A clean concentrated fracturing fluid based on water-soluble polymer

By using a concentrated fracturing liquid composed of tap water and polar generator in oil and gas extraction, the problems of high insoluble content and high cost in water-based polymer liquid are solved, and efficient Oil and gas mining fracturing effect and environmentally friendly production process.

CN116179180BActive Publication Date: 2024-11-19SICHUAN SHENHE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310226063.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-11-19
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

The existing water-based polymer liquid concentrate fracturing liquid has high content, high cost and complex production process, making it difficult to achieve "instant injection and distribution" and efficient oil and gas exploitation fracturing effects.

Method used

Using a continuous phase composed of tap water, polarity generator, stabilizer and free water fixative, combined with water-soluble polymer, a clean concentrated fracturing liquid based on water-soluble polymer is prepared through physically changing dissolution and mixing processes. , simplify equipment processes and reduce energy consumption.

Benefits of technology

It realizes efficient water-based polymer suspension, reduces insoluble residues, improves salt resistance and reduces resistance, simplifies production processes, reduces costs, and is suitable for oil and gas mining and fracturing construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179180B_ABST
    Figure CN116179180B_ABST
Patent Text Reader

Abstract

The invention discloses a clean concentrated fracturing fluid based on a water-soluble polymer, and belongs to the technical field of increasing the production of oil and gas reservoirs. The concentrated fracturing fluid uses a continuous phase composed of tap water, a polarity generator, a stabilizer and a free water fixative as a basis, combined with a water-soluble polymer, so that the water base can suspend the water-soluble polymer, and the dissolution of the water-soluble polymer in the system is inhibited; the entire system is in a strong polar environment, which can effectively prevent the polymer molecular chain from spreading and dissolving in the system. The fracturing fluid is based on the technical problems existing in oil-based products, and then the water-based product is proposed to solve the technical problems of high insoluble content, high cost, and complex production process in the existing water-based polymer liquid concentrated fracturing fluid. The preparation method uses simple equipment and process, simple operation, low energy consumption requirements, no chemical changes, only dissolution and mixing processes, all of which are physical changes, saving costs and reducing energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil and gas reservoir production enhancement, and in particular relates to a clean concentrated fracturing fluid based on a water-soluble polymer. Background Art

[0002] At the beginning of this century, slickwater volume fracturing technology gradually matured and began to be fully applied in the United States. In the past 10 to 20 years, with the large-scale development of unconventional oil and gas reservoirs in China, the exploitation of unconventional natural oil and gas resources such as tight gas, shale gas, coalbed methane, and shale oil is mainly based on large-volume volume fracturing. The fracturing fluid used is mainly low-viscosity slickwater. At the same time, linear glue and cross-linked glue are combined, and sand fracturing is added to achieve three-dimensional transformation, forming oil and gas channels, and maximizing the permeability of the reservoir. Polyacrylamide and modified polyacrylamide have gradually become the main raw materials for oil and gas exploitation fracturing fluids at home and abroad because of their high synthetic molecular weight, low cost, and mature and stable production process. A certain viscosity can be achieved at a low dosage, and they have a high drag reduction rate under high-speed flow conditions, becoming the first choice for fracturing materials at present.

[0003] At present, the main agents of fracturing fluid can be divided into two categories according to their appearance, one is powder and the other is emulsion; the two types of fracturing fluid main agents each have their own advantages and disadvantages.

[0004] Powdered fracturing fluid polymers are mainly polyacrylamide and modified polyacrylamide, which are polymerized through aqueous solution. It is the earliest process used to synthesize high molecular weight polyacrylamide, with mature and stable production process, high molecular weight of synthesized polymer, few by-products, low cost, the polymer itself does not contain oil phase, emulsifier and other additives, excellent salt resistance, low dosage in high mineralization, good viscosity and drag reduction performance, excellent viscosity increasing performance in different water qualities, etc. It was and is still one of the most commonly used fracturing fluid main agents; however, powdered polymers have a long dissolution time and need to prepare the liquid in advance, so corresponding liquid preparation equipment and storage equipment are needed, and the construction site requirements are relatively higher, requiring a large amount of space, personnel, equipment, etc., and it is difficult to change the liquid anytime and anywhere, and it is difficult to achieve "injection and preparation", which has certain limitations.

[0005] Commonly used emulsion fracturing fluid main agents can be divided into oil-in-water reverse emulsions and suspended concentrated fracturing fluids, both of which have the performance of online mixing and do not require advance liquid preparation. Compared with powders, they can greatly reduce site requirements and do not require liquid preparation equipment. At the same time, they can change the liquid properties at any time according to the construction situation in real time; however, oil-in-water reverse emulsion polymers contain a large number of other additives, and the effective ingredients are relatively low. The salt resistance effect is average, and the viscosity-increasing performance is not particularly outstanding. Therefore, the effect on high-mineralized water quality of return fluid is poor; the main components of suspended concentrated fracturing fluids contain a large amount of mineral oil and some water-insoluble stabilizers, such as organic bentonite. These substances will cause serious damage to storage, directly affect the effective permeability of storage, and are relatively expensive, which seriously limits the promotion and large-scale application of this technology.

[0006] Patent CN108659809B discloses a method for preparing concentrated fracturing fluid based on continuous fracturing, which uses white oil as a continuous phase and adds a stabilizer organic bentonite to achieve the purpose of suspending polymers. The organic bentonite in this type of substance is water-insoluble and will introduce a large amount of residue. At the same time, white oil is used as the main raw material, which is expensive. The rest is less than that shown in the present invention. Concentrated water-soluble polymers on the current market mostly use oil as a continuous phase, and a stabilizer is added to the continuous phase to achieve the purpose of suspension. Summary of the invention

[0007] The first object of the present invention is to provide a clean concentrated fracturing fluid based on a water-soluble polymer, wherein the concentrated fracturing fluid is based on a continuous phase composed of tap water, a polarity generating agent, a stabilizer and a free water fixative, and is combined with a water-soluble polymer to achieve water-based suspension of the water-soluble polymer. The fracturing fluid is based on the technical problems existing in oil-based products, and the water-based product is proposed to solve the technical problems of high insoluble content, high cost, and complex production process in the existing water-based polymer liquid concentrated fracturing fluid.

[0008] The second object of the present invention is to provide a method for preparing a clean concentrated fracturing fluid based on a water-soluble polymer, which uses a simple equipment process, is simple to operate, has low energy consumption requirements, has no chemical changes, and only has dissolution and mixing processes, which are all physical changes, thus saving costs and reducing energy consumption.

[0009] The present invention is achieved through the following technical solutions:

[0010] A clean concentrated fracturing fluid based on a water-soluble polymer, mainly comprising, based on 100 parts by total weight: 58.0-99.0 parts of a continuous phase, 0.1-40.0 parts of a water-soluble polymer, 1.0-2.0 parts of a surface modifier, and 0.1-0.3 parts of a water vapor barrier agent;

[0011] The continuous phase is composed of tap water, a polarity generator, a stabilizer and a free water fixative;

[0012] The steps of the preparation method of the clean concentrated fracturing fluid based on water-soluble polymer are as follows:

[0013] A. Turn on the stirring device, add tap water and polarity generator in proportion, keep the temperature between 20-40°C, add stabilizer, stir and disperse, then add free water fixative until dissolved, cool to no more than 40°C, and obtain a continuous phase;

[0014] B. Transfer the continuous phase to the polymerization kettle, start stirring, add the surface modifier and water-soluble polymer in proportion, stir and disperse them evenly, then add the water vapor barrier agent, stir and mix, and the mixture is complete.

[0015] Preferably, the mass fractions of the raw materials in the continuous phase are: 24.5-34.5 parts of tap water, 22.5-28.0 parts of polarity generator, 1.3-1.5 parts of stabilizer, and 42-46 parts of free water fixative.

[0016] Preferably, the polarity generating agent is industrial ethanol having an ethanol content of not less than 95 wt%.

[0017] Preferably, the polarity generating agent is a stabilizer including any one of nano-silicon dioxide, xanthan gum and modified xanthan gum;

[0018] Preferably, the stabilizer is nano-silicon dioxide.

[0019] The above is preferably nano-silicon dioxide, which is based on the principle that it has a large specific surface area, a spherical microstructure, a flocculent and mesh-like quasi-particle structure and a three-dimensional mesh structure, so that its surface has good anti-sedimentation performance.

[0020] Preferably, the polarity generating agent is a free water fixing agent, which is any one of anhydrous calcium chloride, anhydrous calcium chloride and anhydrous magnesium chloride, or anhydrous calcium chloride and magnesium chloride hydrate salt;

[0021] The anhydrous calcium chloride accounts for at least 65% of the total weight of the free water fixative.

[0022] Preferably, the water-soluble polymer is anion-modified polyacrylamide;

[0023] The anionic modified polyacrylamide includes one or any combination of modified polyacrylamide obtained by homopolymerization, modified polyacrylamide obtained by post-hydrolysis, and modified polyacrylamide containing salt-tolerant monomers.

[0024] The modified polyacrylamide selected as the water-soluble polymer has no restriction on molecular weight.

[0025] Preferably, the surface modifier is an anionic surfactant or a nonionic surfactant.

[0026] The surface modifier is sodium dodecyl sulfate, but is not limited to sodium dodecyl sulfate. Anionic or nonionic surfactants with equivalent functions may be used.

[0027] Preferably, the water vapor barrier agent is one or more of light white oil, solvent oil and diesel.

[0028] Preferably, in the A, a stabilizer is added and stirred and dispersed for 20-30 minutes;

[0029] The polarity generator is added and mixed for 5-10 minutes.

[0030] Preferably, in B, a surface modifier and a water-soluble polymer are added and fully stirred and dispersed for 30-40 minutes;

[0031] The water vapor barrier agent is added and stirred for 10-15 minutes.

[0032] Compared with the prior art, the present invention has at least the following technical effects:

[0033] (I) The present invention provides a clean concentrated fracturing fluid based on a water-soluble polymer, which is prepared by ① adding a free water fixative and a polarity generator to water, which not only has good anti-swelling performance, but also forms a super-strong charge environment, thereby inhibiting the dissolution of the water-soluble polymer in the system; ② the free water fixative mainly utilizes its principle of easy absorption of water to absorb and fix the free water in the system into "calcium chloride bound water", so that it cannot be transferred to the polymer molecular chain; ③ the polarity generator is added mainly by utilizing the strong polarity of alcohol to put the entire system in a strong polarity environment, which can effectively prevent the polymer molecular chain from spreading and dissolving in the system; ④ the stabilizer is added to effectively achieve long-term uniform dispersion and stability of the polymer in the continuous phase, ⑤ the surface interface regulator sodium dodecyl sulfate is added at the same time, which can effectively change the surface interface tension of the liquid, and ⑥ the water vapor shielding agent is added to form a protective film on the surface of the system to prevent water vapor from passing through the protective film, thereby effectively preventing the water vapor that may be generated by temperature changes from condensing to form water droplets, and at the same time, due to the low friction coefficient of the oil, the fluidity of the system has a certain promoting effect.

[0034] (ii) The above-mentioned entire production process has simple equipment and process, simple operation, low energy consumption requirements, no chemical changes, only dissolution and mixing processes, which are all physical changes. Therefore, if the stirring time is too short, it is easy to cause insufficient mixing, and if the time is too long, it will invisibly increase energy consumption, waste time, and increase costs. Therefore, it is sufficient to mix evenly. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 To verify the fourth point, the oil-based concentrated fracturing fluid currently on the market was dissolved and degelled in tap water at 1%, and the degelled fluid was left to stand for 24 hours;

[0036] Figure 2 To verify the fourth point, the oil-based concentrated fracturing fluid currently on the market was dissolved and degelled in 30,000 standard brine at 1%, and the degelled fluid was left to stand for 24 hours;

[0037] Figure 3 To verify the fourth, the water-based concentrated fracturing fluid of Example 2 was dissolved and degelled in tap water at 1%, and the degelled fluid was left to stand for 24 hours;

[0038] Figure 4 To verify the fourth, the water-based concentrated fracturing fluid of Example 2 was dissolved and degelled in 30,000 standard brine at 1%, and the degelled fluid was left to stand for 24 hours;

[0039] Figure 5 The appearance of the base solution obtained by dissolving the base solution in tap water and 20,000 standard saline dilution solution at a dosage of 0.5% in Example 3;

[0040] Figure 6 To verify the fifth point, the appearance of the base fluid obtained by dissolving the oil-based concentrated fracturing fluid on the market in tap water and 20,000 standard brine dilution at a dosage of 0.5%;

[0041] Figure 7 Example 4 was dissolved in tap water at 80°C and 170S at a dosage of 1.0%. -1 Rheological curve of constant temperature and constant speed shear for 90 min;

[0042] Figure 8 The 2.0% added amount of Example 4 was dissolved in 20,000 standard saline dilution at 80°C and 170S -1 Rheological curve of constant temperature and constant speed shear for 90 min;

[0043] Fig. 9 The Example 5 was dissolved in tap water at a dosage of 0.1%, and the drag reduction rate curve was measured under the conditions of 8 mm pipe diameter and 10 m / s flow rate;

[0044] Fig.10 The Example 5 was dissolved in 40,000 standard saline dilution solution at a dosage of 0.1%, and the drag reduction rate curve was measured under the conditions of 8 mm pipe diameter and 10 m / s flow rate;

[0045] Fig.11 A clean concentrated fracturing fluid based on a water-soluble polymer prepared in Example 8;

[0046] Fig.12This is a schematic diagram of the preparation method of Example 1. DETAILED DESCRIPTION

[0047] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0048] Unless otherwise specified, the chemicals involved in the examples can be obtained by conventional means.

[0049] Unless otherwise specified, the percentage signs "%" in the examples are all mass percentages.

[0050] Embodiment 1:

[0051] A clean concentrated fracturing fluid based on a water-soluble polymer, the composition of which is shown in Table 1 below:

[0052]

[0053]

[0054] Note: The percentage of dispersed phase raw materials is the percentage of the entire concentrated fracturing fluid system, and the percentage of continuous phase raw materials is only the percentage of continuous phase.

[0055] The water-soluble polymer is a modified polyacrylamide SFR-3 drag reducer for fracturing provided by Sichuan Shenhe New Material Technology Co., Ltd. The modified polyacrylamide is prepared by polymerization of acrylamide, sodium acrylate and sodium 2-acrylamide-2-methylpropane sulfonate through aqueous solution.

[0056] The above-mentioned specific preparation method is as follows: Fig.12 As shown:

[0057] (1) In a batching kettle, start stirring and add 27.7 parts of tap water in proportion, add 1.3 parts of nano-silicon dioxide while stirring, stir and disperse for 20-30 minutes, then add anhydrous calcium chloride, stir and cool to less than 40°C, add 28.0 parts of industrial alcohol, mix and stir for 5-10 minutes, stop stirring, and the continuous phase is prepared, and transfer it to a polymerization kettle. (2) Start stirring the polymerization kettle, and the speed can form a vortex. Add sodium dodecyl sulfate and modified polyacrylamide in the polymerization kettle in turn, stir and disperse for 30-40 minutes, add a water vapor barrier agent, stir and mix for 10-15 minutes, and obtain a concentrated fracturing fluid with an effective polymer concentration of 40.0%.

[0058] The concentrated fracturing fluid prepared as above was left to stand naturally for 2 months without any stratification and precipitation, and maintained good fluidity. Moreover, after being placed at 50° C. for 48 hours, there was still no swelling, and the fluidity was still maintained very well.

[0059] Verification 1: According to "SY-T 5107-2005 Water-based Fracturing Fluid Performance Evaluation Method" and "NBT14003.2-2016 Drag Reducing Agent Performance Index and Test Method", the concentrated fracturing fluid obtained in Example 1 was added according to the proportions in the following table, dissolved in different water qualities, and its kinematic viscosity, apparent viscosity and drag reduction rate were measured, as shown in Table 2:

[0060]

[0061]

[0062] From the experimental data in Table 2, it can be seen that the concentrated fracturing fluid has good solubility in different water qualities and is less affected by the mineralization. When the addition amount of concentrated fracturing fluid is ≥0.5%, the apparent viscosity is completely unaffected by the water quality in tap water, 20,000 standard brine dilution and 40,000 standard brine dilution.

[0063] When the concentrated fracturing fluid is added less than 0.5%, in the 20,000 and 40,000 standard brine dilutions, the kinematic viscosity is almost unaffected by the mineralization of the brine, showing good salt resistance. At the same time, the measured drag reduction rate is greater than 70%, which can well meet the technical indicators of greater than 70% required in "NBT14003.2-2016 Drag Reducing Agent Performance Indicators and Test Methods", indicating that the concentrated fracturing fluid has good drag reduction performance when dissolved in water, and can well meet the requirements of oil and gas extraction fracturing construction.

[0064] Verification 2: According to the method in "SY / T 5107-2005 Water-based Fracturing Fluid Performance Evaluation Method", the concentrated fracturing fluid obtained in Example 1 was dissolved in water according to the following addition ratio, 0.03% of the breaker (ammonium persulfate) was added, and the breaker was broken at a constant temperature of 90°C for 2 hours, cooled to room temperature, and the surface interfacial tension of the breaker was measured. At the same time, the anti-swelling effect of the breaker was measured with reference to "SY / T5971-2016 Clay Stabilizer Performance Evaluation Method for Oil and Gas Field Fracturing Acidification and Water Injection". The experimental results are shown in Table 3 below: Surface interfacial tension and anti-swelling rate of the breaker measured by dissolving and breaking in different water qualities.

[0065]

[0066]

[0067] From the experimental data in Table 3, it can be seen that the surface tension of the degelling fluid under different conditions is ≤25mN / m, the interfacial tension is less than or equal to 2.0mN / m, and the surface and interfacial tensions are all less than the standard in "SY / T7627-2021 Technical Requirements for Water-Based Fracturing Fluids", which is: the surface and interfacial tensions of the technical requirements for slick water and linear gel fracturing fluids are less than 32.0mN / m and 3.0mN / m, respectively. This shows that the concentrated fracturing fluid has a good ability to reduce the surface interface after being dissolved in water, which is conducive to the return of the fracturing fluid after degelling.

[0068] At the same time, whether the addition ratio is lower than 0.5% or higher than 0.5%, the anti-swelling rate of the tested gel-breaking fluid is greater than 80%, which is much higher than the technical requirement of an anti-swelling rate greater than 60% in the "SY / T7627-2021 Technical Requirements for Water-Based Fracturing Fluids". This shows that the gel-breaking fluid has a good anti-swelling effect, which helps to better protect the permeability of oil and gas reservoirs; it shows that the highly concentrated fracturing fluid described in the invention has good comprehensive properties such as anti-swelling and reducing the surface interface, and has good application value.

[0069] Embodiment 2:

[0070] The composition of a clean concentrated fracturing fluid based on a water-soluble polymer is shown in Table 4:

[0071]

[0072]

[0073] Remarks: Same as Example 1.

[0074] The water-soluble polymer is selected the same as in Example 1.

[0075] The specific preparation method is as follows: the raw material addition ratio is as recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 35.0% is obtained.

[0076] Verification 3: The concentrated fracturing fluid obtained in Example 2 was compared with the oil-based concentrated fracturing fluid on the existing market. Both were dissolved in different waters according to a certain ratio. 0.03% of the breaker ammonium persulfate was added to the base fluid, and the gel was broken at a constant temperature of 90°C for 2 hours. Then, the residue content and viscosity of the broken gel fluid were determined according to the method in "SY / T 5107-2016 Water-based Fracturing Fluid Performance Evaluation Method". The experimental data are shown in Table 5:

[0077]

[0078]

[0079] It can be seen from the experimental data in Table 5 that the residue content of the concentrated fracturing fluid obtained in Example 2 after gel breaking is much lower than the residue content of the oil-based concentrated fracturing fluid on the existing market, and the residue content is much lower than the technical requirement of the gel breaking liquid residue content ≤100 mg / L in the linear gel fracturing fluid in "SY / T 5107-2016 Performance Evaluation Method for Water-Based Fracturing Fluid", indicating that the residue content of the concentrated fracturing fluid is cleaner.

[0080] Verification 4: The concentrated fracturing fluid of Example 2 and the oil-based concentrated fracturing fluid on the market were dissolved in tap water and 30,000 standard brine at 1.0%, and 0.03% of ammonium persulfate as a breaker was added. The broken gel solution was obtained at 90°C for 2 hours. The broken gel solution was left to stand for 24 hours for observation. After 24 hours, the states of the broken gel solution were as follows: Figure 1 , Figure 2 , Figure 3 , Figure 4 shown.

[0081] like Figure 1 As shown, it is a schematic diagram of the state of the oil-based concentrated fracturing fluid currently on the market being dissolved and degelled in tap water at 1%, and the degelled fluid being left standing for 24 hours; (1) is a top view; (2) is a front view.

[0082] like Figure 2 As shown, it is a schematic diagram of the state of the oil-based concentrated fracturing fluid currently on the market being dissolved and degelled in 30,000 standard brine at 1%, and the degelled fluid being left standing for 24 hours; (1) is a top view; (2) is a front view.

[0083] from Figure 1 and Figure 2 After standing for 24 hours, it was found that after the oil-based concentrated fracturing fluid was broken in tap water and brine, a large number of floating objects visible to the naked eye were distributed on the surface, and the broken fluid was relatively turbid after being left for a long time, indicating that the broken fluid contained a large amount of insoluble matter, because the system contained a large amount of organic bentonite stabilizer, which could not be dissolved in water. At the same time, the organic bentonite stabilizer was modified from a cationic monomer, and had a certain incompatibility with anionic polymers, and could also produce a certain amount of insoluble residue.

[0084] like Figure 3 As shown, the water-based concentrated fracturing fluid of Example 2 is dissolved in tap water at 1%, degelled, and the degelled liquid is left to stand for 24 hours; (1) is a top view; (2) is a front view.

[0085] like Figure 4 As shown, the water-based concentrated fracturing fluid of Example 2 is dissolved and degelled in 30,000 standard brine at 1%, and the degelled liquid is left to stand for 24 hours; (1) is a top view; (2) is a front view.

[0086] from Figure 3 and Figure 4After the water-based concentrated fracturing fluid was degelled in tap water and salt water and left to stand for 24 hours, the degelled liquid was clear and transparent, without any floating objects on the surface and any precipitation at the bottom, indicating that the concentrated fracturing fluid of Example 2 above is more environmentally friendly and less harmful to the reservoir; this is because there is no insoluble matter in the system and it can be well dissolved and dispersed in water.

[0087] Example 3

[0088] A clean concentrated fracturing fluid based on a water-soluble polymer has a composition as shown in Table 6;

[0089]

[0090] Remarks: Same as Example 1.

[0091] The water-soluble polymer provided is the same as in Example 1.

[0092] The specific preparation method is as follows: the raw materials are added in the proportions recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 30.0% is obtained.

[0093] Verification 5: The concentrated fracturing fluid prepared in Example 3 was dissolved in tap water and 20,000 standard brine at a ratio of 0.5%.

[0094] Verification results: Figure 5 The appearance of the base solution obtained by dissolving the base solution in tap water and 20,000 standard saline solution at a dosage of 0.5% in Example 3; (1) in the figure is tap water; (2) is saline solution.

[0095] Figure 6 The appearance of the base fluid obtained by dissolving the oil-based concentrated fracturing fluid on the market at a dosage of 0.5% in tap water and 20,000 standard brine dilution liquid respectively; (1) in the figure is tap water; (2) is brine.

[0096] contrast Figure 5 and Figure 6 It can be found that the concentrated fracturing prepared in Example 3 is dissolved in different water qualities at a ratio of 0.5% to obtain a base fluid with a clear and transparent appearance without any visible residue. Figure 6 It can be found that the fracturing fluid base fluid prepared from the oil-based concentrate on the existing market has a turbid appearance, indicating that it contains a lot of intolerant residues; this further proves the cleanliness and low harm of the concentrated fracturing prepared in Example 3.

[0097] Example 4

[0098] A clean concentrated fracturing fluid based on a water-soluble polymer, the composition of which is shown in Table 7:

[0099]

[0100] Remarks: Same as Example 1.

[0101] The water-soluble polymer is provided in the same manner as in Example 1.

[0102] The specific preparation method is as follows: the raw materials are added in the proportions recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 25.0% is obtained.

[0103] Verification 6: The concentrated fracturing fluid prepared in Example 4 was dissolved in tap water and 20,000 standard brine dilution at a ratio of 1.0% and 2.0%, respectively, and then heated at 80°C and 170S -1 Shear at constant temperature and constant speed for 90 min.

[0104] Figure 7 Example 4 was dissolved in tap water at 80°C and 170S at a dosage of 1.0%. -1 Rheological curve of constant temperature and constant speed shear for 90 min; Figure 8 The 2.0% added amount of Example 4 was dissolved in 20,000 standard saline dilution at 80°C and 170S -1 Rheological curve of constant temperature and constant shearing speed for 90 min.

[0105] pass Figure 7 and Figure 8 It can be seen that at 80℃, 170S -1 After 90 minutes of constant temperature and constant speed shearing under the conditions, the viscosity is greater than 130mP.s, indicating that it has good heat and shear resistance after being dissolved in water, and can well meet the technical indicators of heat and shear resistance ≥20mPa.s in the technical requirements of linear gel fracturing fluid in "SY / T7627-2021 Technical Requirements for Water-based Fracturing Fluid", indicating that it has good application performance in both tap water and salt water.

[0106] Example 5

[0107] A clean concentrated fracturing fluid based on a water-soluble polymer, the composition of which is shown in Table 8:

[0108]

[0109]

[0110] Remarks: Same as Example 1.

[0111] The water-soluble polymer is provided in the same manner as in Example 1.

[0112] The specific preparation method is as follows: the raw material addition ratio is as recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 20.0% is obtained.

[0113] Verification 7: The concentrated fracturing fluid prepared in Example 5 was dissolved in tap water and 40,000 standard brine dilution at an addition amount of 0.1%, and its drag reduction rate was measured at a pipe diameter of 8 mm and a flow rate of 10 m / s.

[0114] Fig. 9 The Example 5 was dissolved in tap water at a dosage of 0.1%, and the drag reduction rate curve was measured under the conditions of 8 mm pipe diameter and 10 m / s flow rate; Fig.10 The Example 5 was dissolved in 40,000 standard saline dilution solution at an addition amount of 0.1%, and the drag reduction rate curve was measured under the conditions of 8 mm pipe diameter and 10 m / s flow rate.

[0115] from Fig. 9 and Fig.10 It can be seen that whether in tap water or 40,000 standard brine dilution liquid, the drag reduction rate is greater than 70%, and the highest drag reduction rate reaches 75%, which fully meets the technical indicators of the drag reduction rate of low-viscosity and slippery water required by the "SYT7627-2021 Technical Requirements for Water-based Fracturing Fluids" that is greater than 70%, indicating that it has excellent salt resistance and drag reduction performance, and it has good application value.

[0116] Example 6

[0117] A clean concentrated fracturing fluid based on a water-soluble polymer, the composition of which is shown in Table 9:

[0118]

[0119]

[0120] Remarks: Same as Example 1.

[0121] The water-soluble polymer provided is the same as in Example 1.

[0122] The specific preparation method is as follows: the raw material addition ratio is as recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 15.0% is obtained.

[0123] Example 7

[0124] A clean concentrated fracturing fluid based on a water-soluble polymer, the composition of which is shown in Table 10:

[0125]

[0126] Remarks: Same as Example 1.

[0127] The water-soluble polymer provided is the same as in Example 1.

[0128] The specific preparation method is as follows: the raw materials are added in the proportions recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 10.0% is obtained.

[0129] Example 8

[0130] A clean concentrated fracturing fluid based on a water-soluble polymer, the composition of which is shown in Table 11:

[0131]

[0132] Remarks: Same as Example 1.

[0133] The water-soluble polymer provided is the same as in Example 1.

[0134] The specific preparation method is as follows: the raw materials are added in the proportions recorded in the above table, and the preparation process is the same as that in Example 1. A concentrated fracturing fluid with an effective polymer concentration of 5.0% is obtained.

[0135] like Fig.11 The present invention is a finished product of a clean concentrated fracturing fluid based on a water-soluble polymer prepared in the above Example 8.

[0136] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A clean concentrated fracturing fluid based on a water-soluble polymer, characterized in that: Based on 100 parts by total weight, the composition includes: 58.0-99.0 parts of continuous phase, 0.1-40.0 parts of water-soluble polymer, 1.0-2.0 parts of surface modifier, and 0.1-0.3 parts of water vapor barrier agent; The continuous phase is composed of tap water, a polarity generator, a stabilizer and a free water fixative; The mass fractions of the raw materials in the continuous phase are: 24.5-34.5 parts of tap water, 22.5-28.0 parts of polarity generating agent, 1.3-1.5 parts of stabilizer, and 42-46 parts of free water fixing agent; The polarity generating agent is industrial ethanol with an ethanol content of not less than 95wt%; The stabilizer is nano silicon dioxide; The free water fixing agent is any one of anhydrous calcium chloride, anhydrous calcium chloride and anhydrous magnesium chloride, and anhydrous calcium chloride and magnesium chloride hydrate salt; The anhydrous calcium chloride accounts for at least 65% of the total weight of the free water fixative; The water-soluble polymer is anion-modified polyacrylamide; The anionic modified polyacrylamide includes one or any combination of modified polyacrylamide obtained by homopolymerization, modified polyacrylamide obtained by post-hydrolysis, and modified polyacrylamide containing salt-tolerant monomers; The surface modifier is an anionic surfactant or a nonionic surfactant; The water vapor barrier agent is one or more of light white oil, solvent oil and diesel oil; The steps of the preparation method of the clean concentrated fracturing fluid based on water-soluble polymer are as follows: A. Turn on the stirring device, add tap water and polarity generator in proportion and mix for 5-10 minutes, keep the temperature between 20-40°C, then add stabilizer, stir and disperse for 20-30 minutes, then add free water fixative until dissolved, cool to no more than 40°C, and obtain a continuous phase; B. Transfer the continuous phase to the polymerization kettle, start stirring, add the surface modifier and water-soluble polymer in proportion, stir and disperse them for 30-40 minutes, add the water vapor barrier agent after it is evenly distributed, stir and mix for 10-15 minutes, and the mixture is completed.