Yttrium-doped barium magnesium fluoride transparent ceramic and its preparation method and application
By controlling the raw material ratio and sintering process, yttrium-doped magnesium barium fluoride transparent ceramics with high transmittance and uniformity were prepared, solving the problems of opacity and inhomogeneity of existing transparent ceramic materials and realizing the application of high-efficiency deep ultraviolet lasers.
Patent Information
- Application Number
- CN202310500790.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing transparent ceramic materials suffer from opacity and inhomogeneity during the preparation process, which affects the generation and application of lasers, especially in deep ultraviolet all-solid-state lasers. Furthermore, traditional magnesium barium fluoride crystals suffer from cracking, long preparation cycles, low efficiency, and high costs.
By using yttrium-doped magnesium barium fluoride transparent ceramic material and controlling the molar ratio of barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride to (100-150):(100-150):(5-12):(750-900), combined with water bath method and vacuum hot pressing sintering process, yttrium-doped magnesium barium fluoride powder with small particle size, uniformity and no agglomeration was prepared, solving the problems of opacity and non-uniformity.
Yttrium-doped magnesium barium fluoride transparent ceramics with high transmittance and small and uniform grain size were prepared. The transmittance reached more than 50.5% in the 400-800nm wavelength range, which solved the problems of transparency and uniformity in the prior art and maintained nonlinear characteristics, making it suitable for large-scale industrial production.
Smart Images

Figure CN116514552B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a new material, in particular to a yttrium-doped barium magnesium fluoride transparent ceramic and a preparation method and application thereof. Background Art
[0002] Any discussion of the prior art throughout the specification should not be considered as an admission that such prior art is widely known or forms part of the common general knowledge in the field.
[0003] In order to meet the scientific research and production needs in the fields of ultraviolet lithography, high-resolution emission spectroscopy, photonic device manufacturing, micro-nano processing, and pharmaceutical synthesis, the research on deep ultraviolet all-solid-state lasers has attracted widespread attention at home and abroad. Compared with the commonly used solid laser materials limited to cubic structures (such as CaF2, Y2O3, Lu2O3, and YAG), low-symmetry system materials working at shorter wavelengths (below 200nm) have higher luminous efficiency and greater development potential.
[0004] Barium magnesium fluoride (BaMgF4, orthorhombic system, space group Cmc21, point group mm2) is a nonlinear crystal with the advantages of extremely short ultraviolet cutoff wavelength (125nm), wide transmittance range from deep ultraviolet to mid-infrared (126nm-13μm) and full-band quasi-phase matching capability, making it an ideal candidate material for deep ultraviolet all-solid-state lasers. Studies have shown that quasi-phase matching frequency conversion can be achieved in periodically polarized BaMgF4 crystals in the visible and ultraviolet spectral regions, and the shortest conversion wavelength obtained in ultraviolet light is 368nm. However, due to the problems of cracking, long preparation cycle, low efficiency and high overall cost in the preparation process of BaMgF4 crystals, it is difficult to apply them in large quantities.
[0005] Compared with single crystals, ceramic laser technology has the advantages of short production cycle, low manufacturing cost, and convenient processing. The prepared laser ceramics often have more advantages than ordinary optical materials, such as high strength, high insulation, corrosion resistance, high temperature resistance, etc., and have good light transmittance. They can be made into a variety of electro-optical and electro-mechanical military and civilian dual-use devices, and have broad application prospects in space science, laser, infrared detection, special instrument manufacturing, electronic technology and high temperature technology, aerospace and national defense equipment. However, as a polycrystalline material, the incompleteness of the grain boundaries, pores, and lattices inside ceramics will lead to the opacity and unevenness of the material and increase the light scattering loss, thereby affecting the generation of lasers. Therefore, the difficulty in preparing transparent laser ceramics currently lies mainly in light transmittance and uniformity.
[0006] The purpose of the present invention is to overcome or improve at least one disadvantage of the prior art, or to provide a useful alternative. Unless the context clearly requires otherwise, throughout the specification and claims, the words "include", "comprises", etc. should be interpreted from an inclusive perspective rather than an exclusive or exhaustive perspective; that is, from the perspective of "including, but not limited to". Summary of the invention
[0007] The present invention provides a transparent ceramic material and a preparation method and application thereof. The transparent ceramic material of the present invention is high-purity yttrium-doped magnesium barium fluoride, with magnesium barium fluoride as the matrix and yttrium as the doping element. The transparent ceramic material has a smaller grain size, higher transmittance and good nonlinear characteristics. The present invention also provides a preparation method of yttrium-doped magnesium barium fluoride transparent ceramics. The yttrium-doped magnesium barium fluoride powder prepared by the improved water bath method has a small particle size, is uniform without agglomeration, is pure phase without impurities, is highly active and is easy to sinter, which solves the difficult problems of opacity and unevenness of the currently prepared magnesium barium fluoride transparent ceramics.
[0008] Specifically, the technical solution of the present invention is as follows:
[0009] In the first aspect of the present invention, the present invention provides a transparent ceramic material, which is obtained by sintering magnesium barium fluoride as a matrix and yttrium as a doping element, wherein the barium ion (Ba 2+ ), magnesium ion (Mg 2+ ), yttrium ion (Y 3+ ) and fluoride ion (F - )'s molar ratio is (100-150):(100-150):(5-12):(750-900).
[0010] In an embodiment of the present invention, the barium ions (Ba 2+ ), magnesium ion (Mg 2+ ), yttrium ion (Y 3+ ) and fluoride ion (F - ) are respectively derived from barium salts, magnesium salts, yttrium salts and fluoride salts, and the barium salts, magnesium salts, yttrium salts and fluoride salts are barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride respectively.
[0011] In the present invention, the raw materials of the ceramic directly affect the structure and properties of the ceramic. The inventors have found in existing research and further implementation that, for example, magnesium fluoride barium fluoride powders made of magnesium fluoride, barium fluoride and trifluoroacetic acid often have thermal stability problems, and an amorphous mixture of magnesium fluoride and barium fluoride will exist in the product, making it difficult to obtain a pure product; for example, replacing magnesium fluoride and barium fluoride with barium carbonate and magnesium acetate can improve the thermal stability of the powder, but the powder particle size is too large, often exceeding 0.5 μm. On this basis, rhenium nitrate is tried to be added, and it is found that the addition of rare earth ion rhenium easily causes the particles to form aggregates and irregular particles, and the purity still needs to be improved; and, in some embodiments, In the embodiment, an attempt is made to change the type of fluoride, such as using ammonium bifluoride, and using barium nitrate and magnesium nitrate as raw materials at the same time, so that the magnesium barium fluoride prepared has a reduced powder particle size, but the powder particles are easy to agglomerate and the particle size distribution is uneven; in some other embodiments, magnesium chloride and barium chloride are used as raw materials, and terbium chloride is used as a raw material and ammonium fluoride is added, so that the magnesium barium fluoride powder obtained has good dispersibility, but the particle size of the powder particles is too large at the micron level. Although the particle size problem can be improved by controlling the ion concentration, the improvement is limited and it is difficult to further control the particle growth and obtain nanometer-scale powders, and the addition of other organic solvents will reduce the purity of the product. In addition, in some embodiments, magnesium barium fluoride prepared with magnesium chloride, barium chloride, ytterbium nitrate and / or erbium nitrate and potassium fluoride as raw materials also has the problem of too large separation particle size and too large grain size; and the optical transmittance of the magnesium barium fluoride ceramic material obtained in the above embodiments is often general, which needs to be improved.
[0012] In the technical solution of the present invention, in order to provide transparent ceramics with high optical quality, the present invention uses barium magnesium fluoride as a matrix, yttrium as a doping element, and magnesium chloride, barium chloride, yttrium nitrate and potassium fluoride as raw materials, and controls the molar ratio of barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride to be (100-150): (100-150): (5-12): (750-900).
[0013] Among them, Y 3+ The doping can prevent the growth of magnesium barium fluoride powder particles, which is beneficial to the preparation of magnesium barium fluoride powder with small and uniform particle size, and can also alleviate the concentration quenching effect caused by the aggregation of other ions.
[0014] In addition, in the present invention, the ratio between the raw materials will also affect the structure and performance of the ceramic material. In the present invention, the molar ratio of barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride is controlled at (100-150): (100-150): (5-12): (750-900). For example, potassium fluoride is added in this amount and mixed with other raw materials in this ratio for at least two reasons: one is to increase the number of fluoride ions when reacting with barium ions and magnesium ions in the solution, that is, to make the cations such as barium ions and magnesium ions in the solution react completely; the other is that excess fluoride ions have a certain effect of reducing the particle size of magnesium barium fluoride powder after the reaction, but the excess should also be within the above limits. This situation can be explained as follows: Since the magnesium barium fluoride crystal cell is composed of anions (MgF6) 4- and cations (Ba 2+ ), and the anion group (MgF6) 4- It shows an octahedral shape with Mg atoms as the center and F atoms surrounding it, arranged in a zigzag shape on one axis, and connected to a layered plate-like structure through the vertices on the other axis, so there must be a part of fluoride ions inside the unit cell. In the process of synthesizing the sample, because the fluoride ions exceed the corresponding standard stoichiometry, there are many fluoride ions in the solution. When the concentration of fluoride ions in the solution increases, the mutual repulsion of FF ions increases, and the strong resistance generated will squeeze the unit cell and inhibit the growth of sample particles, resulting in a smaller particle size of magnesium barium fluoride particles and a shape closer to spherical. According to sintering theory, in general, the finer the particle size of the raw material powder, the higher the density during sintering, and the corresponding internal porosity and sintering temperature will also be reduced. In addition, under the condition of the same particle size, the particle shape of the ceramic powder also has a certain influence on the density of the ceramic after sintering. The more complex the shape of the powder particles, the worse its fluidity will be, the easier it will be to form an arch bridge phenomenon (powder when stacking, due to the irregular surface, there is friction between each other, adjacent particles bridge each other to form an arch bridge shape), which will cause the ceramic density to decrease, directly have an adverse effect on sintering. Therefore, the magnesium barium fluoride powder with a surface shape close to spherical is selected to reduce the sintering temperature of the magnesium barium fluoride powder and improve the density of the magnesium barium fluoride transparent ceramic sintered body. Therefore, in the sintering process of magnesium barium fluoride ceramic, the synthesized magnesium barium fluoride powder particle size is on the small side, and the shape is close to spherical. During the reaction, the amount of fluoride ions in the solution can play a certain benefit for the sintering of high-quality magnesium barium fluoride ceramics. However, the inventors also found that the powder particle size is too fine and can cause adjacent magnesium barium fluoride particles to adhere to each other. After the magnesium barium fluoride particles are agglomerated, the average particle size will be increased on the one hand, and impurities will be easily adsorbed on the other hand, affecting the sintering performance, which will lead to a reduction in the strength of the ceramic after sintering.
[0015] In an embodiment of the present invention, the yttrium-doped barium magnesium fluoride transparent ceramic of the present invention has a smaller grain size and better visible light transmittance, wherein the grain size is ≤3 μm, the maximum transmittance is ≥50.5% in the visible light band of 400-800 nm, and the minimum transmittance is ≥48.3%.
[0016] Of course, in the embodiments of the present invention, the numerical range includes all the values within this range, and includes the range value composed of any two values within this range, and these combinations can cover all possible situations, including the minimum value, the maximum value and any value in between; for example, taking the amount of barium chloride as 100-150 mol, the amount of magnesium chloride as 100-150 mol, the amount of yttrium nitrate as 5-12 mol and the amount of potassium fluoride as 750-900 mol as an example, it can be understood that the above-mentioned dosage range can be proportionally expanded or reduced without affecting the proportional relationship between the substances, such as the amount of each substance is reduced by 1000 times; therefore, in the above-mentioned assumed dosage range The amount of each substance is selected within a range or further reduced range, and the ratio or ratio range of the amount of the four raw materials obtained by any combination is within the scope of the present invention. For example, the amount of barium chloride or magnesium chloride can be further reduced to 100-110mol, 100-120mol, 100-130mol, 100-140mol, 110-150mol, 120-150mol, 130-150mol, 140-150mol, 110-120mol, 110-130mol, 110-140mol, 120-130mol, 120-140mol, 130-140mol l, 100mol, 110mol, 120mol, 130mol, 140mol or 150mol, etc. The amount of yttrium nitrate can be further reduced to 6-12mol, 7-12mol, 8-12mol, 9-12mol, 10-12mol, 11-12mol, 5-7mol, 5-8mol, 5-9mol, 5-10mol, 5-11mol, 6-7mol, 6-8mol, 6-9mol, 6-10mol, 6-11mol, 7-8mol, 7-9mol, 7-10mol, 7-11mol, 8-9mol, 8-10mol 1, 8-11 mol, 9-10 mol, 9-11 mol, 10-11 mol, 5 mol, 6 mol, 7 mol, 8 mol, 9 mol, 10 mol, 11 mol or 12 mol and the like, the amount of potassium fluoride can be further reduced to 780-900 mol, 800-900 mol, 850-900 mol, 750-780 mol, 750-800 mol, 750-850 mol, 780-800 mol, 780-850 mol, 800-850 mol, 750 mol, 780 mol, 800 mol, 850 mol or 900 mol.
[0017] For example, in some preferred embodiments, the molar ratio of barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride is selected from the following ratio combinations: (150:100:5:750), (120:140:8:780), (100:150:12:900), (100:100:5:750), (150:150:12:900), (110:120:6:800), (130:140:9:850), (140:110:8:800), (130:130:12:800), (140:100:12:850), (110:100:7:750) and (100:120:6:800). In these embodiments, the particle size of the yttrium-doped barium magnesium fluoride powder described in the present invention is smaller and more uniform, with a size range of 50-100nm, almost no agglomeration, and therefore has better sintering activity. The grain size of the yttrium-doped barium magnesium fluoride material is 1-3μm, and can be better up to 1-2μm or 2-3μm, and has good optical transmittance, with a maximum transmittance of ≥50.5% and a minimum transmittance of ≥48.3% in the visible light band of 400-800nm, and its composition has not changed compared with the composition of the magnesium barium fluoride ceramic phase, and still has nonlinear characteristics.
[0018] In the process of ceramic preparation, raw material synthesis and ceramic sintering are two key steps, which directly affect the structure and performance of the ceramic. The purity, morphology, particle size, dispersion and other factors of the powder determine the sintering activity and density of the ceramic, which in turn affect the transparency and uniformity of the ceramic. Therefore, in order to prepare magnesium barium fluoride transparent ceramics with high optical quality, the present invention strictly controls and optimizes the powder so that it has the characteristics of uniformity without agglomeration, pure phase without impurities, high activity and easy sintering. And provide a better method for preparing yttrium-doped magnesium barium fluoride transparent ceramic material.
[0019] Therefore, in the second aspect of the present invention, the present invention provides a method for preparing the transparent ceramic material described in the first aspect, namely, yttrium-doped magnesium barium fluoride transparent ceramic material, which comprises: preparing an aqueous solution 1 with barium salt, magnesium salt and yttrium salt, and preparing an aqueous solution 2 with fluoride salt; pouring the aqueous solution 2 into the aqueous solution 1 under stirring to obtain an emulsion 3, and continuing to stir; placing the emulsion 3 in a water bath for heating, standing after the heating, centrifuging, washing and drying the emulsion 3 after standing, and grinding after drying to obtain yttrium-doped magnesium barium fluoride powder; sintering the powder to obtain a transparent ceramic material. Wherein, the barium salt, magnesium salt, yttrium salt and fluoride salt are barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride, respectively.
[0020] In some embodiments of the present invention, the barium ion (Ba 2+ ), magnesium ion (Mg 2+ ), yttrium ion (Y3+ ) and fluoride ion (F - ) is (100-150): (100-150): (5-12): (750-900). This ratio range or the ratio within this range or the combination of ratio ranges can, as described in the first aspect of the present invention, increase the amount of fluorine ions when reacting with barium ions and magnesium ions in the solution, so that the cations such as barium ions and magnesium ions in the solution react completely; and reduce the particle size of magnesium barium fluoride powder after the reaction within a suitable degree, improve the uniformity, make the shape of the powder particles closer to spherical, but make the particle size of the powder not too fine to cause undesirable aggregation such as adhesion, thereby reducing the sintering temperature and increasing the density of the sintered body.
[0021] In the embodiments of the present invention, the numerical range includes all the values within the range, and includes the range values composed of any two values within the range, and these combinations can cover all possible situations, including the minimum value, the maximum value and any value in between; for example, taking the amount of barium chloride as 100-150 mol, the amount of magnesium chloride as 100-150 mol, the amount of yttrium nitrate as 5-12 mol and the amount of potassium fluoride as 750-900 mol as an example, it can be understood that the above-mentioned dosage range can be proportionally expanded or reduced without affecting the proportional relationship between the substances, for example, the amount of each substance is reduced by 1000 times; therefore, in the above-mentioned assumed dosage range or The amount of each substance is selected within a further narrowed range, and the ratio or ratio range of the amount of the four raw materials obtained by any combination is within the scope of the present invention. For example, the amount of barium chloride or magnesium chloride can be further reduced to 100-110mol, 100-120mol, 100-130mol, 100-140mol, 110-150mol, 120-150mol, 130-150mol, 140-150mol, 110-120mol, 110-130mol, 110-140mol, 120-130mol, 120-140mol, 130-140mol , 100mol, 110mol, 120mol, 130mol, 140mol or 150mol, etc., the amount of yttrium nitrate can be further reduced to 6-12mol, 7-12mol, 8-12mol, 9-12mol, 10-12mol, 11-12mol, 5-7mol, 5-8mol, 5-9mol, 5-10mol, 5-11mol, 6-7mol, 6-8mol, 6-9mol, 6-10mol, 6-11mol, 7-8mol, 7-9mol, 7-10mol, 7-11mol, 8-9mol, 8-10mol , 8-11mol, 9-10mol, 9-11mol, 10-11mol, 5mol, 6mol, 7mol, 8mol, 9mol, 10mol, 11mol or 12mol and so on, the amount of potassium fluoride can be further reduced to 780-900mol, 800-900mol, 850-900mol, 750-780mol, 750-800mol, 750-850mol, 780-800mol, 780-850mol, 800-850mol, 750mol, 780mol, 800mol, 850mol or 900mol.
[0022] For example, in some preferred embodiments, the molar ratio of barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride is selected from the following ratio combinations: (150:100:5:750), (120:140:8:780), (100:150:12:900), (100:100:5:750), (150:150:12:900), (110:120:6:800), (130:140:9:850), (140:110:8:800), (130:130:12:800), (140:100:12:850), (110:100:7:750) and (100:120:6:800). In these embodiments, the particle size of the yttrium-doped barium magnesium fluoride powder described in the present invention is smaller and more uniform, with a size range of 50-100nm, and almost no agglomeration, so the sintering activity is better, and the grain size of the yttrium-doped barium magnesium fluoride ceramic material obtained by sintering the powder is 1-3μm, and can reach 1-2μm or 2-3μm, and has good optical transmittance, with a maximum transmittance of ≥50.5% and a minimum transmittance of ≥48.3% in the visible light band of 400-800nm, and its composition has not changed compared with the composition of the magnesium barium fluoride ceramic phase, and still has nonlinear characteristics.
[0023] In an embodiment of the present invention, the concentration of barium ions or magnesium ions in the aqueous solution 1 is in the range of 0.5-1.5 mol / L, and the concentration of fluoride ions in the aqueous solution 2 is in the range of 1-1.5 mol / L. In a more preferred embodiment, the concentration range of barium ions in the aqueous solution 1 is selected from the following: 0.5-1.5mol / L, 0.5-1mol / L, 0.5-0.8mol / L, 0.5-0.93mol / L, 0.5-0.73mol / L, 0.5-0.7mol / L; the concentration range of magnesium ions in the aqueous solution 1 is selected from the following: 0.5-1.5mol / L, 0.5-1.2mol / L, 0.5-1mol / L, 0.5-0.93mol / L, 0.5-0.73mol / L, 0.5-0.67mol / L; the concentration range of fluoride ions in the aqueous solution 2 is selected from the following: 1-1.36mol / L, 1-1.33mol / L, 1-1.30mol / L.
[0024] Generally speaking, for the reaction system with gas or solution (except solid or pure liquid) participating, if the concentration of reactant increases, the reaction rate is accelerated, and the concentration of reactant decreases, the reaction rate slows down. But the inventor finds that in the reaction of the present invention, the size of the anion and cation solution concentration of the reaction has a certain influence on the particle diameter of magnesium barium fluoride powder particles, and the reason for this phenomenon is mainly the solution reacted under two different concentrations, and their supersaturation difference is very large. It can be known by classical nucleation growth theory that the higher the supersaturation, the less the energy required for nucleation, so the system will have a higher nucleation rate. Therefore, compared with the low concentration reaction system, the system supersaturation of high reaction concentration is larger, which makes it mainly based on particle growth in low concentration solution and mainly based on nucleation in high concentration solution, so the reaction under high concentration is more conducive to obtaining magnesium barium fluoride powder particles with smaller particle diameter.
[0025] In an embodiment of the present invention, in the above preparation method, the aqueous solution 2 is poured into the aqueous solution 1 under stirring to react to obtain the emulsion 3, and the stirring is continued. In some embodiments, the stirring time is 30-60 minutes or 40-60 minutes.
[0026] In the present invention, the role of stirring is to strengthen the convection of the mixed solution after the anion and cation solutions are mixed, enhance the material transfer in the anion and cation mixed solution, and maintain the uniform concentration of anions, cations and reaction products in each area of the reaction system. The reaction can proceed without stirring, but this will seriously hinder mass transfer. The anion and cation reaction only relies on gravity and diffusion, which will not only make the concentration of reactants and even products uneven, but also take more time.
[0027] In an embodiment of the present invention, the water bath temperature is 60-80°C.
[0028] In an embodiment of the present invention, as described in the above preparation method, the emulsion 3 is placed in a water bath for heating and then allowed to stand after the heating is completed. In some embodiments, the temperature in the water bath is 60-80°C, the reaction time is 10-30min, and the standing time is 60-120min; or in some embodiments, the temperature in the water bath is 70-80°C, the reaction time is 20-30min, and the standing time is 90-120min.
[0029] A water bath is a method of using water as a hot bath material. Since the water temperature is at most 100°C under standard atmospheric pressure, the maximum temperature of the water bath is 100°C. For example, the method of using the water bath method to process container products can be: immerse the container that needs a water bath in a larger container filled with water, and the container that needs a water bath must not be in direct contact with the larger container, and then place the larger container on a heat source for heating, stop heating when the temperature reaches an appropriate level, and take out the water bath container after cooling. The advantage of the water bath method is that it avoids the excessive intensity and uncontrollability of temperature caused by direct heating, and can heat steadily. In the present invention, the water bath heating can make the anion and cation mixed solution evenly heated while strictly controlling the water bath reaction temperature, avoiding the uneven particle size of the magnesium barium fluoride particles caused by local overheating or overcooling of the anion and cation mixed solution, thereby obtaining higher quality magnesium barium fluoride powder particles.
[0030] In an embodiment of the present invention, in the above preparation method, the emulsion 3 after standing is centrifuged. In some embodiments, the number of centrifugation is not less than 4 times, and the centrifugation time each time is not less than 20 minutes. Alternatively, in some embodiments, the number of centrifugation is not less than 5 times, and the centrifugation time each time is not less than 25 minutes.
[0031] Centrifugal separation is a separation process based on the difference in density between solid particles and the surrounding liquid, which accelerates the sedimentation of solid particles of different densities in a centrifugal field. When the suspension is left to stand, the solid particles with higher density gradually sink under the action of gravity, and this process is called sedimentation. When the particles are finer and the solution viscosity is larger, the sedimentation rate is slow, and it takes longer to achieve the purpose of separating the particles from the suspension. If centrifugal technology is used, the particle sedimentation process can be accelerated and the sedimentation time can be shortened. Because the solid concentrate produced by centrifugation is different from the concentrate produced by filtration, centrifugation can usually only obtain a more concentrated suspension or slurry, while filtration can obtain a filter cake with a lower moisture content. Compared with filtering equipment, centrifugal equipment is expensive, but in the present invention, the solid particles are small and difficult to filter, and it is more effective to select centrifugal operation, which can better achieve the separation of solid solute particles with smaller particle size from liquid solvent in the present invention.
[0032] Sintering refers to the process in which powder or formed green body gradually becomes a densified body with a certain geometric shape and a strong sintered body under the action of high temperature, through the mutual bonding and material transfer between particles of the green body, the elimination of pores, volume shrinkage, and strength improvement. Observing the sintering phenomenon at the macro and micro levels, it can be seen that, at the macro level, the volume of the sintered product shrinks, the density increases, and the strength increases. At the micro level, the shape of the pores changes and the crystals grow. According to the changes in the sintering process, sintering is mainly divided into the early sintering stage and the late sintering stage. In the early sintering stage, as the sintering temperature increases, atomic diffusion intensifies, the voids shrink, the particles change from point contact to surface contact, the voids shrink, the connected pores become closed, and are distributed in isolation. Small particles first appear grain boundaries, the grain boundaries move, and the grains become larger. In the late sintering stage, the main thing is the elimination of pores and the growth of grains. The substances on the grain boundaries continue to diffuse into the pores, so that the pores are gradually eliminated, and at the same time the grain boundaries move and the grains grow. Sintering can control the growth of grains, which has a vital impact on the performance of the material. So far, ceramic sintering technology has been an area where people continue to make breakthroughs.
[0033] Ceramic sintering can be mainly divided into liquid phase sintering and solid phase sintering, and they correspond to different reaction mechanisms. Liquid phase sintering refers to the sintering process of a multi-component system in which the sintering temperature is higher than the melting point or eutectic temperature of the low-melting component of the sintering system, or the powder sintering process in which a liquid phase appears during the sintering process. Solid phase sintering refers to the process in which the mixed powder or sample diffuses mutually at high temperature, so that the microscopic discrete particles gradually form a continuous solid structure. In the present invention, the sintering of yttrium-doped barium magnesium fluoride transparent ceramics belongs to solid phase sintering. According to the structural characteristics of the sintered body, the solid phase sintering mechanism can be divided into three stages: the initial sintering stage, the middle sintering stage and the late sintering stage. Initial sintering: In the initial sintering stage, the particles are close to each other, and the contact points between different particles form necks through material diffusion and body contraction. At this stage, the grains in the particles do not change, and the shape of the particles remains basically unchanged. Mid-sintering: The sintering neck begins to grow, atoms migrate to the particle bonding surface, the distance between particles is reduced, and a continuous pore network is formed. The density and strength of the sintered body are increased at this stage. Late sintering: Generally, when the density of the sintered body reaches 90%, the sintering enters the late sintering stage. At this time, most of the pores are separated, and the materials on the grain boundaries continue to diffuse and fill the pores. As the densification continues, the grains continue to grow. In this stage, the sintered body shrinks mainly through the disappearance of small pores and the reduction of the number of pores, but the shrinkage is slow.
[0034] In the present invention, the yttrium-doped barium magnesium fluoride transparent ceramic of the present invention is prepared by vacuum hot pressing sintering. Vacuum sintering refers to the sintering process of a ceramic body under vacuum conditions, and vacuum sintering belongs to the method of pressureless sintering. Under a vacuum environment, a pressure difference is formed between the inside of the ceramic and the outside world, which is conducive to the discharge of pores, reduces the porosity of the ceramic, and makes the grains grow to form a ceramic material with a higher density. The vacuum environment can also inhibit the decomposition of the ceramic under high temperature conditions or the volatilization of elements. This method has the advantages of simple operation, low cost, and high production efficiency. It is the most widely used transparent ceramic sintering technology. Some oxide-based ceramic materials, such as rare earth activated YAG, Y2O3 and Al2O3 ceramic materials, can be prepared by vacuum sintering. Hot pressing sintering is to place powder or ceramic body in a mold, generally a high melting point metal or graphite mold, and apply a certain pressure to the ceramic body while sintering at high temperature, and complete the sintering process in a short time. The obtained ceramic has high density and fine grains. This method can directly sinter the ceramic blank, and can also combine the molding process and the sintering process into one and perform them simultaneously. The vacuum hot pressing sintering used in the present invention is a process in which loose powder placed in a mold of a limited shape or a powder compact is heated and pressure is applied to it under a vacuum environment, so that the material molding and sintering are completed simultaneously. Vacuum hot pressing sintering has the following advantages: during hot pressing, the powder is in a thermoplastic state, with low deformation resistance and low required molding pressure; since heating and pressurization are carried out simultaneously, it is conducive to the contact, diffusion and flow mass transfer of powder particles, which can reduce the sintering temperature and shorten the sintering time, thereby inhibiting grain growth; hot pressing sintering is completed under vacuum conditions, and the sintered body obtained has low porosity, high degree of densification, and fine grains, and the mechanical and electrical properties of the product are good. Among them, increasing the sintering temperature is beneficial to mass transfer such as solid-phase diffusion, but too high a temperature will promote secondary crystallization and deteriorate the material properties. The low-temperature stage of sintering is mainly surface diffusion, and the high-temperature stage is mainly volume diffusion. If the low-temperature sintering time is too long, it is not good for densification and the performance of the material will deteriorate. Therefore, high-temperature short-time sintering is usually used to improve the density of the material. At the same time, the heating rate cannot be too fast. If the heating rate is too fast, the various parts of the blank in the mold will be heated differently, thereby changing the sintering conditions of each part, resulting in different forces on each part, causing the blank to crack or even break. Therefore, the heating rate during the heating process should be kept within a certain range to prevent the product from cracking. The molding pressure of the blank is also crucial to the performance of the material. The greater the molding pressure, the tighter the contact between the particles in the blank, and the smaller the diffusion resistance during sintering; but too high a molding pressure may cause the blank to fracture brittlely. In the present invention, by controlling the heating rate, sintering temperature, sintering pressure and other processes during the sintering of yttrium-doped magnesium barium fluoride transparent ceramics, it is more conducive to obtaining pure phase yttrium-doped magnesium barium fluoride transparent ceramics with higher transmittance.
[0035] Therefore, in the present invention, the preferred sintering method is vacuum hot pressing sintering, and the vacuum degree during sintering is not higher than 5×10 -3 Pa, sintering temperature is 650-850℃.
[0036] In some preferred embodiments, the vacuum hot pressing sintering process of the present invention is: at a temperature not higher than 5×10 -3 In a vacuum environment of 1.5 Pa, the temperature is raised from room temperature to 300-350°C at a rate of 20-40°C / min, kept warm for 1-2 hours, and then raised to 650-850°C at a rate of 10-20°C / min, kept warm for 5-8 hours. This process can better control the sintering process and is more conducive to obtaining pure phase yttrium-doped magnesium barium fluoride transparent ceramics with higher transmittance. Of course, the parameters in the sintering process can be selected within the above range or within a further narrowed range, for example, the sintering temperature can be 650°C, 750°C, 850°C, or a temperature range formed by these temperatures, or any value within the temperature range formed.
[0037] In the third aspect of the present invention, the present invention provides an optical element or optical device, which comprises the transparent ceramic material described in the first aspect above, or is prepared from the transparent ceramic material described in the first aspect above.
[0038] The yttrium-doped barium magnesium fluoride transparent ceramic of the present invention has a relatively small grain size, which is ≤3 μm, a maximum transmittance of ≥50.5% and a minimum transmittance of ≥48.3% in the visible light band of 400-800 nm, and the ceramic phase composition does not change after sintering. The main diffraction peaks in its XRD diagram can correspond one-to-one with the standard card of barium magnesium fluoride, and the nonlinear characteristics are maintained. The ceramic can be used as a nonlinear crystal, for example, it can be used to make a laser.
[0039] In a fourth aspect of the present invention, the present invention provides an application of the yttrium-doped barium magnesium fluoride transparent ceramic material described in the first aspect in the optical field. For example, the transparent ceramic material can be used as a nonlinear photonic crystal in the optical field, such as for preparing optical elements or optical devices, such as lasers.
[0040] Compared with the prior art, the advantages of the present invention are:
[0041] The invention provides a yttrium-doped magnesium barium fluoride transparent ceramic material, provides a brand-new raw material composition and a preparation process, wherein barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride are used as raw materials and a specific raw material dosage relationship is provided. The technical scheme enables the yttrium-doped magnesium barium fluoride powder to have a smaller and more uniform particle size, a narrow size distribution in the range of 50-100nm, and almost no agglomeration, so the sintering activity is good, and after sintering, the composition of the magnesium barium fluoride ceramic phase does not change compared with that of the magnesium barium fluoride ceramic phase, and still has nonlinear characteristics, especially the ceramic sample prepared by sintering has higher purity, the grain size of the sample is ≤3μm, the maximum transmittance in the visible light band of 400 to 800nm is ≥50.5%, and the minimum transmittance is ≥48.3%. At the same time, the phase composition of the material does not change before and after sintering, and the nonlinear characteristics of the material are maintained, thereby solving the difficulties of opacity and unevenness in the preparation of transparent ceramics at present.
[0042] In addition, the raw materials used in the present invention are simple, an improved water bath method is adopted, the reaction involved is highly efficient, the requirements for the reaction environment are low, the product is pure and free of impurities, and it is more suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The drawings constituting part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. The implementation scheme of the present application is described in detail below in conjunction with the drawings, wherein:
[0044] Figure 1 This is the XRD pattern of the yttrium-doped barium magnesium fluoride powder prepared in Examples 1-3 of the present invention.
[0045] Figure 2 This is a SEM image of the yttrium-doped barium magnesium fluoride powder prepared in Example 1 of the present invention.
[0046] Figure 3 These are XRD patterns of yttrium-doped barium magnesium fluoride transparent ceramic samples prepared at different sintering temperatures in Examples 1-3 of the present invention.
[0047] Figure 4 This is a SEM image of the ceramic cross-section of the yttrium-doped barium magnesium fluoride powder prepared in Example 1 of the present invention after vacuum hot pressing and sintering.
[0048] Figure 5 This is a graph showing the transmittance of the yttrium-doped barium magnesium fluoride transparent ceramic prepared in Example 1 of the present invention in the range of 390-1000nm. DETAILED DESCRIPTION
[0049] The present application is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.
[0050] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in this application can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in this application are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the content described herein can be applied to the method of this application. The preferred implementation methods and materials described in the text are for demonstration purposes only.
[0051] Example 1 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0052] Solution 1 was prepared by dissolving 0.15 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O) and 0.005 mol of yttrium nitrate (Y(NO3)3·6H2O) in 200 mL of water, and solution 2 was prepared by dissolving 0.75 mol of potassium fluoride (KF·2H2O) in 750 mL of water.
[0053] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0054] The obtained emulsion 3 was placed in a water bath at 60°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0055] The obtained product was centrifuged at 12000 r / min (30 min, 4 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0056] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, heat from room temperature to 300℃ at a rate of 30℃ / min and keep warm for 1h; then heat to 650℃ at a rate of 10℃ / min, pressurize to 30MPa and keep warm for 5h.
[0057] The yttrium-doped magnesium barium fluoride transparent ceramic obtained in this example was double-sided polished, and its density was measured to be >99.7%. The XRD curve of the yttrium-doped magnesium barium fluoride powder obtained in this example is shown in FIG. Figure 1(a) By comparing with the standard PDF card of magnesium barium fluoride, it can be found that the main diffraction peaks can obviously correspond one to one, which indicates that higher purity magnesium barium fluoride powder particles are synthesized by the improved water bath method. Figure 2 This is a SEM image of the yttrium-doped barium magnesium fluoride powder prepared in Example 1 of the present invention. It can be seen from the image that the particle size of the barium magnesium fluoride powder is relatively small, ranging from 50 to 100 nm, and there is almost no agglomeration, so the sintering activity is good. Figure 3 The XRD pattern of the yttrium-doped barium magnesium fluoride transparent ceramic obtained in this example is compared with the standard card of barium magnesium fluoride, and it can be seen that the main diffraction peaks can correspond one to one, indicating that the phase composition of the barium magnesium fluoride ceramic after sintering has not changed. Figure 4 This is a scanning electron microscope photo of the ceramic cross section after vacuum sintering of magnesium barium fluoride powder. From the photo, it can be seen that the microstructure of the sample after sintering of magnesium barium fluoride powder is uniform, there is no residual pores, and the grain size is 1-3μm. Figure 5 The transmittance diagram of the yttrium-doped barium magnesium fluoride transparent ceramic obtained in this example shows that the fewer pores and smaller grain size inside the ceramic are beneficial to the improvement of its transparency, and the maximum transmittance in the visible light band of 400 to 800 nm reaches 50.5%. Specific process parameters and sample properties are shown in Table 1.
[0058] Example 2 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0059] Solution 1 was prepared by dissolving 0.12 mol of barium chloride (BaCl2·2H2O), 0.14 mol of magnesium chloride (MgCl2·6H2O) and 0.008 mol of yttrium nitrate (Y(NO3)3·6H2O) in 150 mL of water, and solution 2 was prepared by dissolving 0.78 mol of potassium fluoride (KF·2H2O) in 600 mL of water.
[0060] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0061] The obtained emulsion 3 was placed in a water bath at 70°C and heated to continue the reaction for 20 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 90 minutes.
[0062] The obtained product was centrifuged at 12000 r / min (25 min, 5 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0063] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3Pa vacuum environment, heat from room temperature to 330℃ at a rate of 25℃ / min and keep warm for 1.5h; then heat to 750℃ at a rate of 15℃ / min, pressurize to 30MPa and keep warm for 7h.
[0064] The XRD curve of the yttrium-doped barium magnesium fluoride powder obtained in this example is shown in Figure 1 (b), by comparing with the standard PDF card of magnesium barium fluoride, it can be found that the main diffraction peaks can correspond one to one, which indicates that magnesium barium fluoride powder particles with higher purity are synthesized by the improved water bath method. The XRD pattern of the yttrium-doped magnesium barium fluoride transparent ceramic obtained in this example is as follows: Figure 3 As shown in the figure, compared with the standard card of magnesium barium fluoride, the main diffraction peaks can correspond one to one, indicating that the phase composition of magnesium barium fluoride ceramics has not changed after sintering. Specific process parameters and sample properties are shown in Table 1.
[0065] Example 3 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0066] Dissolve 0.1 mol of barium chloride (BaCl2·2H2O), 0.15 mol of magnesium chloride (MgCl2·6H2O) and 0.012 mol of yttrium nitrate (Y(NO3)3·6H2O) in 200 mL of water to prepare solution 1, and dissolve 0.9 mol of potassium fluoride (KF·2H2O) in 600 mL of water to prepare solution 2;
[0067] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0068] The obtained emulsion 3 was placed in a water bath at 80°C and heated to continue the reaction for 10 min. After the reaction was completed, the emulsion was taken out and allowed to stand for 120 min.
[0069] The obtained product was centrifuged at 12000 r / min (20 min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0070] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, the temperature was raised from room temperature to 350°C at a rate of 30°C / min and kept warm for 2h; then it was raised to 850°C at a rate of 20°C / min, pressurized to 30MPa and kept warm for 8h.
[0071] The XRD curve of the yttrium-doped barium magnesium fluoride powder obtained in this example is shown in Figure 1(c), by comparing with the standard PDF card of magnesium barium fluoride, it can be found that the main diffraction peaks can correspond one to one, which indicates that magnesium barium fluoride powder particles with higher purity are synthesized by the improved water bath method. The XRD pattern of the yttrium-doped magnesium barium fluoride transparent ceramic obtained in this example is as follows: Figure 3 As shown in the figure, compared with the standard card of magnesium barium fluoride, the main diffraction peaks can correspond one to one, indicating that the phase composition of magnesium barium fluoride ceramics has not changed after sintering. Specific process parameters and sample properties are shown in Table 1.
[0072] Example 4 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0073] Dissolve 0.1 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O) and 0.005 mol of yttrium nitrate (Y(NO3)3·6H2O) in 200 mL of water to prepare solution 1, and dissolve 0.75 mol of potassium fluoride (KF·2H2O) in 750 mL of water to prepare solution 2;
[0074] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0075] The obtained emulsion 3 was placed in a 60°C water bath and heated to continue the reaction for 10 min. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 min.
[0076] The obtained product was centrifuged at 12000 r / min (20 min, 4 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0077] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, heat from room temperature to 300℃ at a rate of 30℃ / min and keep warm for 1h; then heat to 650℃ at a rate of 10℃ / min, pressurize to 30MPa and keep warm for 5h.
[0078] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0079] Example 5 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0080] Solution 1 was prepared by dissolving 0.15 mol of barium chloride (BaCl2·2H2O), 0.15 mol of magnesium chloride (MgCl2·6H2O) and 0.012 mol of yttrium nitrate (Y(NO3)3·6H2O) in 100 mL of water, and solution 2 was prepared by dissolving 0.9 mol of potassium fluoride (KF·2H2O) in 600 mL of water.
[0081] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 60 minutes.
[0082] The obtained emulsion 3 was placed in a water bath at 80°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 120 minutes.
[0083] The obtained product was centrifuged at 12000r / min (40min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar;
[0084] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -4 Pa, the temperature was raised from room temperature to 350°C at a rate of 20°C / min and kept warm for 2h; then it was raised to 850°C at a rate of 20°C / min, pressurized to 30MPa and kept warm for 8h.
[0085] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0086] Example 6 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0087] Solution 1 was prepared by dissolving 0.11 mol of barium chloride (BaCl2·2H2O), 0.12 mol of magnesium chloride (MgCl2·6H2O) and 0.006 mol of yttrium nitrate (Y(NO3)3·6H2O) in 200 mL of water, and solution 2 was prepared by dissolving 0.8 mol of potassium fluoride (KF·2H2O) in 700 mL of water.
[0088] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 35 minutes.
[0089] The obtained emulsion 3 was placed in a water bath at 80°C and heated to continue the reaction for 15 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 120 minutes.
[0090] The obtained product was centrifuged at 12000 r / min (25 min, 5 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0091] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 4×10 -3 Pa vacuum environment, heat from room temperature to 345℃ at a rate of 35℃ / min and keep warm for 2h; then heat to 840℃ at a rate of 20℃ / min, pressurize to 30MPa and keep warm for 7h.
[0092] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0093] Example 7 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0094] Solution 1 was prepared by dissolving 0.13 mol of barium chloride (BaCl2·2H2O), 0.14 mol of magnesium chloride (MgCl2·6H2O) and 0.09 mol of yttrium nitrate (Y(NO3)3·6H2O) in 100 mL of water, and solution 2 was prepared by dissolving 0.85 mol of potassium fluoride (KF·2H2O) in 800 mL of water.
[0095] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 45 minutes.
[0096] The obtained emulsion 3 was placed in a water bath at 75°C and heated to continue the reaction for 15 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 100 minutes.
[0097] The obtained product was centrifuged at 12000r / min (30min, 7 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar;
[0098] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, heat from room temperature to 335℃ at a rate of 35℃ / min and keep warm for 1.5h; then heat to 810℃ at a rate of 10℃ / min, pressurize to 30MPa and keep warm for 7h.
[0099] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0100] Example 8 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0101] Solution 1 was prepared by dissolving 0.14 mol of barium chloride (BaCl2·2H2O), 0.11 mol of magnesium chloride (MgCl2·6H2O) and 0.008 mol of yttrium nitrate (Y(NO3)3·6H2O) in 200 mL of water, and solution 2 was prepared by dissolving 0.8 mol of potassium fluoride (KF·2H2O) in 600 mL of water.
[0102] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain an emulsion 3, and stirring was continued for 40 minutes.
[0103] The obtained emulsion 3 was placed in a water bath at 75°C and heated to continue the reaction for 20 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 90 minutes.
[0104] The obtained product was centrifuged at 12000 r / min (35 min, 5 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0105] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 4×10 -3 Pa vacuum environment, heat the temperature from room temperature to 330℃ at a rate of 25℃ / min and keep it warm for 2h; then heat it to 830℃ at a rate of 10℃ / min, pressurize to 30MPa and keep it warm for 8h.
[0106] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0107] Example 9 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0108] Solution 1 was prepared by dissolving 0.13 mol of barium chloride (BaCl2·2H2O), 0.13 mol of magnesium chloride (MgCl2·6H2O) and 0.012 mol of yttrium nitrate (Y(NO3)3·6H2O) in 100 mL of water, and solution 2 was prepared by dissolving 0.8 mol of potassium fluoride (KF·2H2O) in 650 mL of water.
[0109] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 45 minutes.
[0110] The obtained emulsion 3 was placed in a 70°C water bath and heated to continue the reaction for 15 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 80 minutes.
[0111] The obtained product was centrifuged at 12000 r / min (25 min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0112] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 1.5×10 - 3 Pa vacuum environment, heat from room temperature to 335℃ at a rate of 40℃ / min and keep warm for 2h; then heat to 815℃ at a rate of 20℃ / min, pressurize to 30MPa and keep warm for 6.5h.
[0113] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0114] Example 10 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0115] Solution 1 was prepared by dissolving 0.14 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O) and 0.012 mol of yttrium nitrate (Y(NO3)3·6H2O) in 150 mL of water, and solution 2 was prepared by dissolving 0.85 mol of potassium fluoride (KF·2H2O) in 650 mL of water.
[0116] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain an emulsion 3, and stirring was continued for 40 minutes.
[0117] The obtained emulsion 3 was placed in a water bath at 65°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 115 minutes.
[0118] The obtained product was centrifuged at 12000 r / min (30 min, 5 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0119] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 2.5×10 - 3 Pa vacuum environment, heat from room temperature to 325℃ at a rate of 20℃ / min and keep warm for 1h; then heat to 805℃ at a rate of 20℃ / min, pressurize to 30MPa and keep warm for 5.5h.
[0120] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0121] Embodiment 11 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0122] Solution 1 was prepared by dissolving 0.11 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O) and 0.007 mol of yttrium nitrate (Y(NO3)3·6H2O) in 150 mL of water, and solution 2 was prepared by dissolving 0.75 mol of potassium fluoride (KF·2H2O) in 550 mL of water.
[0123] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain an emulsion 3, and stirring was continued for 50 minutes.
[0124] The obtained emulsion 3 was placed in a water bath at 75°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 70 minutes.
[0125] The obtained product was centrifuged at 12000 r / min (25 min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0126] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 3.5×10 - 3 Pa vacuum environment, heat from room temperature to 305℃ at a rate of 30℃ / min and keep warm for 2h; then heat to 750℃ at a rate of 10℃ / min, pressurize to 30MPa and keep warm for 5.5h.
[0127] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0128] Example 12 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0129] Solution 1 was prepared by dissolving 0.1 mol of barium chloride (BaCl2·2H2O), 0.12 mol of magnesium chloride (MgCl2·6H2O) and 0.006 mol of yttrium nitrate (Y(NO3)3·6H2O) in 100 mL of water, and solution 2 was prepared by dissolving 0.8 mol of potassium fluoride (KF·2H2O) in 700 mL of water.
[0130] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 55 minutes.
[0131] The obtained emulsion 3 was placed in a water bath at 60°C and heated to continue the reaction for 25 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0132] The obtained product was centrifuged at 12000 r / min (35 min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0133] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 3.5×10 - 3 Pa vacuum environment, heat from room temperature to 315℃ at a rate of 30℃ / min and keep warm for 2h; then heat to 780℃ at a rate of 10℃ / min, pressurize to 30MPa and keep warm for 7h.
[0134] The XRD curves of the yttrium-doped barium magnesium fluoride powder obtained in this example before and after sintering are basically consistent with those of the product in Example 1. Specific process parameters and sample properties are shown in Table 1.
[0135] Comparative Example 1 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0136] Dissolve 0.16 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O) and 0.005 mol of yttrium nitrate (Y(NO3)3·6H2O) in 200 mL of water to prepare solution 1, and dissolve 0.75 mol of potassium fluoride (KF·2H2O) in 1500 mL of water to prepare solution 2;
[0137] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 52 minutes;
[0138] The obtained emulsion 3 was placed in a 90°C water bath and heated for 26 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0139] The obtained product was centrifuged at 12000r / min (30min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar;
[0140] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 3.0 × 10 - 3 Pa vacuum environment, the temperature was raised from room temperature to 310°C at a rate of 30°C / min and kept at that temperature for 2 hours; then the temperature was raised to 750°C at a rate of 10°C / min and kept at that temperature for 7 hours while applying a pressure of 30MPa. The specific process parameters and sample properties are shown in Table 2.
[0141] Comparative Example 2 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0142] Solution 1 was prepared by dissolving 0.12 mol of barium chloride (BaCl2·2H2O), 0.14 mol of magnesium chloride (MgCl2·6H2O) and 0.008 mol of yttrium nitrate (Y(NO3)3·6H2O) in 150 mL of water, and solution 2 was prepared by dissolving 0.78 mol of potassium fluoride (KF·2H2O) in 600 mL of water.
[0143] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain an emulsion 3, and stirring was continued for 50 minutes.
[0144] The obtained emulsion 3 was placed at room temperature of 25°C to continue reacting for 26 minutes. After the reaction was completed, it was taken out and allowed to stand for 60 minutes.
[0145] The obtained product was centrifuged at 12000 r / min (35 min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0146] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 1.5×10 - 2Pa vacuum environment, the temperature was raised from room temperature to 310°C at a rate of 30°C / min and kept at that temperature for 2h; then the temperature was raised to 870°C at a rate of 10°C / min and kept at that temperature for 3h under a pressure of 30MPa. The specific process parameters and sample properties are shown in Table 2.
[0147] Comparative Example 3 Preparation of Yttrium-doped Barium Magnesium Fluoride Transparent Ceramics
[0148] Solution 1 was prepared by dissolving 0.1 mol of barium chloride (BaCl2·2H2O), 0.15 mol of magnesium chloride (MgCl2·6H2O) and 0.012 mol of yttrium nitrate (Y(NO3)3·6H2O) in 50 mL of water, and solution 2 was prepared by dissolving 0.9 mol of potassium fluoride (KF·2H2O) in 1800 mL of water.
[0149] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 53 minutes.
[0150] The obtained emulsion 3 was placed in a water bath at 55°C and heated to continue the reaction for 25 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0151] The obtained product was centrifuged at 12000 r / min (30 min, 6 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0152] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering at 1.0×10 - 3 Pa vacuum environment, the temperature was raised from room temperature to 310°C at a rate of 30°C / min and kept at that temperature for 2h; then the temperature was raised to 890°C at a rate of 10°C / min and kept at that temperature for 10h under a pressure of 30MPa. The specific process parameters and sample properties are shown in Table 2.
[0153] Comparative Example 4 Preparation of Transparent Magnesium Barium Fluoride Ceramics
[0154] Solution 1 was prepared by dissolving 0.15 mol of barium chloride (BaCl2·2H2O) and 0.1 mol of magnesium chloride (MgCl2·6H2O) in 200 mL of water, and solution 2 was prepared by dissolving 0.75 mol of potassium fluoride (KF·2H2O) in 750 mL of water.
[0155] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0156] The obtained emulsion 3 was placed in a water bath at 60°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0157] The obtained product was centrifuged at 12000 r / min (30 min, 4 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0158] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, the temperature was raised from room temperature to 300°C at a rate of 30°C / min and kept at that temperature for 1 hour; then the temperature was raised to 650°C at a rate of 10°C / min and kept at that temperature for 5 hours while applying a pressure of 30 MPa. The specific process parameters and sample properties are shown in Table 2.
[0159] Comparative Example 5 Preparation of Ytterbium-doped Barium Magnesium Fluoride Transparent Ceramics
[0160] Solution 1 was prepared by dissolving 0.15 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O) and 0.005 mol of ytterbium nitrate (Yb(NO3)3·6H2O) in 200 mL of water, and solution 2 was prepared by dissolving 0.75 mol of potassium fluoride (KF·2H2O) in 750 mL of water.
[0161] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0162] The obtained emulsion 3 was placed in a water bath at 60°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0163] The obtained product was centrifuged at 12000 r / min (30 min, 4 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar.
[0164] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, the temperature was raised from room temperature to 300°C at a rate of 30°C / min and kept at that temperature for 1 hour; then the temperature was raised to 650°C at a rate of 10°C / min and kept at that temperature for 5 hours while applying a pressure of 30 MPa. The specific process parameters and sample properties are shown in Table 2.
[0165] Comparative Example 6 Preparation of Ytterbium-Erbium Doped Barium Magnesium Fluoride Transparent Ceramics
[0166] Dissolve 0.15 mol of barium chloride (BaCl2·2H2O), 0.1 mol of magnesium chloride (MgCl2·6H2O), 0.003 mol of ytterbium nitrate (Yb(NO3)3·6H2O) and 0.002 mol of erbium nitrate (Er(NO3)3·6H2O) in 200 mL of water to prepare solution 1, and dissolve 0.75 mol of potassium fluoride (KF·2H2O) in 750 mL of water to prepare solution 2.
[0167] The obtained solution 2 was poured into the solution 1 under magnetic stirring to obtain the emulsion 3, and the stirring was continued for 30 minutes.
[0168] The obtained emulsion 3 was placed in a water bath at 60°C and heated to continue the reaction for 30 minutes. After the reaction was completed, the emulsion was taken out and allowed to stand for 60 minutes.
[0169] The obtained product was centrifuged at 12000r / min (30min, 4 times), the obtained product was washed with deionized water and dried in an oven, and the dried powder was ground with an agate mortar;
[0170] About 3.0 g of the ground powder product was mixed evenly and placed in a graphite mold. Both sides were pressed with graphite presses. The powder and the mold were separated by cut graphite paper. The mold with pressed powder was placed in a hot press furnace for sintering. -3 Pa vacuum environment, the temperature was raised from room temperature to 300°C at a rate of 30°C / min and kept at that temperature for 1 hour; then the temperature was raised to 650°C at a rate of 10°C / min and kept at that temperature for 5 hours while applying a pressure of 30 MPa. The specific process parameters and sample properties are shown in Table 2.
[0171] Table 1 Specific process parameters and sample properties of magnesium barium fluoride transparent ceramic samples sintered in Examples 1-12 of the present invention
[0172]
[0173]
[0174] Table 2 Specific process parameters and sample properties of magnesium barium fluoride transparent ceramic samples sintered in comparative examples 1-6 of the present invention
[0175]
[0176] Embodiment 1-12 successfully prepared high-purity nano-scale magnesium barium fluoride powder by controlling the ratio of raw materials and their components, the concentration of anion and cation solutions, and the reaction temperature. By controlling the process parameters of powder sintering (including vacuum degree, sintering pressure, sintering time, etc.), magnesium barium fluoride transparent ceramics with high optical transmittance and purity were obtained. As can be seen from Table 1, the grain size of magnesium barium fluoride transparent ceramics prepared by the corresponding raw materials and processes in Embodiments 1-12 of the present invention is ≤3μm, and in terms of optical transmittance, within the range of 400-800nm, the maximum transmittance is ≥50.5%, and the minimum transmittance is ≥48.3%. It can be seen that the magnesium barium fluoride transparent ceramics prepared by Embodiments 1-12 of the present invention have good optical transmittance. The magnesium barium fluoride transparent ceramics prepared by Comparative Examples 1-6 have low transmittance, with a maximum transmittance of only 42.6%, poor light transmittance of the sample, and the powder particle size and crystal size are also significantly higher than those of Embodiments 1-12.
[0177] The numerical range described in the present invention includes all the values within this range, and includes the range value composed of any two values within this range. For example, "the concentration range of barium ions or magnesium ions in solution 1 is 0.5-1.5 mol / L", this numerical range includes all the values between 0.5-1.5, and includes the range value (0.4-1.4) composed of any two values within this range (for example: 0.4, 1.4); different values of the same indicator appearing in all embodiments of the present invention can be arbitrarily combined to form a range value.
[0178] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be combined arbitrarily, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0179] In the specification of the present invention, a lot of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some embodiments, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this specification.
[0180] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. Although the present application is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A transparent ceramic material, which is obtained by sintering magnesium barium fluoride as a matrix and yttrium as a doping element, and its raw materials are composed of barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride, wherein: The molar ratio of barium ion, magnesium ion, yttrium ion and fluoride ion is (100-150): (100-150): (5-12): (750-900); The grain size of the transparent ceramic material is less than 3 μm; The transparent ceramic material has a maximum transmittance of ≥50.5% and a minimum transmittance of ≥48.3% in the visible light band of 400-800nm; The sintering process is: at a temperature not higher than 5×10 -3 In a vacuum environment of 0.04 Pa, heat the temperature from room temperature to 300-350°C at a rate of 20-40°C / min, keep warm for 1-2h, then heat the temperature to 650-850°C at a rate of 10-20°C / min, keep warm for 5-8h.
2. A method for preparing the transparent ceramic material according to claim 1, comprising: Take barium salt, magnesium salt and yttrium salt to prepare aqueous solution 1, take fluoride salt to prepare aqueous solution 2; pour aqueous solution 2 into aqueous solution 1 under stirring to react to obtain emulsion 3, and continue stirring; place emulsion 3 in a water bath for heating, let it stand after heating, centrifuge, wash and dry the emulsion 3 after standing, grind it after drying to obtain yttrium-doped magnesium barium fluoride powder; sinter the powder to obtain a transparent ceramic material; the barium salt, magnesium salt, yttrium salt and fluoride salt are barium chloride, magnesium chloride, yttrium nitrate and potassium fluoride respectively.
3. The method according to claim 2, characterized in that The concentration range of barium ions or magnesium ions in aqueous solution 1 is 0.5-1.5 mol / L, and the concentration range of fluoride ions in aqueous solution 2 is 1-1.5 mol / L.
4. The method according to claim 2, characterized in that: The water bath temperature is 60-80°C.
5. The method according to claim 2, characterized in that: The sintering is carried out by vacuum hot pressing, and the vacuum degree during sintering is not higher than 5×10 -3 Pa, sintering temperature is 650-850℃.
6. An optical element or optical device, comprising the transparent ceramic material according to claim 1, or prepared from the transparent ceramic material according to claim 1.
7. Use of the transparent ceramic material according to claim 1 in the field of optics.
8. The use according to claim 7, characterized in that: The transparent ceramic material can be used as a two-dimensional nonlinear photonic crystal in the optical field.
Citation Information
Patent Citations
Preparation method of erbium ion-doped calcium fluoride laser transparent ceramic material
CN102126858A