Negative pressure hollow tungsten arc-laser coaxial composite welding method

By forming a negative pressure area in hollow tungsten arc-laser coaxial composite welding, the problem of shielding laser energy by metal steam is solved, the welding efficiency and stability are improved, efficient melting deep welding is achieved, and welding defects are reduced. Suitable for complex paths and medium-thick plate welding.

CN118023712BActive Publication Date: 2024-11-22SHANGHAI UNIV OF ENG SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410273327.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-11
Publication Date
2024-11-22
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

Hollow tungsten arc-laser coaxial composite welding technology has the effect of shielding and hindering laser energy by metal steam in the arc area, resulting in low welding stability and efficiency. The melt pool melting depth is insufficient during welding of medium and thick plates, which is easy to cause welding. Defects and positive arc pressure lead to instability of the melt pool, affecting welding forming and accuracy.

Method used

The negative pressure hollow tungsten arc-laser coaxial composite welding method is adopted to form a negative pressure area in the center of the arc, change the metal steam density distribution and molten pool movement law, and use the negative pressure to transform the arc positive pressure into the upward adsorption negative pressure to increase the Welding efficiency and stability, and negative pressure is generated through magnetic field or pumping + magnetic field, and the negative pressure is regulated to optimize the welding process.

Benefits of technology

It improves welding efficiency and stability, increases weld melting depth, concentrates central energy, reduces welding defects, is suitable for welding complex paths and medium-thick plates, and improves welding quality and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118023712B_ABST
    Figure CN118023712B_ABST
Patent Text Reader

Abstract

The invention provides a negative pressure hollow tungsten electrode arc-laser coaxial hybrid welding method, comprising: preparation before welding, adjusting the relative position of the laser and the axis of the hollow tungsten electrode, setting a welding power supply, setting laser parameters and hollow tungsten electrode arc parameters, and turning on the welding power supply and the laser to form a negative pressure area; through the above steps, a negative pressure is formed in the center of the hollow tungsten electrode, the shielding and obstruction effect of the metal vapor in the center of the hollow tungsten electrode arc on the laser energy is reduced, and the laser energy utilization rate is improved; the energy density of the laser entering the keyhole is increased, the weld penetration is increased, the welding defects are reduced, the weld quality is improved, and the efficiency and stability of the arc-laser coaxial hybrid welding are further increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hollow arc-laser welding, and in particular to a negative pressure hollow tungsten arc-laser coaxial composite welding method. Background Art

[0002] Hollow tungsten arc welding technology changes the welding current density distribution and arc pressure form by changing the shape of the tungsten electrode, greatly reducing the arc pressure and ensuring good weld formation. However, when using a hollow tungsten arc, the current density, temperature, and plasma flow rate on the arc center axis are significantly reduced, resulting in low welding speed and low production efficiency.

[0003] Further development of hollow tungsten arc-laser coaxial hybrid welding technology, the synergistic effect of laser addition, the composite heat source can give full play to the respective advantages of laser and arc, and can improve the stability of welding process and welding efficiency to a certain extent; at the same time, reduce the spatial size of the welding gun and the influence of asymmetric heat source in complex path welding. However, hollow tungsten arc-laser coaxial hybrid welding technology also has technical bottlenecks: (1) The shielding and obstruction of the metal vapor in the arc area on the laser energy leads to low laser energy utilization, which in turn causes poor welding stability and low welding efficiency; at the same time, when welding medium and thick plates, due to the lack of energy concentration in the central area, it is easy to cause the molten pool of the workpiece to be welded to have a shallow molten depth, and it is impossible to obtain an efficient and stable large molten depth welding process, which is easy to cause energy waste and increase welding defects; (2) In conventional hollow tungsten arc-laser coaxial hybrid welding technology, the excavation effect of the positive pressure of the arc on the molten pool will cause the molten pool to be unstable and produce welding defects. In thin-wall cladding and tilted welding, the weld pool will flow to the side wall under the action of gravity, arc blowing force and surface tension, reducing the accuracy and performance of the welded workpiece. Although the side wall flow phenomenon of the weld pool can be improved by physical constraints, physical constraints occupy a large welding workpiece and have poor flexibility in dealing with different welding situations, which cannot meet the welding and forming of complex components. At the same time, excessive arc pressure will also produce spatter during the welding process, reducing the welding quality.

[0004] In view of this, the present invention proposes a negative pressure hollow tungsten arc-laser coaxial hybrid welding method to solve the above problems. Summary of the invention

[0005] In order to solve the above problems, the purpose of the present invention is to propose a negative pressure hollow tungsten arc-laser coaxial hybrid welding method to obtain more stable welding quality and higher welding efficiency.

[0006] The above purpose is achieved through the following technical solutions:

[0007] A negative pressure hollow tungsten arc-laser coaxial composite welding method specifically comprises the following steps:

[0008] Step 1: Preparation before welding: Before welding, grind or clean the workpiece to be welded, and fix the grinded or cleaned workpiece to be welded;

[0009] Step 2: Adjust the relative position of the laser and the hollow tungsten electrode axis: Make the laser pass vertically through the center of the hollow tungsten electrode to ensure that the laser can be coaxially set with the hollow tungsten electrode;

[0010] Step 3: Set the welding power supply: Connect one end of the welding power supply to the hollow tungsten electrode and the other end to the workpiece to be welded. The direction and size of the welding current can be changed according to the welding process requirements;

[0011] Step 4: Set the laser parameters and hollow tungsten arc parameters: laser power 100-5000W, laser spot diameter 0.3-0.5mm; set the hollow tungsten welding current 90-360A, welding speed 1-100mm / s, tungsten outer diameter 1.8-5mm, tungsten inner diameter 0.8-1.2mm, tungsten height 3-8mm;

[0012] Step 5: Turn on the welding power supply and laser to form a negative pressure area: The laser is emitted from the center of the hollow tungsten electrode to the arc area, forming an arc-laser coaxial composite heat source, which acts together on the surface of the workpiece to be welded, so that the workpiece moves with the operating platform. By forming a negative pressure area in the center of the arc, the negative pressure is 0 to -300Pa. The negative pressure is transformed from the digging effect of the positive pressure of the arc on the molten pool to the negative pressure of upward adsorption, thereby changing the density distribution of metal vapor in the arc and the movement law in the molten pool, thereby improving the welding efficiency and welding stability.

[0013] Furthermore, in step 5, the laser is CO 2 Gas laser, YAG solid laser, semiconductor laser or fiber laser; the laser output mode is continuous laser or pulsed laser;

[0014] Further, the laser is a scanning laser, and the laser scanning path is in the shape of a straight line, a figure eight, a circle, a polygon, a sawtooth or a sine wave, and each scanning path has two different beam movement directions, clockwise and counterclockwise;

[0015] Furthermore, the negative pressure of 0 to -300Pa in step 5 is generated by magnetic field or vacuum + magnetic field; the magnetic field mode is continuous alternating magnetic field mode, intermittent alternating magnetic field mode, pulsed magnetic field mode, or pulsed alternating magnetic field mode; the magnetic field mode is longitudinal magnetic field mode or rotating longitudinal magnetic field mode;

[0016] Furthermore, the magnitude of the negative pressure in step 5 can be changed to different degrees by changing the magnetic field strength and the current magnitude, the magnetic field strength is 0.02 to 0.06 T, and the negative pressure is a relative pressure based on the atmospheric pressure;

[0017] Further, the method is applicable to negative pressure arc-laser composite welding technology, or negative pressure arc-laser composite additive manufacturing technology, or negative pressure arc-laser paraxial composite welding technology, or negative pressure arc-laser composite cladding technology, or negative pressure arc-high energy beam composite welding technology, or negative pressure arc-high energy beam composite cladding technology, or negative pressure arc-high energy beam composite additive manufacturing technology, or negative pressure arc-laser composite cleaning technology, or negative pressure arc-laser composite cutting technology, or negative pressure arc-laser composite surface shot peening strengthening treatment technology, or negative pressure arc-laser composite brazing technology, or negative pressure arc-laser composite processing technology;

[0018] Furthermore, the method is applicable to aluminum alloy materials, or magnesium alloy materials, or titanium alloy materials, or high-temperature alloy materials, or copper alloy materials, or cemented carbide materials, or ferrous metal materials, or metal-based composite materials, or high-entropy alloy materials, or refractory metal materials.

[0019] Beneficial effects of the present invention:

[0020] 1. By generating a negative pressure area at the center of the arc and adjusting the negative pressure of appropriate size, the metal vapor in the center of the hollow tungsten electrode arc can be guided to impact upward and disperse to the surroundings, thereby reducing the shielding and obstruction of the metal vapor on the laser energy during the arc-laser coaxial hybrid welding process, improving the laser energy utilization rate, and further increasing the efficiency and stability of the arc-laser coaxial hybrid welding; at the same time, the energy density of the laser entering the keyhole is increased, the weld penetration is increased, the center energy is more concentrated, and the energy utilization rate is improved, so that an efficient and stable large penetration welding process can be obtained, which has significant advantages for deep penetration welding of medium and thick plate materials.

[0021] 2. The hollow tungsten arc and laser heat source are coaxially combined to ensure welding efficiency while ensuring welding quality. At the same time, the spatial size of the welding gun is reduced, and the influence of the asymmetry of the heat source on the welding direction is reduced, the stability of the welding process is improved, and automatic welding, deposition and additive manufacturing of complex paths can be easily realized.

[0022] 3. Compared with the solid tungsten electrode arc, the use of hollow tungsten electrode can improve the welding efficiency by applying a large current, while avoiding abnormal welding defects such as melt-through and hump caused by the increase in arc pressure due to the increase in current during the welding process.

[0023] 4. By forming an arc negative pressure on the surface of the welding molten pool in the opposite direction of gravity, the molten pool can be sucked upward and the flow behavior of the molten pool can be changed. The use of arc negative pressure can improve the molten pool flow problem and welding defects during the welding process, thereby improving the welding quality and efficiency, which has important research significance.

[0024] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a process principle diagram of the present invention;

[0026] Figure numerals: 1 workpiece; 2 hollow tungsten electrode; 3 laser; 4 arc; 5 negative pressure area; 6 molten pool; 7 magnetic field; 8 welding power supply. DETAILED DESCRIPTION

[0027] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0028] In the description of the present invention, unless otherwise specified, "plurality" means two or more than two; the orientations or positional relationships indicated by the terms "upper", "lower", "left", "right", "inner", "outer", "front end", "rear end", "head", "tail", etc. are based on the orientations or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0029] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0030] Combine the following Figure 1 The present invention provides a negative pressure hollow tungsten arc-laser coaxial hybrid welding method, which specifically includes the following steps:

[0031] Step 1: Preparation before welding;

[0032] Step 2: Adjust the relative position between the laser and the hollow tungsten electrode axis;

[0033] Step 3: Set up welding power supply;

[0034] Step 4: Set the laser parameters and hollow tungsten arc parameters;

[0035] Step 5: Turn on the welding power supply and laser to form a negative pressure area.

[0036] like Figure 1 As shown, before welding, the workpiece 1 to be welded is polished or cleaned, and after the polished or cleaned workpiece 1 to be welded is fixed, the laser 3 is vertically passed through the center of the hollow tungsten electrode 2 to ensure that the laser 3 can be coaxially arranged with the hollow tungsten electrode 2, and one end of the welding power supply 8 is connected to the hollow tungsten electrode 2, and the other end is connected to the workpiece 1 to be welded. According to the welding process requirements, the direction and size of the welding current 8 can be changed; the laser power is 100-5000W, and the laser spot diameter is 0.3-0.5mm; the hollow tungsten electrode 2 welding current is set to 90-360A, the welding speed is 1-100mm / s, the outer diameter of the tungsten electrode is 1.8-5mm, and the inner diameter of the tungsten electrode is 0.8 ~1.2mm, tungsten electrode height 3~8mm; laser 3 is injected from the center of hollow tungsten electrode 2 into arc 4 area, forming arc-laser coaxial composite heat source, which acts together on the surface of workpiece 1 to be welded, so that workpiece 1 moves with the operating platform, and forms negative pressure area 5 in the center of arc 4 (negative pressure arc is defined as an arc that forms negative pressure in the horizontal position opposite to the direction of gravity), the negative pressure is 0 to -300Pa, and the negative pressure is converted from the digging effect of the positive pressure of the arc on the molten pool to the negative pressure of upward adsorption, thereby changing the density distribution of metal vapor in arc 5 and the movement law in the molten pool, thereby improving welding efficiency and welding stability.

[0037] The laser in step 5 is CO 2 Gas laser, YAG solid laser, semiconductor laser or fiber laser; the laser output mode is continuous laser or pulsed laser.

[0038] The laser is a scanning laser, and the laser scanning path is in the shape of a straight line, an 8, a circle, a polygon, a sawtooth or a sine wave. Each scanning path has two different beam movement directions, clockwise and counterclockwise.

[0039] The negative pressure of 0 to -300Pa in step 5 is generated by magnetic field 7 or vacuum + magnetic field 7; the magnetic field mode is continuous alternating magnetic field mode, intermittent alternating magnetic field mode, pulsed magnetic field mode, or pulsed alternating magnetic field mode; the magnetic field mode is longitudinal magnetic field mode or rotating longitudinal magnetic field mode. It should be noted that the magnetic field is only a means of forming negative pressure. The invention emphasizes the impact of negative pressure on hollow tungsten arc-laser coaxial composite welding. Other means of forming negative pressure in the future will fall within the scope of protection of the invention.

[0040] The magnitude of the negative pressure in step 5 can be changed to different degrees by changing the magnetic field strength and the current. The magnetic field strength is 0.02 to 0.06 T, and the negative pressure is a relative pressure based on the atmospheric pressure.

[0041] The method is applicable to negative pressure arc-laser composite welding technology, or negative pressure arc-laser composite additive manufacturing technology, or negative pressure arc-laser paraxial composite welding technology, or negative pressure arc-laser composite cladding technology, or negative pressure arc-high energy beam composite welding technology, or negative pressure arc-high energy beam composite cladding technology, or negative pressure arc-high energy beam composite additive manufacturing technology, or negative pressure arc-laser composite cleaning technology, or negative pressure arc-laser composite cutting technology, or negative pressure arc-laser composite surface shot peening strengthening treatment technology, or negative pressure arc-laser composite brazing welding technology, or negative pressure arc-laser composite processing technology.

[0042] The method is applicable to aluminum alloy materials, or magnesium alloy materials, or titanium alloy materials, or high-temperature alloy materials, or copper alloy materials, or hard alloy materials, or ferrous metal materials, or metal-based composite materials, or high-entropy alloy materials, or refractory metal materials.

[0043] Embodiment 1

[0044] The negative pressure hollow tungsten arc-laser coaxial hybrid welding method for 316 stainless steel in this embodiment specifically includes the following steps:

[0045] The first step is preparation before welding; grind or clean the 316 stainless steel to remove surface burrs or bumps, and fix the cleaned 316 stainless steel on a plane with a plate thickness of 10mm;

[0046] The second step is to adjust the relative position of the axis of the laser 3 and the hollow tungsten electrode 2; move the hollow tungsten electrode 2 to the top of the 316 stainless steel to be welded. The parameters of the hollow tungsten electrode 2 are 1.8mm tungsten electrode outer diameter, 0.8mm tungsten electrode inner diameter, and 3mm tungsten electrode height. After the position of the hollow tungsten electrode 2 is set, move the laser so that the laser 3 passes through the center of the hollow tungsten electrode 2 to ensure that the hollow tungsten electrode 3 and the laser 2 are on the same axis during welding;

[0047] The third step is to set the welding power supply 8; connect the welding power supply 8 through the wire, connect one end of the welding power supply 8 to the hollow tungsten electrode 2, and the other end to the workpiece 1 to be welded. The direction and size of the welding current 8 can be changed according to the welding process requirements;

[0048] The fourth step is to set the laser parameters and hollow tungsten electrode arc parameters; select a fiber laser, the laser output mode is continuous laser, the laser scanning path is "I" shaped, the laser power is 900W, the laser spot diameter is 0.5mm, and the scanning path is clockwise; set the hollow tungsten electrode 2 welding current to 100A and the welding speed to 10mm / s.

[0049] The fifth step is to turn on the welding power supply 8 and the laser to form a negative pressure area 5; the laser 3 is injected from the center of the hollow tungsten electrode 2 into the arc 4 area to form an arc-laser coaxial composite heat source, which acts together on the surface of the 316 stainless steel to be welded, so that the 316 stainless steel moves with the operating platform, and applies a downward external longitudinal continuous alternating magnetic field 7, by forming a negative pressure area 5 in the center of the arc 4, and obtaining a negative pressure of -100Pa by changing the magnetic field strength and the current size. The negative pressure is converted from the excavation effect of the positive pressure of the arc on the molten pool 6 to an upward adsorption negative pressure, guiding the metal vapor in the center of the hollow tungsten electrode arc to impact upward and disperse to the surroundings, slowing down the shielding and obstruction of the metal vapor on the laser energy during the arc-laser coaxial composite welding process, improving the laser energy utilization rate, and further increasing the efficiency and stability of the arc-laser coaxial composite welding, and the welding efficiency is improved by 22-25%; by forming an arc negative pressure opposite to the gravity direction on the surface of the welding molten pool, the molten pool 6 can be sucked upward, changing the flow behavior of the molten pool 6, Figure 1 The concave molten pool 6 surface in the dotted line area is transformed into a full molten pool 6 surface in the solid line area, reducing welding defects; at the same time, increasing the energy density of the laser entering the keyhole, Figure 1 The dotted area at the bottom of the molten pool 6 is transformed into a solid area, the penetration depth is increased by 20%, the molten width is increased by 12%, the center energy is more concentrated, the energy utilization rate is improved, and an efficient and stable large penetration welding process is obtained.

[0050] Embodiment 2

[0051] The hollow tungsten electrode negative pressure hollow tungsten electrode arc-laser coaxial hybrid welding method of Invar alloy in this embodiment specifically includes the following steps:

[0052] The first step is preparation before welding; grind or clean the Invar alloy to remove surface burrs or bumps, and fix the cleaned Invar alloy on a plane with a plate thickness of 7mm;

[0053] The second step is to adjust the relative position of the axis of the laser 3 and the hollow tungsten electrode 2; move the hollow tungsten electrode 2 to the top of the Invar alloy to be welded. The parameters of the hollow tungsten electrode 2 are 2.5mm tungsten electrode outer diameter, 1mm tungsten electrode inner diameter, and 3.5mm tungsten electrode height. After the position of the hollow tungsten electrode is set, move the laser so that the laser 3 passes through the center of the hollow tungsten electrode 2 to ensure that the hollow tungsten electrode 3 and the laser 2 are on the same axis during welding;

[0054] The third step is to set the welding power supply 8; connect the welding power supply 8 through the wire, connect one end of the welding power supply 8 to the hollow tungsten electrode 2, and the other end to the workpiece 1 to be welded. The direction and size of the welding current 8 can be changed according to the welding process requirements;

[0055] The fourth step is to set the laser parameters and hollow tungsten electrode arc parameters; select a fiber laser, the laser output mode is continuous laser, the laser scanning path is an "I" shape, the laser power is 4000W, the laser spot diameter is 0.45mm, and the scanning path is clockwise; set the hollow tungsten electrode 2 welding current to 160A and the welding speed to 20mm / s.

[0056] The fifth step is to turn on the welding power supply and the laser to form a negative pressure area; the laser 3 is injected from the center of the hollow tungsten electrode 2 into the arc 4 area to form an arc-laser coaxial composite heat source, which acts on the surface of the Invar alloy to be welded, so that the Invar alloy moves with the operating platform, and applies a downward external longitudinal intermittent alternating magnetic field 7, and forms a negative pressure area 5 in the center of the arc 4. By changing the magnetic field strength and the current size, a negative pressure of -180Pa is obtained, and the negative pressure is converted from the excavation effect of the arc positive pressure on the molten pool to an upward adsorption negative pressure, guiding the metal vapor in the center of the hollow tungsten electrode arc to impact upward and disperse to the surroundings, slowing down the shielding and obstruction of the metal vapor on the laser energy during the arc-laser coaxial composite welding process, improving the laser energy utilization rate, and further increasing the efficiency and stability of the arc-laser coaxial composite welding, and the welding efficiency is improved by 11-21%; by forming an arc negative pressure opposite to the gravity direction on the surface of the welding molten pool 6, the molten pool 6 can be sucked upward to change the flow behavior of the molten pool 6. Figure 1 The concave molten pool 6 surface in the dotted line area is transformed into a full molten pool 6 surface in the solid line area, reducing welding defects; at the same time, increasing the energy density of the laser entering the keyhole, Figure 1 The dotted area at the bottom of the molten pool 6 is transformed into a solid area, the penetration depth is increased by 26%, the molten width is increased by 18%, the center energy is more concentrated, the energy utilization rate is improved, and an efficient and stable large penetration welding process is obtained.

[0057] Embodiment 3

[0058] The hollow tungsten electrode negative pressure hollow tungsten electrode arc-laser coaxial hybrid welding method of 6082-T6 aluminum alloy in this embodiment specifically includes the following steps:

[0059] The first step is preparation before welding; grind or clean the 6082-T6 aluminum alloy to remove surface burrs or bumps, and fix the cleaned 6082-T6 aluminum alloy on a plane with a plate thickness of 6mm;

[0060] The second step is to adjust the relative position of the axis of the laser 3 and the hollow tungsten electrode 2; move the hollow tungsten electrode 2 to the top of the 6082-T6 aluminum alloy to be welded. The parameters of the hollow tungsten electrode are 4mm tungsten electrode outer diameter, 1.2mm tungsten electrode inner diameter, and 6mm tungsten electrode height. After the position of the hollow tungsten electrode 2 is set, move the laser so that the laser 3 passes through the center of the hollow tungsten electrode 2 to ensure that the hollow tungsten electrode 2 and the laser 3 are on the same axis during welding;

[0061] The third step is to set the welding power supply 8; connect the welding power supply 8 through the wire, connect one end of the welding power supply 8 to the hollow tungsten electrode 2, and the other end to the workpiece 1 to be welded. The direction and size of the welding current 8 can be changed according to the welding process requirements;

[0062] The fourth step is to set the laser parameters and hollow tungsten electrode arc parameters; select a fiber laser, the laser output mode is continuous laser, the laser scanning path is an "I" shape, the laser power is 3000W, the laser spot diameter is 0.48mm, and the scanning path is clockwise; set the hollow tungsten electrode 2 welding current to 120A and the welding speed to 36mm / s.

[0063] The fifth step is to turn on the welding power supply 8 and the laser to form a negative pressure area 5; the laser 3 is injected from the center of the hollow tungsten electrode 2 into the arc 4 area to form an arc-laser coaxial composite heat source, which acts together on the surface of the 6082-T6 aluminum alloy to be welded, so that the 6082-T6 aluminum alloy moves with the operating platform, and a downward external longitudinal intermittent alternating magnetic field 7 + exhaust (-10kPa) is applied to form a negative pressure area 5 in the center of the arc 4. By changing the magnetic field strength and the current size, a negative pressure of -150Pa is obtained. The negative pressure is exerted by the positive pressure of the arc on the molten metal. The excavation effect of the pool is transformed into an upward adsorption negative pressure, which guides the metal vapor in the center of the hollow tungsten electrode arc to impact upward and disperse to the surroundings, thereby reducing the shielding and obstruction of the metal vapor on the laser energy during the arc-laser coaxial hybrid welding process, improving the laser energy utilization rate, and further increasing the efficiency and stability of the arc-laser coaxial hybrid welding. The welding efficiency is improved by 27-30%; by forming an arc negative pressure opposite to the direction of gravity on the surface of the welding molten pool 6, the molten pool 6 can be sucked upward, changing the flow behavior of the molten pool 6, Figure 1 The concave molten pool 6 surface in the dotted line area is transformed into a full molten pool 6 surface in the solid line area, reducing welding defects; at the same time, increasing the energy density of the laser entering the keyhole, Figure 1 The dotted area at the bottom of the molten pool 6 is transformed into a solid area, the penetration depth is increased by 25%, the molten width is increased by 15%, the center energy is more concentrated, the energy utilization rate is improved, and an efficient and stable large penetration welding process is obtained.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A negative pressure hollow tungsten arc-laser coaxial hybrid welding method, characterized in that: The specific steps include: Step 1: Preparation before welding: Before welding, grind or clean the workpiece to be welded, and fix the grinded or cleaned workpiece to be welded; Step 2: Adjust the relative position of the laser and the hollow tungsten electrode axis: make the laser pass vertically through the center of the hollow tungsten electrode to ensure that the laser and the hollow tungsten electrode are coaxially set; Step 3: Set the welding power supply: Connect one end of the welding power supply to the hollow tungsten electrode and the other end to the workpiece to be welded. The direction and size of the welding current can be changed according to the welding process requirements; Step 4: Set the laser parameters and hollow tungsten arc parameters; Step 5: Turn on the welding power supply and the laser to form a negative pressure area: The laser is injected from the center of the hollow tungsten electrode into the arc area to form an arc-laser coaxial composite heat source, which acts on the surface of the workpiece to be welded, so that the workpiece moves with the operating platform, and an external magnetic field in a downward direction is applied to form a negative pressure area in the center of the arc. The negative pressure is converted from the excavation effect of the positive pressure of the arc on the molten pool to the negative pressure of upward adsorption. By forming an arc negative pressure in the opposite direction of gravity on the surface of the welding molten pool, the molten pool can be sucked upward, the flow behavior of the molten pool is changed, and the metal vapor in the center of the hollow tungsten electrode arc is guided to impact upward and disperse to the surroundings, which reduces the shielding and obstruction of the metal vapor on the laser energy during the arc-laser coaxial composite welding process. At the same time, the energy density of the laser entering the keyhole is increased, the central energy is more concentrated, and the laser energy utilization rate is improved, thereby changing the density distribution of the metal vapor in the arc and the movement law in the molten pool, and the concave molten pool surface is transformed into a full molten pool surface, thereby improving the welding efficiency and welding stability; The process parameters of the negative pressure hollow tungsten electrode arc-laser coaxial hybrid welding method are: welding 316 stainless steel, the plate thickness is 10mm, the outer diameter of the hollow tungsten electrode is 1.8mm, the inner diameter of the tungsten electrode is 0.8mm, the height of the tungsten electrode is 3mm, the laser power is 900W, the laser spot diameter is 0.5mm, the hollow tungsten electrode welding current is 100A, the welding speed is 10mm / s, and a longitudinal continuous alternating magnetic field is applied to form a negative pressure area with a pressure of -100Pa in the center of the arc; or, The process parameters of the negative pressure hollow tungsten electrode arc-laser coaxial hybrid welding method are: welding Invar alloy, plate thickness is 7mm, hollow tungsten electrode outer diameter is 2.5mm, tungsten electrode inner diameter is 1mm, tungsten electrode height is 3.5mm, laser power is 4000W, laser spot diameter is 0.45mm, hollow tungsten electrode welding current is 160A, welding speed is 20mm / s, and longitudinal intermittent alternating magnetic field is applied to form a negative pressure area with a pressure of -180Pa at the center of the arc; or, The process parameters of the negative pressure hollow tungsten electrode arc-laser coaxial composite welding method are: welding 6082-T6 aluminum alloy, plate thickness is 6mm, hollow tungsten electrode outer diameter is 4mm, tungsten electrode inner diameter is 1.2mm, tungsten electrode height is 6mm, laser power is 3000W, laser spot diameter is 0.48mm, hollow tungsten electrode welding current is 120A, welding speed is 36mm / s, and a longitudinal intermittent alternating magnetic field is added in combination with -10kPa exhaust to form a negative pressure area with a pressure of -150Pa in the center of the arc.

2. A negative pressure hollow tungsten arc-laser coaxial hybrid welding method according to claim 1, characterized in that: The laser is a CO2 gas laser, a YAG solid laser, a semiconductor laser or a fiber laser; the laser output mode is a continuous laser or a pulsed laser.

3. A negative pressure hollow tungsten arc-laser coaxial hybrid welding method according to claim 2, characterized in that: The laser is a scanning laser, and the laser scanning path is in the shape of a straight line, a figure eight, a circle, a polygon, a sawtooth or a sine wave. Each scanning path has two different light beam movement directions, clockwise and counterclockwise.

4. The negative pressure hollow tungsten arc-laser coaxial hybrid welding method according to claim 1, characterized in that: The magnitude of the negative pressure in step 5 can be changed to different degrees by changing the magnetic field strength and the current. The magnetic field strength is 0.02 to 0.06 T, and the negative pressure is a relative pressure based on the atmospheric pressure.