), add 100 mL of 1-propanol, and ultrasonicate for 60 seconds to disperse it as evenly as possible; take 5 mL of ferric chloride solution in a glass reaction bottle, take the Ni-MOFNA treated with ultraviolet ozone prepared according to the method of Example 2 and put it into the solution, and react at 80°C for 20 minutes; after cooling to room temperature, the obtained sample is washed with ultrapure water and ultrasonicated for 60 seconds, and dried at 60°C overnight.
[0037] Embodiment 4:
[0038] Use a balance to take 4.0 mg of anhydrous ferric chloride (0.025 mol), add 100 mL of 1-propanol, and ultrasonicate for 60 seconds to disperse it as evenly as possible; take 5 mL of ferric chloride solution in a glass reaction bottle, take the Ni-MOFNA treated with ultraviolet ozone prepared according to the method of Example 2 and put it into the solution, and react at 80°C for 1 hour; after cooling to room temperature, the obtained sample is washed with ultrapure water and ultrasonicated for 60 seconds, and dried at 60°C overnight.
[0039] Embodiment 5:
[0040] Use a balance to take 4.1 mg of anhydrous ferric chloride (0.025 mol), add 100 mL of 1-propanol, and ultrasonicate for 60 seconds to disperse it as evenly as possible; take 5 mL of ferric chloride solution in a glass reaction bottle, take the Ni-MOFNA treated with ultraviolet ozone prepared according to the method of Example 2 and put it into the solution, and react at 80°C for 2 hours; after cooling to room temperature, the obtained sample is washed with ultrapure water and ultrasonicated for 60 seconds, and dried at 60°C overnight.
[0041] Embodiment 6:
[0042] Use a balance to take 4.1 mg of anhydrous ferric chloride (0.025 mol), add 100 mL of 1-propanol, and ultrasonicate for 60 seconds to disperse it as evenly as possible; take 5 mL of ferric chloride solution in a glass reaction bottle, take the Ni-MOFNA treated with ultraviolet ozone prepared according to the method of Example 2 and put it into the solution, and react at 80°C for 6 hours; after cooling to room temperature, the obtained sample is washed with ultrapure water and ultrasonicated for 60 seconds, and dried at 60°C overnight.
[0043] Figure 1This is a scanning electron microscope image of the Ni-MOFNA of Example 1. It can be observed that the original MOF has a lamellar morphology, is evenly dispersed, and has a smooth surface.
[0044] Figure 2 This is a transmission electron microscope image of the Ni-MOFNA of Example 2 after being treated with a UV ozone machine for 1 hour. The lattice fringes of MOF are clearly visible.
[0045] Figure 3 This is a scanning electron microscope image of the Ni-MOFNA of Example 3 after being treated in a UV ozone machine for 1 hour and reacted in a 1-propanol solution of anhydrous ferric chloride at 80°C for 20 minutes. It can be observed that its morphology is lamellar and the thickness is relatively thin.
[0046] Figure 4 This is a scanning electron microscope image of the Ni-MOFNA of Example 4 after being treated with a UV ozone machine for 1 hour and reacted in a 1-propanol solution of anhydrous ferric chloride at 80°C for 1 hour. It can be observed that its morphology is lamellar and evenly dispersed, retaining the morphology of the original MOF and with more iron oxide grown on the surface.
[0047] Figure 5 This is a scanning electron microscope image of the Ni-MOFNA of Example 5 after being treated in a UV ozone machine for 1 hour and reacted in a 1-propanol solution of anhydrous ferric chloride at 80°C for 2 hours. It can be observed that the original flaky morphology is retained, and the surface is rougher.
[0048] Figure 6 This is a scanning electron microscope image of the Ni-MOFNA of Example 6 after being treated in a UV ozone machine for 1 hour and reacted in a 1-propanol solution of anhydrous ferric chloride at 80°C for 6 hours. It can be observed that a large amount of iron oxyhydroxide grows on the surface and the morphology has been severely damaged.
[0049] Figure 7 The oxygen evolution electrocatalytic performance diagram of the samples in Examples 1, 2, 3, 4, 5 and 6 shows that under different reaction times, the MOF in Example 5 grows an appropriate amount of iron oxyhydroxide on the surface without destroying the internal structure of the nanosheets, forming a γ-FeOOH / Ni-MOF heterojunction to accelerate the mass transfer and transfer of charges, and the performance is optimal. -2 Under this condition, the overpotential only needs to be 199mV.
[0050] Figure 8 The electrochemical impedance spectra of the samples in Examples 1, 2, 3, 4, 5 and 6 show that, under different reaction times, the MOF in Example 5 grows an appropriate amount of iron oxyhydroxide on the surface without destroying the internal structure of the nanosheets, forming a γ-FeOOH / Ni-MOF heterojunction to accelerate the mass transfer and transfer of charges, thereby minimizing the charge transfer resistance.
[0051] Fig. 9 The X-ray diffraction diagrams of Examples 1, 2, 3, 4, 5 and 6 show that under ultraviolet ozone and different reaction times, the XRD peaks did not shift or disappear, indicating that the crystal form of the MOF did not change.
[0052] The present invention discloses a method for preparing an electrocatalytic material by synthesizing a heterostructure of γ-FeOOH and MOF nanosheet arrays on nickel foam; the preparation method of the material is: treating Ni-MOFNA grown on nickel foam under an ultraviolet ozone machine, and then adding a metal source to form a γ-FeOOH / Ni-MOF heterojunction on the MOF surface. The present invention solves the problem of low electrocatalytic activity of the original MOF material by forming a γ-FeOOH / Ni-MOF heterojunction on the surface, and the prepared material has excellent electrocatalytic activity, and the electrocatalytic activity is 10 mA cm -2 When the overpotential is only 199mV.
Claims
1. An electrocatalytic material based on iron oxyhydroxide and metal organic framework, Features The electrocatalytic material based on iron oxyhydroxide and metal organic framework is prepared by the following method: (1) Preparation of Ni-MOFNA: dripping an aqueous solution of nickel acetate into an anhydrous ethanol solution of 2,6-naphthalene dicarboxylic acid, after the dripping is completed, a mixed solution is obtained, and nickel foam is horizontally immersed in the mixed solution, and reacted at 60°C-100°C for 16-24 hours under sealed conditions. The obtained once-treated nickel foam is washed and dried to obtain Ni-MOFNA, wherein the Ni-MOFNA is nickel foam supported by a nickel-based metal organic framework nanosheet array; the molar ratio of nickel acetate contained in the aqueous solution of nickel acetate to 2,6-naphthalene dicarboxylic acid contained in the anhydrous ethanol solution of 2,6-naphthalene dicarboxylic acid is 2:2.5-3; the concentration of the aqueous solution of nickel acetate is 7-9 mg / mL; the concentration of the anhydrous ethanol solution of 2,6-naphthalene dicarboxylic acid is 9-11 mg / mL; (2) Preparation of γ-FeOOH / Ni-MOFNA: The Ni-MOFNA described in step (1) is treated with a UV ozone generator for 0.5 to 3 hours, and then placed in a ferric chloride solution and reacted at 60-100° C. for 20 minutes to 24 hours. The secondary treated nickel foam is washed and dried to obtain the electrocatalytic material based on oxyhydroxide and metal organic framework; the concentration of the ferric chloride solution is 0.2-0.3M.
2. The electrocatalytic material based on iron oxyhydroxide and metal organic framework according to claim 1, Features: The nickel foam described in step (1) is 1.5 mm thick and has a shape of 1.5×1.5 cm 2 square.
3. The electrocatalytic material based on iron oxyhydroxide and metal organic framework according to claim 1, Features: The nickel foam in step (1) is also pretreated before being immersed in the mixed solution: ultrasonic cleaning is performed using 0.1-10M hydrochloric acid, acetone, ultrapure water, and ethanol as washing solutions in sequence, and ultrapure water is used for rinsing each time before changing the washing solution.
4. The electrocatalytic material based on iron oxyhydroxide and metal organic framework according to claim 1, Features: The solvent of the ferric chloride solution in step (2) is 1-propanol, water, ethanol or acetonitrile.
5. The electrocatalytic material based on iron oxyhydroxide and metal organic framework according to claim 1, Features: The solvent of the ferric chloride solution in step (2) is 1-propanol.
6. The electrocatalytic material based on iron oxyhydroxide and metal organic framework according to claim 1, Features: The light intensity of the UV ozone generator in step (2) is 14-20 mW / cm 2 .
7. The electrocatalytic material based on iron oxyhydroxide and metal organic framework according to claim 1, Features: The light intensity of the UV ozone generator in step (2) is 16 mW / cm 2 .
8. Use of the electrocatalytic material based on iron oxyhydroxide and metal organic framework as claimed in claim 1 in an electrocatalytic reaction.
9. The use according to claim 8, Features The application is that the electrocatalytic reaction is an electrocatalytic oxygen evolution reaction.
Citation Information
Patent Citations
Loaded type electro-catalyst for oxygen evolution reaction of electrolyzed water and preparation method thereof
CN108970617A
Cited By
Bimetal oxygen evolution pre-catalyst material based on metal organic framework as well as preparation method and application of bimetal oxygen evolution pre-catalyst material
CN119800439A