Method for producing cellulose carbamate
By performing a reduced pressure heating reaction of cellulose and urea in the aqueous phase and removing water-soluble nitrogen-containing compounds by washing water, the problem of by-product generation in cellulose carbamate production is solved, achieving high quality and efficient Cellulose carbamate production.
Patent Information
- Application Number
- CN202280014664.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The production of by-products such as biuret and ammonium carbamate in the existing cellulose carbamate production process affects yield and purity, and the removal process consumes high energy and is economically unreasonable.
The cellulose and urea are mixed in the aqueous phase, subjected to a reduced pressure heating reaction, the temperature is controlled from 130 to 150°C, and the water-soluble nitrogen-containing compound is removed by washing with water, limiting its content in the cellulose carbamate to 12 % or less to reduce the formation of adverse by-products.
High yield production of high-quality cellulose carbamate is achieved, significantly reducing the formation of biuret and ammonium carbamate, improving the economic and efficiency of the process, and allowing more urea recycling.
Smart Images

Figure CN116888158B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing cellulose carbamate. Background Art
[0002] Cellulose is the most widely used biopolymer in the world and has applications in various industries such as paper, board industry and textile industry as both cellulose and cellulose derivatives such as cellulose carbamate, cellulose acetate, ethers and esters. The dissolution of cellulose is difficult due to its semi-crystalline structure, strong hydrogen bonds in the polymer sheets and the presence of hydrophilic and hydrophobic ends in the polymer. For this reason, cellulose needs to be modified in structure by derivatization, or to open the fibers and increase reactivity.
[0003] Several derivatization processes are known in the art, the best known being probably the viscose process, in which cellulose is first treated with alkali and then with carbon disulfide to produce cellulose xanthate. The viscose process is increasingly being discouraged due to the toxicity of carbon disulfide and the adverse environmental impact of the viscose process. Increasingly, a move is being made to other derivatization processes, particularly those that are less expensive, do not suffer from the toxicity and environmental issues of the viscose process, and can still be performed using available infrastructure, such as processes that can be performed in viscose wet spinning plants.
[0004] The carbamate process for producing cellulose carbamate is one such derivatization process. Cellulose carbamate is formed by reacting cellulose with urea. Methods for producing cellulose carbamate are described in, for example, Finnish Patent Nos. 112869 and 112795 and in international patent applications. In one such example, urea is impregnated into cellulose and the reaction between cellulose and urea is carried out in a mixture of cellulose, liquid, urea and optionally hydrogen peroxide.
[0005] During the carbamation process, harmful by-products such as biuret and ammonium carbamate are produced, which have a negative impact on the yield and purity of cellulose carbamate. The by-products cause the degree of polymerization (DP) of cellulose carbamate to decrease uncontrollably during the carbamation process, lack of ideal solubility in alkaline aqueous solution when preparing cellulose carbamate spinning dope, and thus negatively affect the usefulness of the produced cellulose carbamate.
[0006] Removal of nitrogenous by-products and unreacted urea is described in Finnish Patent No. 128164. The waste stream containing nitrogenous by-products and unreacted urea can be directed to an evaporation plant to produce dry fertilizer. However, evaporation is an energy-intensive process and, in addition to the loss of urea in the carbamate reaction, adds an economic problem that needs to be solved. Producing dry fertilizer does not solve the problem of one such nitrogenous by-product, namely biuret, which can be toxic to plants depending on, for example, soil conditions. Summary of the invention
[0007] It is an object of the present invention to overcome at least some of the above problems and to provide a method for producing cellulose carbamate. The method comprises mixing cellulose and urea and reacting the resulting mixture to form cellulose carbamate.
[0008] The invention is defined by the features of the independent claims. Specific embodiments are defined in the dependent claims.
[0009] According to a first aspect of the present invention, there is provided a method for producing cellulose carbamate in an aqueous phase, comprising: providing a cellulose feedstock, providing urea, mixing cellulose and urea to provide a mixture, subjecting the mixture to a reduced pressure of not more than 350 mbar(a), heating the mixture to a temperature of 130 to 150°C, reacting the cellulose with urea to form cellulose carbamate, releasing the pressure, recovering the cellulose carbamate and washing the cellulose carbamate with water to remove water-soluble nitrogen-containing compounds, wherein the water-soluble nitrogen-containing compounds account for up to 12% by weight, preferably 6% or less, of the total weight of the cellulose carbamate and the water-soluble nitrogen-containing compounds.
[0010] Considerable advantages are obtained by the present invention. The present invention provides a method for producing cellulose carbamate. By the present invention, it has surprisingly been found that high quality cellulose carbamate suitable for spinning solution can be produced in high yield in an economical and reliable method under reduced pressure. It has also surprisingly been found that the formation of undesirable nitrogen-containing by-products such as biuret and ammonium carbamate is minimized by the present invention. Since the formation of undesirable by-products is minimized, more urea can be recycled into the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 is a graph of the amount of urea percentage versus temperature according to at least some embodiments of the present invention and illustrates the amount of urea present in the unreacted wash fraction of a carbamation process at a reduced pressure of 250 mbar (a) in a temperature range of 130 to 150°C.
[0012] Figure 2is a graph of percent biuret versus temperature according to at least some embodiments of the present invention and illustrates the amount of biuret present in an unreacted wash fraction in a carbamation process at a reduced pressure of 250 mbar (a) in a temperature range of 130 to 150°C.
[0013] Figure 3 is a graph of the percentage of the amount of nitrogen-containing compounds other than urea and biuret (such as ammonium carbamate) versus temperature according to at least some embodiments of the present invention, and shows the total amount of nitrogen-containing compounds other than urea and biuret (such as ammonium carbamate) present in the unreacted wash fraction in the carbamation process at a reduced pressure of 250 mbar (a) in the temperature range of 130 to 150°C.
[0014] Figure 4 is a graph of the amount of urea percentage versus pressure according to at least some embodiments of the present invention and illustrates the amount of urea present in the unreacted wash fraction of a carbamation process at a reduced pressure of 500-50 mbar (a).
[0015] Figure 5 is a graph of percent biuret versus pressure according to at least some embodiments of the present invention and illustrates the amount of biuret present in the unreacted wash fraction in a carbamation process at a reduced pressure of 500-50 mbar (a).
[0016] Figure 6 is a graph of the percentage of the amount of nitrogen-containing compounds other than urea and biuret (such as ammonium carbamate) versus pressure according to at least some embodiments of the present invention, and shows the total amount of nitrogen-containing compounds other than urea and biuret (such as ammonium carbamate) present in the unreacted wash fraction in the carbamation process under a reduced pressure of 500-50 mbar (a).
[0017] Figure 7 is the filterability index (K R ) versus carbamation temperature and illustrates the mass of the stock solution prepared by carbamation at normal atmospheric pressure of 1013 mbar(a) and at reduced pressure of 250 mbar(a). DETAILED DESCRIPTION
[0018] definition
[0019] "High consistency pulp" refers to a pulp having a cellulosic solids content greater than 5 wt%, liquid (usually greater than 20 wt%) and liquid.
[0020] "Ultra-high consistency pulp" refers to a pulp having a cellulosic solids content greater than 20 wt% and a liquid that does not release free water.
[0021] For purposes of embodiments of the present invention, cellulose refers to a cellulosic material suitable for carbamate formation, including a cellulose source selected from chemical pulp or dissolving pulp, which is prepared from wood species such as pine, spruce, birch, beech, poplar, maple, larch, acacia, eucalyptus, hemlock, blueberry and oak, or non-wood such as straw fibers (wheat straw, rice straw, barley straw, bamboo, bagasse and reed) and mixtures thereof. The source of the raw materials can be chemical pulp and / or dissolving pulp in virgin form and / or recycled raw materials such as chemical pulp or dissolving pulp containing recycled paper and / or paperboard. In addition, cellulose includes cellulosic natural plant fibers and mixtures thereof, which provide a source of cellulose by themselves or in the form of chemical pulp and / or dissolving pulp or dissolving pulp (such as waste cotton pulp). The source of natural plant fibers can be their virgin form and / or textiles containing natural fibers and / or textiles containing recycled natural plant fibers. Natural plant fibers include seed fibers such as cotton and kapok; bast fibers such as hemp, jute, kenaf, ramie, abaca and flax (flax fiber); leaf fibers such as manilla, sisal, pineapple and banana; fruit fibers such as coconut shell, and mixtures thereof.
[0022] The present invention relates to a method for producing cellulose carbamate. By embodiments, it has surprisingly been found that the amount of undesirable nitrogen-containing byproducts in a stream containing unreacted urea is minimized, thereby alleviating or reducing the need to remove the unreacted urea before it is recovered or directed to further processing. Regardless of the synthetic method selected, the carbamation reaction will produce some nitrogen-containing byproducts. Therefore, byproducts or other impurities accumulate in the process.
[0023] Figure 1 is a graph illustrating the amount of urea present in the unreacted wash liquid (wash) calculated as a percentage in a carbamation process carried out at 250 mbar (a). The process was carried out at 130° C., 140° C. and 150° C. As can be seen from the graph, the proportion of urea present in the unreacted wash liquid (expressed as a percentage of the total weight of the unreacted wash liquid) decreases with increasing temperature applied in the carbamation process. As the fraction of urea in the unreacted wash liquid decreases, there is a concomitant increase in the amount of undesirable by-products such as biuret and other nitrogen-containing by-products such as ammonium carbamate in the unreacted wash liquid.
[0024] Figure 2Graph showing the amount of biuret present in the unreacted washing liquid in a carbamation process carried out at 250 mbar (a) in percentage. The process was carried out at 130° C., 140° C. and 150° C. It can be seen from the graph that the proportion of biuret present in the unreacted washing liquid (expressed as a percentage of the total weight of unreacted washing) increases with increasing temperature in the carbamation process, i.e. more undesirable biuret is produced when the carbamation is carried out at a higher temperature.
[0025] Figure 3 is a graph showing the total amount of nitrogen-containing compounds other than urea and biuret (e.g. by-products such as ammonium carbamate) present in the unreacted wash in a carbamation process carried out at 250 mbar (a) in terms of percentage. The process was carried out at 130° C., 140° C. and 150° C. It can be seen from the graph that the proportion of other nitrogen-containing by-products such as ammonium carbamate present in the unreacted wash (expressed as a percentage of the total weight of the unreacted wash) increases with increasing temperature in the carbamation process, i.e., more undesirable nitrogen-containing by-products such as ammonium carbamate are produced when the carbamation is carried out at a higher temperature.
[0026] Figure 4 is a graph illustrating the amount of urea present in the unreacted scrubbing liquid in a carbamation process as a percentage relative to pressure. As can be seen from the graph, the proportion of urea present in the unreacted scrubbing liquid, expressed as a percentage of the total weight of the unreacted scrubbing, increases as the pressure in the carbamation process decreases. As the fraction of urea in the unreacted scrubbing liquid increases, there is a concomitant decrease in the amount of undesirable byproducts such as biuret and other nitrogen-containing byproducts such as ammonium carbamate in the unreacted scrubbing liquid.
[0027] Figure 5 is a graph showing the amount of biuret present in the unreacted washing liquid in the carbamation process as a percentage versus pressure. It can be seen from the graph that the proportion of biuret present in the unreacted washing liquid, expressed as a percentage of the total weight of unreacted washings, decreases as the pressure in the carbamation process decreases, i.e., less undesirable biuret is produced when the carbamation is carried out at a lower pressure.
[0028] Figure 6is a graph showing the total amount of nitrogen-containing compounds other than urea and biuret (byproducts such as ammonium carbamate) present in the unreacted scrubbing liquid in the carbamation process in percentage terms relative to pressure. It can be seen from the graph that the proportion of other nitrogen-containing byproducts such as ammonium carbamate present in the unreacted scrubbing liquid, expressed as a percentage of the total weight of the unreacted scrubbing liquid, decreases as the pressure in the carbamation process decreases, i.e., when the carbamation is carried out at a lower pressure, less undesirable nitrogen-containing compounds such as ammonium carbamate are produced.
[0029] Figure 7 is a graph showing the filterability of cellulose carbamate stock solutions prepared at a temperature range of 130 to 150° C., at a normal atmospheric pressure of 1013 mbar(a) and at a reduced pressure of 250 mbar(a). K corresponding to the viscosity correction w Value K R The index indicates the filterability of the cellulose carbamate solution. The lower the value, the lower the amount of non-reactive particles with a size of >10 μm that clog the filter found in the recovered cellulose carbamate solution. It can be seen that the filterability of the stock solution prepared by carbamation under a reduced pressure of 250 mbar (a) remains stable at all temperatures in this range, while the quality of the stock solution prepared by carbamation under normal atmospheric pressure deteriorates significantly when prepared at a temperature exceeding 140°C.
[0030] As described above, the present technology relates to a method for producing cellulose carbamate. In one embodiment, the method for producing cellulose carbamate includes the following steps: a) providing a cellulose raw material; b) providing urea; c) mixing cellulose and urea to provide a mixture; d) subjecting the mixture to a reduced pressure of no more than 350 mbar (a); e) heating the mixture to a temperature of 130 to 150° C. to react cellulose with urea to form cellulose carbamate; f) releasing the pressure; and g) recovering cellulose carbamate, and h) washing the cellulose carbamate with water to remove water-soluble nitrogen-containing compounds, wherein the water-soluble nitrogen-containing compounds account for up to 12% by weight of the total weight of cellulose carbamate and the water-soluble nitrogen-containing compounds, preferably 6% or less.
[0031] Cellulose carbamate is usually produced in an aqueous phase, usually by processing ultra-high consistency cellulose pulp or cellulose medium. No organic solvent is used as a reaction medium in the reaction of cellulose with urea. Therefore, in one embodiment, urea is provided in the form of an aqueous solution. Urea is added and contact between urea and cellulose is carried out in the absence of liquid ammonia.
[0032] The range of cellulosic materials suitable for carbamate treatment is diverse according to the embodiment and in one embodiment includes a cellulose source selected from chemical pulp or dissolving pulp made from wood species such as pine, spruce, birch, beech, poplar, maple, larch, acacia, eucalyptus, hemlock, blueberry and oak, or non-wood such as straw fibers (wheat straw, rice straw, barley straw, bamboo, bagasse and reed) and mixtures thereof. The source of the raw material can be chemical pulp and / or dissolving pulp in virgin form and / or recycled raw materials such as chemical pulp or dissolving pulp containing recycled paper and / or paperboard.
[0033] In another embodiment, natural plant fibers and mixtures thereof provide a source of cellulose, either by themselves or in the form of chemical pulp and / or dissolving pulp. The source of natural plant fibers may be in their native form and / or textiles containing natural fibers and / or textiles containing recycled natural plant fibers. Natural plant fibers include seed fibers such as cotton and kapok; bast fibers such as hemp, jute, kenaf, ramie, ramie and flax (flax); leaf fibers such as abaca, sisal, pineapple and banana; fruit fibers such as coconut shells, and mixtures thereof.
[0034] It has been found that subjecting the mixture to a reduced pressure of not more than 350 mbar (a) produces a high quality cellulose carbamate product which can be recovered from a stream comprising unreacted urea and only small amounts of undesirable nitrogen-containing by-products such as biuret and other nitrogen-containing by-products such as ammonium carbamate. Preferably, the unreacted urea is recycled to step b) of the process where it is mixed with fresh urea, optionally before step c), thereby increasing the efficiency of the process in terms of urea usage.
[0035] In another embodiment, the mixture is heated at 130° C. to 140° C., particularly 135±3° C. for 60 to 240 minutes, preferably 120 to 180 minutes, suitably 150 minutes. The preferred range for heating the mixture is in the range of 130° C. to 135° C., which is optimal for balancing reaction efficiency with the use of raw materials and energy.
[0036] In one embodiment, the mixture of cellulose and urea is optionally flushed with an inert gas during heating under reduced pressure to form cellulose carbamate. Preferably, the inert gas is nitrogen. Flushing with an inert gas further reduces the amount of oxygen present in the reaction vessel or reaction zone, thereby reducing the possibility of explosion in the reactor or the plant where the reactor is located.
[0037] In another embodiment, the pressure is released after the reaction of cellulose with urea is complete to form cellulose carbamate. Preferably, this allows the cellulose carbamate to be most easily recovered from the reactor. The end of the reaction between cellulose and urea to form cellulose carbamate is preferably confirmed by monitoring the amount of ammonia formed or released. Alternatively or additionally, this can be achieved by measuring the reduction in the total nitrogen content in a sample extracted directly from the carbamate reactor. The total nitrogen content is reduced while ammonia is formed or released. In particular, the completeness of the reaction can be monitored and determined by measuring the amount of nitrogen bound to the cellulose. The reduction in the total nitrogen content in a sample taken directly from the reactor or the reduction in the amount of nitrogen bound to the cellulose in a sample washed without water-soluble nitrogen-containing compounds can be easily determined, for example, by NIR spectroscopy.
[0038] Although the amount of biuret produced by the process of the present invention is significantly reduced by means of the embodiment, and the amount of other nitrogen-containing byproducts such as ammonium carbamate produced is significantly reduced, in one embodiment, the cellulose carbamate obtained by reacting cellulose and urea is preferably washed with water to remove water-soluble nitrogen-containing compounds and non-urea compounds and optionally other water-soluble compounds from the cellulose carbamate. In one embodiment, the water-soluble nitrogen-containing compounds removed by washing are, for example, urea, biuret, ammonium carbamate, and degradation products of cellulose polymers reacted in the carbamate reaction in the presence of urea. In a further embodiment, other water-soluble compounds include organic matter, such as degradation products of cellulose polymers, and inorganic matter, such as monovalent, divalent and multivalent cations and anions, such as chlorides, sulfates and carbonates. In a preferred embodiment, water-soluble non-gaseous nitrogen-containing compounds and non-urea compounds, and optionally other water-soluble compounds, preferably water-soluble organic matter and water-soluble inorganic matter are recovered separately from the cellulose carbamate and recovered in the form of an aqueous solution. In a particular embodiment, non-urea compounds, preferably a majority of non-urea compounds, are separated from the aqueous solution, preferably allowing urea in the aqueous solution to be recycled to step b) of this embodiment of the process. In another embodiment, the recovered aqueous solution is optionally concentrated by evaporation.
[0039] Various methods of separating non-urea compounds from aqueous solutions are suitable for use in embodiments of the present technology. In preferred embodiments, separation of non-urea compounds is performed by a selective separation method selected from ion exchange, membrane filtration, electrodialysis, and crystallization. In further embodiments, crystallization is performed by centrifugation or filtration. Membrane filtration includes, for example, nanofiltration and reverse osmosis.
[0040] As mentioned above, it is preferred that the amount of biuret produced is reduced by the embodiments. Similarly, it is preferred to reduce the amount of other nitrogen-containing by-products, particularly to minimize the amount of other nitrogen-containing by-products in some embodiments. In one embodiment, after reaction step f), the solid water-soluble nitrogen-containing compound accounts for at most 12% of the total weight of cellulose carbamate and water-soluble nitrogen-containing compound, preferably 6% or less. The gaseous ammonia released in the reaction is evaporated, leaving only solid water-soluble nitrogen-containing compounds in the mixture. In embodiments, nitrogen-containing compounds refer to unreacted urea and non-urea compounds such as biuret and other nitrogen-containing compounds.
[0041] Water-soluble substances recovered from cellulose carbamate, such as divalent and multivalent metal ions, will accumulate in the process if they are not removed before urea is recycled to step b. In an embodiment, a wash filtrate containing urea and non-urea compounds in soluble form is recovered and preferably eluted by an ion exchange resin filled in, for example, a suitable column, preferably containing a cation exchange resin type, more preferably a strong acid cation exchange resin type, most preferably containing Amberlite SR1L NA. In a preferred embodiment, the filtrate is eluted by a cation exchange resin to remove divalent and / or multivalent cations, preferably calcium ions and optional magnesium ions from the filtrate, thereby providing an eluent. The amount of divalent cations and multivalent cations in the eluent can be ignored. In one embodiment, the wash filtrate feed is eluted at a rate appropriately varying between 2-75 dm3 / kg / h and preferably 5-25 dm3 / kg / h per kilogram of the selected cation exchange resin type. The cation exchange treatment can be carried out in the presence of monovalent cations such as sodium ions in the wash filtrate feed. In one embodiment, the wash filtrate contains up to 3000 mg / dm3 of sodium ions, more suitably up to 600 mg / dm3. In a further embodiment, the feed temperature is between 5°C and 80°C, preferably between 25°C and 45°C.
[0042] In addition to water-soluble substances such as divalent and polyvalent metal ions recovered from the cellulose carbamate, monovalent ions such as sodium ions, water-soluble anions such as chlorides, sulfates and carbonates and water-soluble organic degradation products of the cellulose polymer may also be present in the recovered wash filtrate and will accumulate in the process if they are not removed before recycling the urea to step b. In one embodiment, the eluate obtained from the ion exchange treatment is preferably treated by membrane filtration, suitable for separating the following substances: monovalent ions, anions, dissolved degradation products of the cellulose polymer, and preferably most of other nitrogen-containing compounds such as sodium and ammonium carbamate, and degradation products of the cellulose polymer reacted in the carbamation reaction of urea and biuret in the presence of urea. In a particular embodiment, the membrane filtration is carried out using a spiral wound ion-selective type membrane with a pore size suitably less than 1000 Da, preferably 100-400 Da. In one embodiment, the feed pressure is between 1.0 and 80 bar(g), more suitably between 5 and 45 bar(g), between 4 and 20 bar(g). In a further embodiment, the feed temperature is between 10°C and 70°C, and suitably between 25°C and 45°C. In an embodiment, at least a portion of the ion exchange treatment solution is collected as a permeate, suitably >60% and preferably >80% of the ion exchange treatment solution or >60% and preferably >80% volume fraction of the ion exchange treatment solution is collected as a permeate, and a second portion or the remaining volume fraction of the ion exchange treatment solution, suitably <40% and preferably <20%, is collected as a concentrate. In one embodiment, the concentrate is diafiltered, for example diluted with water and further concentrated to increase the recovery of urea and biuret. In a further embodiment, the diafiltered permeate is mixed with the permeate, or alternatively mixed with the eluate feed of the ion exchange treatment. The color of the eluent feed and the color of the recovered permeate indicate the presence of soluble degradation products of the cellulose polymer and degradation products of the cellulose polymer reacted in the carbamation reaction in the presence of urea. The permeate recovered from membrane filtration is found to be generally visually colorless. Alternatively, the color may be measured spectrophotometrically at 430 nm.
[0043] In a further embodiment, the desalination of the eluate of the ion exchange treatment is performed by electrodialysis.The amount of inorganic salts in the eluate is reduced by the electrodialysis treatment.
[0044] In another embodiment, the permeate obtained from the membrane filtration step is concentrated by evaporation, preferably from a total dissolved solids content of about 0.1 wt % up to a total dissolved solids content of about 70 wt %.
[0045] A further embodiment relates to removing biuret from the evaporated concentrate, in particular by biuret crystallization. In one embodiment, the evaporated concentrate is then suitably cooled (preferably with continuous stirring) to 5-50°C, preferably to 15-30°C, to obtain a precipitate.
[0046] In one embodiment, the obtained precipitate is filtered or centrifuged from the mother liquor. In a preferred embodiment, the unwashed precipitate contains 60 to 95% by weight of biuret, typically 75% by weight or more of biuret (analysis method: biuret with potassium sodium tartrate and Cu 2+ ions, according to the method published in Regulation (EC) No. 2003 / 2003, or by HPLC, quantitatively measured by spectrophotometer at 546 nm). Most of the biuret is present in the biuret-rich precipitate. In one embodiment, 80% to 95%, in particular 90% or more of the total amount of biuret is in the biuret-rich precipitate. In another embodiment, 5% to 20%, suitably 10% or less of the total amount of biuret is present in the mother liquor. The urea:biuret ratio in the mother liquor is preferably greater than 25:1, suitably greater than 30:1. In a further embodiment, the filtered or centrifuged biuret-rich precipitate can be suitably washed to further increase the biuret content and reduce the urea content of the recovered precipitate. The washing of the precipitate can be suitably carried out in a centrifuge or a filtering device. The washing water can be circulated and evaporated.
[0047] In a particularly preferred embodiment, urea is recovered and preferably recycled to the urea providing step b, where it is preferably combined with any fresh urea feed. This recycling of urea significantly reduces the use of raw materials, thereby reducing the environmental burden, in particular reducing the amount of nitrogen entering the wastewater system.
[0048] Further embodiments relate to extracting ammonia from the reactor. In one embodiment, the ammonia released during the reaction of cellulose and urea is separate and preferably discharged continuously. In a preferred embodiment, ammonia is recovered from the reactor by a vacuum pump and subsequent absorption in water, and optionally reacts directly with an acid to form an ammonium salt of the acid used, such as reacting with sulfuric acid to form ammonium sulfate. In another embodiment, the ammonia recovery rate is improved by injecting an inert gas stream (such as a nitrogen stream) into the reactor. The ammonia solution in the water generally has a concentration of up to about 33% by weight of ammonia solution, preferably 25% by weight of an ammonia solution. Gaseous ammonia can optionally be directed to other integrated processes or condensed into liquid ammonia. Salts of ammonia and acid, such as ammonium sulfate, are generally recovered in the form of a saturated aqueous solution, or further crystallized into a hydrated salt or a dehydrated salt in solid form.
[0049] As mentioned above, the pressure of the mixture is preferably not more than 350 mbar(a). In one embodiment, the mixture is subjected to a pressure of not more than 300 mbar(a), in particular to a pressure of 10 mbar(a) to less than 250 mbar(a), for example to a pressure of 50 to 200 mbar(a). In a preferred embodiment, the mixture obtained in step c) is subjected to reduced pressure in step d) without the need for an intermediate step of removing water from the mixture. Preferably, eliminating the intermediate step of removing water from the mixture reduces the complexity of the process. In the initial stages of the carbamate reaction, reduced pressure is used to help remove residual free water from the mixture of cellulose and urea.
[0050] As mentioned above, in one embodiment, the pressure is released after the carbamation reaction. In a specific embodiment, the pressure is released in step f) to ambient pressure.
[0051] In an embodiment, the cellulose and urea are mechanically processed while forming a mixture of cellulose and urea. The mechanical processing preferably changes the accessibility of the cellulose fiber to the urea, thereby increasing, for example, the yield of the carbamation reaction, and in particular increasing the uniformity of the cellulose carbamate recovered from the carbamation reaction. In another embodiment, the mechanical processing includes a step of shear mixing in a mechanical mixing device, in particular a continuous mechanical mixing device. Various mixing devices can be used in embodiments of the present invention. In an embodiment, the mechanical mixing device is selected from a knife mill, a hammer mill, a ball mill, a disc mill, a pelletizer and an extruder. In a preferred embodiment, the mechanical device is a pelletizer, such as a Kahl press. Other pelletizers suitable for mechanical mixing of cellulose-based materials as described herein are also suitable for embodiments of the present invention.
[0052] In a further embodiment, the mixture is continuously mixed during steps d) and e) until the carbamation reaction is complete. Suitably, the continuous mixing drives the carbamation reaction to completion. Optimized continuous mixing helps to discharge released ammonia from the cellulose-urea mixture during the carbamation reaction. Continuous mixing also helps to prevent prolonged contact between the hot surfaces of the reactor and the cellulose-urea mixture during the carbamation reaction. Even if any contact occurs between the cellulose-urea mixture in the reactor, the reduced pressure used also balances the rate of chemical reaction between cellulose and urea and the rate of by-product formation in the side reactions.
[0053] In an embodiment, the initial solids content of the mixture of cellulose and urea in water in the aqueous phase is at least 25% by weight of the composition, preferably at least 50% by weight of the composition, suitably at least 65% by weight of the composition, in particular up to 75% by weight of the mixture, most preferably 71% by weight or 72% by weight or 73% by weight or 74% by weight of the mixture. Mechanical processing of (such as these) ultra-high consistency cellulose media or cellulose pulp provides improved dislocation of the lamellae in the fiber cell wall compared to low consistency cellulose media or cellulose pulp, resulting in improved absorption of chemicals such as urea at the molecular level in the mixture or pulp. An initial solids content of at least 25% by weight of the mixture ensures effective treatment of the cellulose, i.e., the cellulose walls are subjected to sufficient shear forces to effectively disrupt the cell walls and increase the accessibility of the cellulose fibrils to solvents and chemicals. The cellulose is best processed when the initial solids content is at least 50% by weight of the mixture, preferably the initial solids content is 50% by weight of the mixture or more, for example more than 50% by weight of the mixture, such as 51% by weight of the mixture, 52% by weight of the mixture, or for example 55% by weight of the mixture, suitably at least 65% by weight of the mixture, in particular up to 75% by weight, most preferably 71% or 72% or 73% or 74% by weight of the mixture.
[0054] In one embodiment, the dry matter content of the mixture formed from the cellulosic raw material and urea is greater than 50% by weight, in particular greater than 60% by weight, and typically about 65 to 95% by weight.
[0055] The cellulosic raw material can be provided at the desired moisture level or, when provided in the form of an aqueous slurry, can be provided at the desired consistency. After optional pretreatment, when the cellulosic raw material is provided in the form of an aqueous slurry, its consistency can be increased by dehydration or drying. The dehydration or drying step can be performed before mixing with urea or preferably after said mixing.
[0056] Regardless of the source of the raw materials, an alkaline pH may be beneficial for fibrillating cellulose or enhancing its reactivity with urea. In one embodiment, some alkali is usually dehydrated to be fed to step c before it needs to be mixed with the cellulose medium. Alternatively, alkali can be added by sucking an alkaline solution into the cellulose medium during the dehydration step or after dehydration, for example, before the mixture is fed to step c. In one embodiment, the pH of the alkalized cellulose medium is 10.0 or higher, preferably 10.5 or higher, and optionally the pH is in the range of 7.0 to 14.0. The pH of the alkalized cellulose medium corresponds to the pH of the liquid measured by standing or extracting 10g of alkalized and dehydrated cellulose medium in 100g of water and measuring the pH of the obtained water extract or aqueous solution. In order to achieve the preferred pH of the liquid, 1-15g of alkali is usually added per kg of dry cellulose. The alkali can be selected from alkali metal hydroxides or carbonates or a combination thereof. Preferably, the alkali is sodium hydroxide. In case of an integrated unit for the preparation of a cellulose raw material and the carbamation of said raw material, the pH of the cellulose medium can be adjusted to a preferred level for the carbamation process already in the last process stage of the raw material preparation.
[0057] In another embodiment, the cellulosic medium is dewatered and mechanically treated without the addition of alkali.
[0058] In one embodiment, the degree of polymerization (DP) of the cellulose raw material in step a is DP 250 to 800, preferably DP 270 to 400. According to ISO 5351, a degree of polymerization value of DP 250 corresponds to an intrinsic viscosity of 197 ml / g. In addition, for natural fiber derived cellulose raw materials such as cotton derived raw materials, or for chemical or dissolving pulp raw materials or dissolving pulp raw materials, in one embodiment, if the DP is higher than the preferred range of DP 270 to 400, hydrogen peroxide or other peroxy compounds can be used to adjust the DP. For cellulose raw materials, in one embodiment, hydrogen peroxide or other peroxy compounds are used to adjust the DP. In another embodiment, the adjustment of DP is carried out using an acid, such as an inorganic acid or an organic acid, or a combination of acids. Sulfuric acid can be used as the acid for adjusting the DP. It is advantageous for the optimal molecular weight distribution of the raw material to include DP adjustment by acid treatment in the preparation of the cellulose raw material, or to treat the raw material with an acid before mixing the cellulose with urea in step c. Hydrogen peroxide is usually and optionally added in step c.
[0059] In step c, preferably 11-22% urea is added by weight of dry cellulose pulp.
[0060] In one embodiment, the degree of polymerization (DP) of the cellulose carbamate recovered, washed and dried in step g is DP 200 to DP 400, in particular about DP 250 or higher. A degree of polymerization value of DP 250 corresponds to an intrinsic viscosity of 197 ml / g.
[0061] In one embodiment, the degree of substitution (DS) of the cellulose carbamate recovered, washed and dried in step g is from 0.1 to 0.3, in particular about 0.25 or less. After dissolution, the DS of the cellulose carbamate is slightly reduced. The degree of substitution of the cellulose carbamate is determined by the total nitrogen content determination according to SFS 5505:1988. A degree of substitution value of 0.24 corresponds to a total nitrogen content of 2.0% per absolute dry water-insoluble fraction of the cellulose carbamate.
[0062] In one embodiment, the cellulose carbamate recovered, washed and dried in step g has a water-insoluble content of typically at least 99.0%, suitably at least 99.2%, preferably at least 99.5%, as determined by a gravimetric method, i.e., by extracting a known amount of cellulose carbamate with a known amount of hot water and determining the dissolved solid content in the filtered water extract, the water-insoluble content (%) = 100% - water-soluble content (%).
[0063] In one embodiment, the cellulose carbamate recovered, washed and optionally dried in step g can be used as a raw material for making textile staple fibers or filaments, nonwoven fibers, films, sponges and sleeves.
[0064] Next, the embodiments will be explained by the following examples.
[0065] Example
[0066] Example 1.: Batch carbamation under reduced pressure in a mixed reactor
[0067] A cellulose pulp raw material suitable for cellulose carbamate production having a degree of polymerization (DP) of 413 (measured as CED viscosity according to modified ISO 5351) prepared from recycled cotton textile waste was prepared as described in Finnish Patent Application No. FI20205250.
[0068] Cellulose carbamate The cellulose pulp was prepared in a mixing reactor of the type A. The pulp prepared from recycled cotton textile waste was dehydrated in the presence of sodium hydroxide under vacuum conditions at a dosage of 6 g / kg of air-dried cellulosic material to a dry matter content of about 85% by weight of the mixture. The pH of the liquid in the alkali-treated material was determined by placing 10 g of the dehydrated material in 100 g of water, and the pH of the aqueous solution was measured to be 10.5. Hydrogen peroxide (0.24% H2O2 by weight of the dry cellulose pulp) was mixed with an aqueous urea solution (18.5% urea by weight of the dry fiber pulp) and the mixture was added to the pulp. After adding the aqueous solutions of urea and hydrogen peroxide, the dry matter content of the cellulose-urea-sodium hydroxide mixture obtained was 72±2% of the weight of the mixture, which is conducive to flexible mechanical processing. The mechanical pretreatment was carried out six times in sequence by shear mixing in a pelletizer-type continuous mechanical mixing device (6).
[0069] The mixture of mechanically pretreated pulp, urea, hydrogen peroxide and water is placed back into the mixing reactor. The mixture is subjected to a reduced pressure of 350 mbar (a) and continuously mixed while flushing with nitrogen under reduced pressure and elevated temperature to form cellulose carbamate. When the temperature reaches 133° C., the carbamation reaction time is started and the temperature of the actual carbamation reaction is raised to about 135° C. After reaching the target initial temperature of 133° C., the total reaction time is 180 minutes. The ammonia released during the carbamation reaction is washed in water and recovered as aqueous ammonia (as ammonium hydroxide solution).
[0070] After carbamation, the cellulose carbamate particles are ground by a pelletizer device to obtain a mixture in the form of particles. The ground cellulose carbamate in the form of a powder is washed with water to remove soluble nitrogen-containing compounds. The washing procedure is carried out by slurrying the ground cellulose carbamate in water at 50° C., the slurry containing about 10% by weight of cellulose carbamate. The cellulose carbamate slurry is pumped into a filter press device for pressing out a filtrate containing most of the water-soluble nitrogen-containing compounds and non-urea compounds. The filtrate is recovered to recover unreacted urea and separate most of the reaction by-products.
[0071] The washed cellulose carbamate was recovered with a dry matter content of about 54% by weight and subsequently dried at a temperature below 130° C. The degree of polymerization of the cellulose carbamate was DP 268 (determined as CED viscosity according to ISO 5351), the degree of substitution was 0.19 (determined as total nitrogen content according to SFS 5505:1988), the content of water-insoluble matter was 99.2% (determined gravimetrically, i.e. by extracting a known amount of cellulose carbamate with a known amount of hot water and determining the dissolved solid content in the filtered water extract, the amount of water-insoluble matter (%) = 100% - water-soluble matter (%)), and was measured in the washed and dried cellulose carbamate sample.
[0072] The dissolution of cellulose carbamate was performed as described in Finnish Patent Application No. FI20206386.
[0073] For the wet spinning of cellulose carbamate fibers, the obtained cellulose carbamate solution is subsequently filtered using a two-stage backwash filtration process, using a 15 μm filter medium in the second filtration stage. The wet spinning of the filtered and degassed cellulose carbamate stock solution is carried out using a spinning bath optimized for the cellulose carbamate process, which contains, for example, sodium sulfate and free sulfuric acid. Under hot bath stretching conditions, the godet stretching stress applied during fiber sampling is 73-80%. The obtained filament titer is 1.3 dtex. The fiber breaking toughness measured from the filament samples is >22 cN / tex (SFS-EN ISO 5079).
[0074] Example 2: Recovery of unreacted urea and separation of organic carbamate reaction byproducts and inorganic salts from cellulose carbamate washing filtrate
[0075] 1m 3 Wash filtrate, equivalent to the filtrate recovered from the carbamate reaction and suspended in 2.5 m 3 250 kg of cellulose carbamate in demineralized water, obtained from a filter press as described in Example 1. For the ion exchange treatment, the filtrate was passed through an ion exchange column filled with 36 kg of cation exchange resin type Amberlite SR1L NA at about 500 dm 3 / h to remove calcium and magnesium ions from the filtrate.
[0076]
[0077] The eluate obtained from the ion exchange treatment is then treated by membrane filtration to separate monovalent ions and most other nitrogen-containing compounds such as sodium and ammonium carbamate from urea and biuret. Membrane filtration is performed using an ion-selective membrane with a porosity of 200 Da by circulating the solution through the membrane and returning it to the feed container as a concentrate. The feed rate is 440 dm 3 / h and 700dm 3 The feed pressure was varied between 12.0 bar(g) and 13.7 bar(g). 87% of the ion exchange treated solution was collected as permeate and the remaining 13% was collected as concentrate.
[0078]
[0079] The permeate obtained from the membrane filtration step was subsequently concentrated by evaporation from a total dissolved solids content of 0.5 wt % to a total dissolved solids content of 60 wt %.
[0080] The evaporated concentrate was then subjected to a biuret crystallization treatment by cooling the hot concentrate to about 25° C. while continuously stirring. The precipitate obtained was filtered off from the mother liquor. The unwashed precipitate contained 77% by weight of biuret (analytical method: biuret with potassium sodium tartrate and Cu 2+ ion complex, quantitatively measured by spectrophotometer at 546 nm according to the method published in Regulation (EC) No. 2003 / 2003, or quantitatively measured by HPLC). 8% of the total amount of biuret is present in the mother liquor, and the remaining 92% is present in the biuret-rich precipitate. The ratio of urea to biuret in the mother liquor is 30:1.
[0081] Example 3: Carbamate formation under reduced pressure
[0082] The cellulose pulp raw material was treated according to the procedure described in Example 1. The alkaline mixture of cellulose and urea was recovered from the mechanical mixing device in the form of granules.
[0083] The granule batch was divided into 6 equal portions of 500 g each. Each granule portion was separately placed in a stainless steel cooking pot in a thin layer of about 1 cm. Each portion in the cooking pot was separately carbamate-treated in a vacuum oven under the following conditions: 1) 180 minutes at 130°C and 250 mbar(a), 2) 180 minutes at 140°C and 250 mbar(a), 3) 180 minutes at 150°C and 250 mbar(a), 4) 180 minutes at 135°C and 500 mbar(a), 5) 180 minutes at 135°C and 150 mbar(a), 6) 180 minutes at 135°C and 50 mbar(a). Tests 1-4 were carried out under nitrogen flushing, tests 5-6 were carried out without nitrogen flushing.
[0084] The obtained cellulose carbamate particles are recovered and ground. The powdered material is washed to remove water-soluble nitrogen-containing compounds as follows: about 25 g of cellulose carbamate of known water content are accurately weighed into a 1000 ml volumetric flask, about 800 ml of boiling demineralized water are added, and the water-soluble compounds are extracted from the cellulose carbamate into the aqueous solution. The slurry of cellulose carbamate in water is cooled and tempered to 20° C. The volumetric flask is filled to the mark (1000 ml) with demineralized water. The cellulose carbamate slurry is allowed to settle in the volumetric flask. An aliquot of the solution is taken and the undissolved particles are filtered out. The urea and biuret contents in the filtrate are selectively determined by HPLC, and the total nitrogen content is determined by SFS 5505:1988. The total amount of water-soluble compounds in the aqueous solution is determined gravimetrically by evaporating an aliquot of the aqueous solution. Based on HPLC analysis, urea and nitrogen were converted to nitrogen stoichiometrically and the content of other nitrogen-containing compounds other than urea and biuret was calculated by subtracting urea and biuret nitrogen from the total nitrogen content. These results were calculated as the percentage of urea, biuret and other nitrogen-containing compounds in the water-soluble portion of the recovered cellulose carbamate.
[0085]
[0086]
[0087] It should be understood that the embodiments of the present invention disclosed are not limited to the specific structures, process steps or materials disclosed herein, but are extended to equivalents thereof recognized by those of ordinary skill in the relevant art. It should also be understood that the terminology employed herein is only used for the purpose of describing specific embodiments and is not intended to be limiting.
[0088] In this specification, reference to an embodiment or embodiments means that a particular feature, structure or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present invention. Therefore, the phrases "in one embodiment" or "in an embodiment" appearing in various places in this specification do not necessarily all refer to the same embodiment. Where terms such as, for example, "about" or "substantially" are used to refer to a value, the exact value is also disclosed.
[0089] As used herein, for convenience, multiple items, structural elements, constituent elements and / or materials can be presented in a public list. However, these lists should be understood as each member in the list being individually identified as a separate and unique member. Therefore, in the absence of contrary instructions, no single member on such a list should be interpreted as being in fact equivalent to any other member in the same list based solely on its performance in a common group. In addition, various embodiments and embodiments of the present invention may be mentioned herein together with alternatives to the various components of the present invention. It should be understood that such embodiments, embodiments and alternatives should not be interpreted as equivalents to each other in fact, but should be regarded as independent and autonomous manifestations of the present invention.
[0090] In addition, the described features, structures or characteristics can be combined in any suitable manner in one or more embodiments. In the following description, many specific details, such as examples of length, width, shape, etc., are provided to provide a comprehensive understanding of the embodiments of the present invention. However, those skilled in the relevant art will recognize that the present invention can be practiced without one or more specific details, or practiced using other methods, components, materials, etc. In other cases, well-known structures, materials or operations are not shown or described in detail to avoid confusing various aspects of the present invention.
[0091] Although the above embodiments illustrate the principles of the present invention in one or more specific applications, it is obvious that those skilled in the art can make a lot of modifications to the form, usage and implementation details without creative work and without departing from the principles and concepts of the present invention. Therefore, except for the limitations of the attached claims, the above is not intended to limit the present invention.
[0092] In this document, the verbs "comprise" and "include" are used as open limitations, neither excluding nor requiring the presence of unrecited features. The features recited in the dependent claims are mutually freely combinable unless expressly stated otherwise. Furthermore, it is to be understood that the use of "a" or "an" throughout this document, i.e. the singular, does not exclude the plural.
[0093] Industrial Applicability
[0094] At least some embodiments of the present invention have industrial application in the production of cellulose carbamates, particularly in the production of cellulose carbamates suitable for use in spinning dopes for preparing cellulose carbamate fibers for use in woven and nonwoven fabrics.
[0095] Reference List
[0096] Patent Literature
[0097] Finnish Patent No.112869
[0098] Finnish Patent No.112795
[0099] Finnish Patent No.128164
Claims
1. A method for producing cellulose carbamate in an aqueous phase, The following steps are involved: a) providing cellulose raw material; b) providing urea; c) mixing cellulose and urea to provide a mixture; d) subjecting the mixture to a reduced pressure not exceeding 350 mbar absolute; e) heating the mixture to a temperature of 130 to 150° C. to react the cellulose with urea to form cellulose carbamate, provided that the reaction is carried out in the absence of liquid ammonia; f) Relieve pressure; g) recovering the cellulose carbamate, and h) washing the cellulose carbamate with water to remove water-soluble nitrogen-containing compounds, wherein the water-soluble nitrogen-containing compounds account for up to 12% of the total weight of the cellulose carbamate and the water-soluble nitrogen-containing compounds.
2. The method according to claim 1, wherein the water-soluble nitrogen-containing compound accounts for 6% or less of the total weight of cellulose carbamate and the water-soluble nitrogen-containing compound.
3. The method according to claim 1, wherein the urea is an aqueous solution of urea. The method according to claim 2 , wherein the urea is an aqueous solution of urea.
5. The method according to any one of claims 1 to 4, wherein the mixture is heated at 130 to 140°C for 60 to 240 minutes.
6. The method of claim 5, wherein the mixture is heated at 135±3°C for 60 to 240 minutes.
7. The method of claim 6, wherein the mixture is heated at 135±3°C for 120 to 180 minutes.
8. The method of claim 7, wherein the mixture is heated at 135±3°C for 150 minutes.
9. The method of any one of claims 1-4 and 6-8, wherein the mixture of cellulose and urea is optionally flushed with an inert gas during heating under reduced pressure to form cellulose carbamate.
10. The method of any one of claims 1-4 and 6-8, wherein the pressure is released after the reaction of cellulose with urea is complete thereby forming cellulose carbamate.
11. The method of claim 9, wherein the pressure is released after the reaction of cellulose and urea is complete to thereby form cellulose carbamate.
12. The method according to any one of claims 1 to 4, 6 to 8 and 11, wherein the cellulose carbamate obtained by the reaction of cellulose and urea is washed with water to remove non-urea compounds from the cellulose carbamate.
13. The method of any one of claims 1-4, 6-8 and 11, wherein water-soluble non-gaseous nitrogen-containing compounds and non-urea compounds are recovered separately from the cellulose carbamate and recovered in the form of an aqueous solution.
14. The method of claim 12, wherein the water-soluble non-gaseous nitrogen-containing compounds and non-urea compounds are recovered separately from the cellulose carbamate and recovered in the form of an aqueous solution.
15. The method of claim 13, wherein non-urea compounds are separated from the aqueous solution.
16. The method of claim 14, wherein non-urea compounds are separated from the aqueous solution.
17. The method of claim 15, wherein a majority of the non-urea compounds are separated from the aqueous solution.
18. The method of claim 16, wherein a majority of the non-urea compounds are separated from the aqueous solution.
19. The process of claim 13, wherein the recovered aqueous solution is optionally concentrated by evaporation.
20. The process of claim 14, wherein the recovered aqueous solution is optionally concentrated by evaporation.
21. The process according to any one of claims 15 to 18, wherein the recovered aqueous solution is optionally concentrated by evaporation.
22. The process according to any one of claims 15 to 18, wherein the separation of non-urea compounds is performed by a selective separation method selected from ion exchange, membrane filtration, electrodialysis and crystallization.
23. The process according to claim 21, wherein the separation of non-urea compounds is performed by a selective separation method selected from the group consisting of ion exchange, membrane filtration, electrodialysis and crystallization.
24. The process according to any one of claims 15-18 and 21, wherein urea is recovered.
25. The method according to claim 24, wherein urea is recovered and recycled to the urea providing step b.
26. A process according to claim 25, wherein in step b the urea is combined with any fresh urea feed.
27. The method of any one of claims 1-4, 6-8, 11, 14-20, 23 and 25-26, comprising separately extracting any ammonia released during the reaction between cellulose and urea.
28. A method according to claim 27, comprising continuously extracting any ammonia released during the reaction between cellulose and urea.
29. The process of claim 27, wherein the ammonia gas is recovered and optionally reacted with an acid to form an ammonium salt of the corresponding acid.
30. The process of claim 28, wherein the ammonia gas is recovered and optionally reacted with an acid to form an ammonium salt of the corresponding acid.
31. The method of any one of claims 1-4, 6-8, 11, 14-20, 23, 25-26, and 28-30, wherein the mixture is subjected to a pressure not exceeding 300 mbar absolute.
32. The method of claim 31 , wherein the mixture is subjected to a pressure of from 10 mbar absolute to less than 250 mbar absolute.
33. The method of claim 32, wherein the mixture is subjected to a pressure of 50 to 200 mbar absolute.
34. The method of claim 31, wherein the pressure is relieved in step f to become ambient pressure.
35. The method of claim 32, wherein the pressure is relieved in step f to become ambient pressure.
36. The method of claim 33, wherein the pressure is relieved in step f to become ambient pressure.
37. The method of any one of claims 1-4, 6-8, 11, 14-20, 23, 25-26, 28-30, and 32-36, wherein the cellulose and urea are subjected to mechanical processing when forming the mixture of cellulose and urea.
38. The method of claim 37, wherein the mechanical processing comprises a step of shear mixing in a mechanical mixing device.
39. The method of claim 38, wherein the mechanical processing comprises a step of shear mixing in a continuous mechanical mixing device.
40. The method of any one of claims 1-4, 6-8, 11, 14-20, 23, 25-26, 28-30, 32-36, and 38-39, wherein the mixture of cellulose and urea has an initial solids content of at least 25% by weight of the mixture.
41. The process of claim 40, wherein the mixture of cellulose and urea has an initial solids content of at least 50% by weight of the mixture.
42. The process of claim 41, wherein the mixture of cellulose and urea has an initial solids content of at least 65% by weight of the mixture.
43. The process of claim 42, wherein the mixture of cellulose and urea has an initial solids content of at most 75% by weight of the mixture.
44. The process of claim 43, wherein the mixture of cellulose and urea has an initial solids content of 71 % or 72 % or 73 % or 74 % by weight of the mixture.
45. The process according to any one of claims 1-4, 6-8, 11, 14-20, 23, 25-26, 28-30, 32-36, 38-39 and 41-44, wherein the mixture obtained in step c) is subjected to reduced pressure in step d) without an intermediate step of removing water from the mixture.
46. The method of any one of claims 1-4, 6-8, 11, 14-20, 23, 25-26, 28-30, 32-36, 38-39, and 41-44, wherein the mixture is continuously mixed during steps d) and e) until the carbamation reaction is complete.
47. The method of claim 45, wherein the mixture is continuously mixed during steps d) and e) until the carbamation reaction is complete.
Citation Information
Patent Citations
Method for producing cellulose carbamate
FI128164B
Separation of polycotton blends
FI20205250A
Method for the production of cellulose carbamate moulded bodies
CA2487248A1
Process for the preparation of cellulose derivatives
CN111592603A