Composite current collector with lithium-philic structure, preparation method and battery
By forming a modified copper cluster structure with surface-loaded silver particles in the composite liquid collection, the problems of uneven lithium deposition and dendrite growth in lithium metal batteries are solved, the electrochemical performance and cycle life are improved, and the internal resistance of the battery is reduced.
Patent Information
- Application Number
- CN202311346035.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-10-18
AI Technical Summary
The composite liquid collector has problems such as uneven lithium deposition, disordered growth of lithium dendrites and instability of SEI interface in lithium metal batteries, which affect cycle life and safety.
Using polyimide film as the substrate, a composite metal film is formed by magnetron sputtering and two-stage constant voltage electrodeposition, covering the sputtered metal layer and the electroplating metal layer, and forming a surface through modified solution drop coating and temperature gradient changes. The modified copper cluster structure of silver particles is improved by improving the lithium-philicity of the composite fluid collection.
Effectively alleviate the problems of uneven lithium deposition and dendrite growth, improve electrochemical performance, reduce battery internal resistance, extend cycle life and improve safety.
Smart Images

Figure CN117219783B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery current collectors, and in particular to a composite current collector with a lithium-philic structure, a preparation method and a battery. Background Art
[0002] Composite current collectors generally refer to composite materials composed of a polymer film as the middle layer and thin metal layers on both sides. Compared with conventional current collectors made of metal foil, composite current collectors have obvious advantages in reducing costs, improving safety performance and increasing battery energy density, and have received extensive attention and development in recent years.
[0003] Although composite current collectors have significant effects in improving the electrochemical performance and safety performance of batteries, there are also some problems that need to be solved, such as the weak interaction between the relatively smooth metal layer and the active material, the large contact resistance at the interface between the composite current collector and the active material, etc., which will lead to battery capacity loss and poor rate performance. When composite current collectors are used in lithium metal batteries, problems such as disordered growth of lithium dendrites, unstable SEI interface layer, and large volume changes of lithium metal will also seriously affect the cycle life and safety of lithium metal batteries. Summary of the invention
[0004] In view of this, the present invention provides a composite current collector with a lithium-philic structure, a preparation method and a battery, which can effectively alleviate the problems of uneven lithium deposition and disordered growth of lithium dendrites in lithium metal batteries during the cycle process. The composite current collector prepared by this method has better electrochemical properties.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] In a first aspect, an embodiment of the present invention provides a method for preparing a composite current collector having a lithium-philic structure, the method comprising:
[0007] A composite metal film with a sputtered metal layer and an electroplated metal layer on the surface is obtained in sequence by magnetron sputtering and two-stage constant voltage electrodeposition using a polyimide film as a substrate; wherein the sputtered metal layer covers the surface of the polyimide film, and the electroplated metal layer covers the surface of the sputtered metal layer; wherein the electroplated metal layer includes a copper cluster consisting of a plurality of copper columns growing perpendicular to the sputtered metal layer;
[0008] The modified solution is dripped onto the surface of the composite metal film, and the liquid level change of the modified solution is controlled by changing the temperature gradient to obtain a composite current collector with a lithium-philic structure on the surface; wherein the lithium-philic structure is a modified copper cluster with silver particles loaded on the surface.
[0009] Preferably, the modified solution is an N-methylpyrrolidone solution with a silver nitrate content of 0.01 to 0.1 M.
[0010] Preferably, the step of controlling the liquid level of the solution by changing the temperature gradient comprises:
[0011] The modified solution is dropped onto the clean surface of the composite metal film, and the reaction environment is adjusted to a vacuum state. The initial temperature of the reaction environment is 25-30°C and maintained for 10-20 minutes; then the ambient temperature is adjusted to 45-50°C, the heating rate is 1-10°C / min, and maintained for 10-20 minutes; then the ambient temperature is adjusted to 60-65°C, the heating rate is 1-10°C / min, and maintained for 10-20 minutes to complete the gradient distribution treatment of the silver particles.
[0012] Preferably, the silver particles have a particle size of 100 to 300 nm, and are distributed in a gradient manner on the copper clusters vertical to the film, with a change rate of -0.3 to 0.5 wt.% / μm.
[0013] Preferably, the aspect ratio of each copper column in the copper cluster is 2-3:1, the distance between two adjacent copper columns is 1-5 μm, and the height of each copper column is 6-10 μm.
[0014] Preferably, the voltage of the first stage of the two-stage constant voltage electrodeposition is 0.1-0.3V, and the voltage of the second stage is 1.5-2V.
[0015] In a second aspect, an embodiment of the present invention provides a composite current collector having a lithium-philic structure, which is prepared by the method for preparing a composite current collector having a lithium-philic structure described in any embodiment of the present invention.
[0016] In a third aspect, an embodiment of the present invention provides a battery, comprising the composite current collector with a lithium-philic structure as described in any embodiment of the present invention.
[0017] The embodiment of the present invention provides a composite current collector with a lithium-philic structure, a preparation method and a battery. A polyimide film is used as a substrate, and a composite metal film with a sputtered metal layer and an electroplated metal layer on the surface is obtained in sequence by magnetron sputtering and two-stage constant voltage electrodeposition; wherein the sputtered metal layer covers the surface of the polyimide film, and the electroplated metal layer covers the surface of the sputtered metal layer; wherein the electroplated metal layer includes a copper cluster composed of a plurality of copper columns growing perpendicular to the sputtered metal layer; a modified solution is dripped onto the surface of the composite metal film, and the liquid level height of the modified solution is controlled by changing the temperature gradient to obtain a composite current collector with a lithium-philic structure on the surface; wherein the lithium-philic structure is a modified copper cluster with silver particles loaded on the surface.
[0018] Compared with the prior art, it has the following beneficial effects:
[0019] (1) The present application is based on an in situ substitution reaction between a lithium-philic metal and a base metal, and controls the liquid level change of the modified solution by changing the temperature gradient, thereby obtaining a modified copper cluster with good binding force and gradient distribution characteristics on the surface of the composite current collector. The method is simple, efficient, and has strong applicability;
[0020] (2) The electroplated metal layer containing copper clusters in the present application, wherein the gaps between the copper columns provide space for the deposition of lithium and limit the volume change of lithium during the deposition process, and the gradient distribution of lithium-philic silver particles on the surface of the modified copper clusters can not only reduce the nucleation overpotential of lithium, but also guide the deposition of lithium metal at the bottom of the modified copper clusters, alleviate the uncontrollable growth of lithium dendrites on the surface of the current collector, and improve the cycle performance of the battery;
[0021] (3) The modified copper cluster structure on the surface of the composite current collector in the present application can improve the conductivity of the copper cluster structure on the surface of the composite current collector to a certain extent, reduce the internal resistance of the battery, and reduce voltage polarization due to the presence of silver particles on the surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A cross-sectional view of a composite metal film that has not been treated with a modified solution provided in one embodiment of the present invention;
[0023] Figure 2 A surface image of a composite metal film that has not been treated with a modified solution provided in one embodiment of the present invention;
[0024] Figure 3 A cross-sectional view of a composite metal film treated with a modified solution provided in one embodiment of the present invention;
[0025] Figure 4 A surface image of a composite metal film treated with a modified solution provided in one embodiment of the present invention. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0027] Embodiment 1
[0028] A composite current collector with a lithium-philic structure prepared in accordance with an embodiment of the present invention is as follows:
[0029] (1) placing a polyimide film in a vacuum chamber, evacuating the vacuum chamber, and introducing argon gas as a protective gas, wherein the argon gas pressure is 0.1 to 10 Pa; magnetron sputtering is performed on the surface of the polyimide film through the action of a direct current negative high voltage radio frequency voltage to prepare a sputtered metal layer with a thickness of 0.5 μm, thereby completing the metallization treatment of the polyimide film;
[0030] (2) immersing the metallized polyimide film in an acetone solution, performing ultrasonic treatment at an ultrasonic frequency of 40 kHz for 5 minutes; then immersing the film in a 5% dilute sulfuric acid solution for 20 seconds; placing the cleaned metallized polyimide film in an electrodeposition solution at a solution temperature of 25° C., a first constant voltage electrodeposition voltage of 0.2 V, an electrodeposition time of 20 seconds, and a second electrodeposition voltage of 1.8 V, an electrodeposition time of 2.5 minutes, completing the construction of a copper cluster structure to obtain a composite metal film;
[0031] (3) Place the composite metal film with the copper cluster structure in a silver nitrate solution so that the surface of the composite metal film is flush with the liquid surface. The concentration of the silver nitrate solution is 0.05M, and the solvent of the silver nitrate solution is N-methylpyrrolidone. Adjust the reaction environment to a vacuum state with a vacuum degree of -0.1MPa. The initial temperature of the reaction environment is 25-30°C and maintained for 15 minutes; then adjust the ambient temperature to 45-50°C, the heating rate is 5°C / min, and maintained for 15 minutes; then adjust the ambient temperature to 60-65°C, the heating rate is 5°C / min, and maintained for 15 minutes. Complete the gradient distribution of silver particles to obtain the composite current collector with a lithium-philic structure;
[0032] (4) The composite current collector with a lithium-philic structure obtained above is used in a lithium metal battery, that is, lithium metal is used as the negative electrode active material, lithium bis(trifluoromethanesulfonyl imide) dissolved in 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME) (v / v) = 1:1 and 2 wt.% LiNO3 is used as the electrolyte in the battery, and Celgard 2400 is used as the separator to prepare a lithium metal battery. 2 The current density is 1 mAh / cm 2 The area capacity of the composite current collector was cycled to test the nucleation point of lithium and the polarization voltage after cycling for 400 hours.
[0033] Embodiment 2
[0034] A composite current collector with a lithium-philic structure prepared in accordance with an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the second step of the electrodeposition time is adjusted to 3 minutes in the "electrodeposition" step for the experiment.
[0035] Embodiment 3
[0036] A composite current collector with a lithium-philic structure prepared in accordance with an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the second step of the electrodeposition time is adjusted to 2 minutes in the "electrodeposition" step for the experiment.
[0037] Embodiment 4
[0038] A composite current collector with a lithium-philic structure prepared in an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the concentration of the silver nitrate solution is adjusted to 0.01M in the "chemical silver plating treatment" step for the experiment.
[0039] Embodiment 5
[0040] A composite current collector with a lithium-philic structure prepared in accordance with an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the concentration of the silver nitrate solution is adjusted to 0.1 M in the "chemical silver plating treatment" step for the experiment.
[0041] Embodiment 6
[0042] A composite current collector with a lithium-philic structure prepared in an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the heating rate is adjusted to 10°C / min in the "chemical silver plating treatment" step for the experiment.
[0043] Embodiment 7
[0044] A composite current collector with a lithium-philic structure prepared in an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the heating rate is adjusted to 1°C / min in the "chemical silver plating treatment" step for the experiment.
[0045] Embodiment 8
[0046] A composite current collector with a lithium-philic structure prepared in an embodiment of the present invention is consistent with the specific implementation method of Example 1, except that the insulation time in the "chemical silver plating treatment" step is adjusted to 20 minutes for the experiment.
[0047] Embodiment 9
[0048] A composite current collector with a lithium-philic structure prepared in accordance with an embodiment of the present invention is consistent with the specific implementation method in Example 1, except that the insulation time in the "chemical silver plating treatment" step is adjusted to 10 minutes for the experiment.
[0049] Comparative Example 1
[0050] The comparative example of the present invention omits two constant voltage electrodeposition steps, and directly performs the modification and subsequent steps on the composite current collector.
[0051] The average change rate of silver content in the upward direction of the composite current collector surface prepared in this experiment is zero. After 400 hours of cycling, the polarization voltage increases rapidly and the battery short-circuits.
[0052] Comparative Example 2
[0053] A composite current collector with a lithium-philic structure is prepared as a comparative example of the present invention. The specific implementation method is consistent with that of Example 1, except that the concentration of the silver nitrate solution is 1M in the step of "dropping the modified solution onto the composite metal film".
[0054] A composite current collector with a lithium-philic structure prepared by using these experimental parameters has a high surface silver content, and the average change rate of the silver content in the upward direction of the composite current collector surface is zero.
[0055] Comparative Example 3
[0056] A composite current collector with a lithium-philic structure is prepared as a comparative example of the present invention. The specific implementation method is consistent with that of Example 1, except that the solution of the modified solution is changed to deionized water for the experiment.
[0057] The silver content on the surface of the composite current collector prepared by this experimental parameter is zero. The modified solution prepared by this experimental parameter is difficult to fully infiltrate the surface of the composite current collector. The gaps between the copper clusters cannot be exposed to the modified solution, and the silver particles are difficult to adhere to the surface of the copper clusters.
[0058] See Table 1 and Table 2, which are comparative summaries of the effects of the second electrodeposition time, silver nitrate concentration, heating rate, and holding time on the average change rate of silver content, lithium nucleation overpotential, and polarization voltage after 400 hours of cycling in the embodiments of the present invention. The average change rate of silver content in the table refers to: the average silver content is calculated at three points at the bottom, middle, and top of the copper cluster, and the average change rate of the silver content of the entire copper cluster is calculated based on the average silver content of the three parts. It can be seen from the table:
[0059] (1) The second electrodeposition time in Example 1 is 2.5 min, the silver nitrate concentration is 0.05 M, the heating rate is 5°C / min, and the holding time is 15 min. The prepared composite current collector with a lithium-philic structure is a composite current collector with optimal parameters, with an average change rate of silver content of -0.473 wt.% / μm, a lithium nucleation overpotential of 42 mV, and a polarization voltage of 24 mV after 400 hours of circulation.
[0060] (2) By comparing Example 1 with Comparative Examples 1 and 2, it can be concluded that in Comparative Example 1, since there is no two-stage constant voltage electrodeposition step, it is difficult to complete the construction of the copper cluster structure on the surface of the composite current collector, and the silver particles do not have a gradient distribution on the surface of the composite current collector, which makes it difficult to guide the deposition of lithium from bottom to top, which is not conducive to improving the electrochemical performance of the battery; in Comparative Example 2, the silver content on the surface of the composite current collector is very high, and a metallic silver layer has been formed covering the surface of the composite current collector, and the metallic silver fills the gaps between the copper clusters. At this time, it is difficult for the composite current collector to effectively limit the volume change of lithium during the deposition process.
[0061] (3) By comparing Examples 1, 4, and 5, it can be concluded that the silver nitrate concentration has the greatest influence on the average change rate of the silver content of the composite current collector with a lithium-philic structure. By comparing the average change rate of the silver content and the polarization voltage after 400 hours of cycling, too high or too low a silver nitrate content will affect the electrochemical properties of the composite current collector.
[0062] (4) By comparing Examples 1, 2, 3, 6, 7, 8, and 9, it can be concluded that the second stage electrodeposition time, heating rate, and holding time have little effect on the average change rate of the silver content of the composite current collector with a lithium-philic structure. By comparing the nucleation point positions and the polarization voltage after 400 hours of circulation, it can be concluded that the electrodeposition parameters in Example 1 are optimal.
[0063]
[0064] Table 1
[0065]
[0066] Table 2
[0067] In summary, the embodiments of the present invention provide a composite current collector with a lithium-philic structure, a preparation method and a battery, wherein a polyimide film is used as a substrate, and a composite metal film having a sputtered metal layer and an electroplated metal layer on the surface is obtained in sequence by magnetron sputtering and two-stage constant voltage electrodeposition; a modified solution is dripped onto the surface of the composite metal film, and the liquid level height change of the modified solution is controlled by changing the temperature gradient to obtain a composite current collector having a lithium-philic structure on the surface; wherein the sputtered metal layer covers the surface of the polyimide film, and the electroplated metal layer covers the surface of the sputtered metal layer; wherein the electroplated metal layer includes a copper cluster composed of a plurality of copper columns growing perpendicular to the sputtered metal layer; wherein the lithium-philic structure is a modified copper cluster with silver particles loaded on the surface.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement and improvement made within the spirit and scope of the present invention are included in the protection scope of the present invention.
Claims
1. A method for preparing a composite current collector having a lithium-philic structure, characterized in that: The method comprises: A composite metal film with a sputtered metal layer and an electroplated metal layer on the surface is obtained in sequence by magnetron sputtering and two-stage constant voltage electrodeposition using a polyimide film as a substrate; wherein the sputtered metal layer covers the surface of the polyimide film, and the electroplated metal layer covers the surface of the sputtered metal layer; wherein the electroplated metal layer includes a copper cluster consisting of a plurality of copper columns growing perpendicular to the sputtered metal layer; The modified solution is dripped onto the surface of the composite metal film, and the liquid level of the modified solution is controlled by changing the temperature gradient to obtain a composite current collector having a lithium-philic structure on the surface; wherein the lithium-philic structure is a modified copper cluster with silver particles loaded on the surface; The modified solution is a 0.01-0.1 M silver nitrate solution, and the solvent is N-methylpyrrolidone; The step of controlling the liquid level of the modified solution by changing the temperature gradient comprises: The modified solution is drop-coated on the surface of the composite metal film, and the reaction environment is adjusted to a vacuum state. The initial temperature of the reaction environment is 25-30 °C and maintained for 10-20 min; then the ambient temperature is adjusted to 45-50 °C, the heating rate is 1-10 °C / min, and maintained for 10-20 min; then the ambient temperature is adjusted to 60-65 °C, the heating rate is 1-10 °C / min, and maintained for 10-20 min to complete the gradient distribution of silver particles.
2. The method for preparing a composite current collector having a lithium-philic structure according to claim 1, characterized in that: The silver particles have a particle size of 100-300 nm, and are distributed in a gradient manner on the copper clusters of the vertical film, with a change rate of -0.3-0.5 wt.% / μm.
3. The method for preparing a composite current collector having a lithium-philic structure according to claim 1, characterized in that: The aspect ratio of each copper column in the copper cluster is 2-3:1, the distance between two adjacent copper columns is 1-5 μm, and the height of each copper column is 6-10 μm.
4. The method for preparing a composite current collector having a lithium-philic structure according to claim 1, characterized in that: The voltage of the first stage of the two-stage constant voltage electrodeposition is 0.1-0.3 V, and the voltage of the second stage is 1.5-2 V.
5. A composite current collector having a lithium-philic structure, characterized in that: The composite current collector having a lithium-philic structure is prepared by the preparation method according to any one of claims 1 to 4.
6. A battery, characterized in that: It includes the composite current collector with a lithium-philic structure as described in claim 5.