Anti-PID EVA packaging film and preparation method thereof

By using modified zeolite adsorbent and silane coupling agent modification, combined with cross-linking agent and antioxidant, the problems of aging and PID effect of EVA encapsulation film are solved, and the high-efficiency anti-PID and anti-aging performance of the film is achieved. Extends the life of photovoltaic cell components and improves photoelectric conversion efficiency.

CN118126636BActive Publication Date: 2024-10-15SUZHOU YISHENG OPTICAL MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410242681.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-04
Publication Date
2024-10-15
Estimated Expiration
2044-03-04

AI Technical Summary

Technical Problem

The existing EVA encapsulation film is prone to aging during long-term use, causing the PID effect and affecting the output power of the photovoltaic power station. Moreover, existing anti-PID measures have problems with material performance degradation and long-term failure.

Method used

Zeolite is used as the adsorbent, and through rare earth metal ion exchange and phosphate modification, combined with silane coupling agent modification, an anti-PID EVA encapsulating film with excellent adsorption and dispersion is prepared, and through the use of cross-linking agents and antioxidants Cooperate to improve the cross-linking density and antioxidant properties of the film.

Benefits of technology

It significantly improves the anti-PID performance and aging resistance of the adhesive film, prolongs the service life of photovoltaic cell components, improves photoelectric conversion efficiency, and avoids material performance degradation and long-term failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118126636B_ABST
    Figure CN118126636B_ABST
Patent Text Reader

Abstract

The present invention provides an anti-PID EVA encapsulation film and a preparation method thereof, and relates to the field of photovoltaic materials. According to weight parts, the anti-PID EVA encapsulation film is made of 100 parts of EVA resin; 0.5-1.5 parts of cross-linking agent; 1.0-2.0 parts of co-cross-linking agent; 2.0-4.0 parts of adsorbent; 0.1-0.3 parts of antioxidant; 0.1-0.3 parts of light stabilizer; 0.3-0.5 parts of coupling agent as raw materials, through a homemade adsorbent, formula optimization design, extrusion by an extruder, and cast film preparation. The encapsulation film effectively solves the problem that the currently commonly used EVA film decomposes and produces free acetic acid during outdoor use, and the presence of free acetic acid further promotes the decomposition of EVA and the PID effect, thereby affecting the service life of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photovoltaic materials, and in particular to an anti-PID EVA encapsulation adhesive film and a preparation method thereof. Background Art

[0002] Since 2013, as the photovoltaic power stations invested in the early stage at home and abroad have been connected to the grid and operated for a period of time, quality problems have emerged on a large scale. Many power stations have experienced quality problems such as snail pattern and potential induced degradation (PID). Some domestic power stations used inferior EVA (Ethylene Vinyl Acetate, ethylene-vinyl acetate copolymer) film, resulting in a degradation of up to 60% in about a year of operation.

[0003] The formation mechanism of PID is closely related to the hydrolysis of EVA and the sodium ions in the glass. When water vapor enters the interior of the module through the edge-sealed silicone or backplane, the ester bonds in the EVA are decomposed by water to produce acetic acid that can move freely. After the acetic acid reacts with the alkali precipitated on the surface of the glass, sodium ions that can move freely are produced. These sodium ions move to the surface of the battery cell under the action of an external electric field to form a leakage current. Under the action of the leakage current, positively charged carriers pass through the glass and flow to the ground through the frame, causing negative charges to accumulate on the surface of the battery cell, attracting photoelectric carriers (holes) to flow to the surface of the N-type silicon and gather, instead of flowing to the positive electrode (P pole) as in the normal state. As a result, the PID effect of output power attenuation caused by surface polarization occurs.

[0004] At present, the main basis for solving PID from the packaging material is to reduce the hydrolysis of EVA materials and increase the insulation resistance of EVA itself. Therefore, most of them adopt the method of reducing the VA (Vinyl Acetate) content in EVA film, or appropriately changing the formula to increase the volume resistivity, thereby hindering the migration of sodium ions and delaying the attenuation of PID.

[0005] CN105820764A discloses an EVA composite film for photovoltaic encapsulation with anti-PID performance. By selecting EVA resin with a VA content of 20% to 26% and combining it with other additives, the film has an anti-PID effect. Reducing the VA content can certainly alleviate PID attenuation, but it reduces the polarity of the material, deteriorates the peel strength, and reduces the degree of cross-linking, thereby increasing the risk of using the EVA film.

[0006] CN103756578A discloses a fluorine-modified EVA encapsulation film, which has good hydrolysis resistance and insulation, and achieves the purpose of anti-PID. However, by increasing its insulation, that is, increasing the volume resistivity of the EVA film, although PID can be well controlled in the short term, there is a hidden danger of failure in the long term. Because the EVA film will age and degrade during use, the volume resistivity will decrease over time, resulting in the failure of the anti-PID effect.

[0007] Therefore, in the art, it is desired to develop an effective auxiliary agent and formula for modifying the EVA encapsulation film, so as to improve the aging resistance and anti-PID performance of the EVA encapsulation film. Summary of the invention

[0008] The purpose of the present invention is to solve the problems of aging and PID effect caused by long-term use of EVA packaging films in the prior art. The present invention discloses an anti-PID EVA packaging film. By utilizing the porous structure advantage of zeolite and the synergistic effect between various components, the obtained anti-PID EVA packaging film can have excellent acetic acid adsorption and anti-PID performance, as well as excellent aging resistance.

[0009] The technical solution adopted by the present invention to solve its technical problem is:

[0010] The present invention provides an anti-PID EVA packaging film, comprising the following raw materials in parts by weight:

[0011]

[0012]

[0013] Optionally, the adsorbent is prepared according to the following method:

[0014] (1) zeolite and rare earth metal solution are subjected to ion exchange reaction under alkaline conditions to obtain modified zeolite I;

[0015] (2) placing the modified zeolite I in an amine solution and then a phosphate solution to obtain a modified zeolite II;

[0016] (3) The modified zeolite II and a silane coupling agent are placed in an alcohol solvent for a silylation coupling reaction to obtain a modified zeolite III, i.e., an adsorbent.

[0017] Optionally, the rare earth metal solution is a lanthanide metal aqueous solution with a concentration of 1.5-3.5 wt%.

[0018] Optionally, the usage ratio of the zeolite to the rare earth metal solution is 1 g: 25-50 mL.

[0019] Optionally, the concentration of the amine solution is 100-150 mg / L; the concentration of the phosphate solution is 10-20 mg / L.

[0020] Optionally, the usage ratio of the modified zeolite to the amine solution and the phosphate solution is 0.6-2.0 g:100 mL:100 mL.

[0021] Optionally, the silane coupling agent is selected from one or more of a mercaptosilane coupling agent, a vinylsilane coupling agent, an acryloxysilane coupling agent or a long-chain hydrocarbon silane coupling agent.

[0022] Optionally, the usage ratio of the modified zeolite II, the silane coupling agent and the alcohol solvent is 1 g: 3.0-5.0 g: 80 mL.

[0023] Optionally, the crosslinking agent is an organic peroxide crosslinking agent; the auxiliary crosslinking agent is an allyl type and / or an acryloxy type; the antioxidant is a hindered phenol and phosphite type compound antioxidant; the light stabilizer is a hindered amine and benzophenone type compound light stabilizer.

[0024] Another object of the present invention is to provide a method for preparing the anti-PID EVA packaging film as described above, comprising the following steps:

[0025] S1: Mixing: Mixing the raw materials according to the formula ratio to obtain a mixed raw material;

[0026] S2: Extrusion: melt blending, extrusion, casting, and cooling the mixed raw materials in step S1 in sequence to obtain an intermediate product;

[0027] S3: Film forming: The intermediate product in step S2 is subjected to thickness measurement, edge pressing, shaping, edge cutting and winding to obtain the anti-PID EVA packaging film.

[0028] Beneficial effects of the present invention:

[0029] (1) The anti-PID EVA encapsulation film provided by the present invention has a formula system containing a self-made adsorbent, which is based on zeolite and modified with phosphate, amine, rare earth structure, and a silane coupling agent. First, zeolite is a porous aluminate structure, an inorganic mineral, and can withstand high-temperature processing; at the same time, it has excellent small molecule, gas and ion adsorption, and can effectively adsorb free acetic acid produced by the decomposition of EVA; second, the amino structure adsorbed in the zeolite is alkaline, and can be neutralized with free acetic acid to form salts to reduce the content of free acetic acid in the system; third, after the rare earth metal and zeolite undergo ion exchange, on the one hand, it can effectively adsorb phosphates; on the other hand, the rare earth metal ions can form coordination with free acetic acid, further adsorb free acetic acid, and inhibit the decomposition of EVA. effect; Fourth, rare earth can absorb ultraviolet rays, slow down aging, and has photostability; Fifth, after absorbing ultraviolet rays, rare earth undergoes electron orbit energy level transition, releases visible light, and improves photoelectric conversion efficiency; Sixth, the phosphate structure in zeolite can effectively capture sodium ions and has anti-PID effect; Seventh, silane-modified zeolite has excellent dispersibility, low mobility, and long-term effects such as anti-ultraviolet aging, acid binding, anti-PID, and improved photoelectric conversion efficiency; Eighth, the adsorbent is a zeolite structure with a high specific surface area and a synergistic function.

[0030] (2) The anti-PID EVA encapsulation film provided by the present invention adopts a cross-linking agent and a co-cross-linking agent through formula design to improve the cross-linking density of the EVA film, which has a positive effect on limiting the diffusion of free acetic acid and metal ions (mainly sodium ions), slowing down the aggregation of ions on the surface of EVA and glass to the surface of the battery, and reducing the aging rate.

[0031] (3) The anti-PID EVA encapsulation film provided by the present invention has an antioxidant and a light stabilizer in the formula system. The antioxidant is a compound of hindered phenols and phosphites, and plays a role in different oxidation processes according to its antioxidant mechanism, and has an excellent antioxidant effect; the light stabilizer is a compound of hindered amine structure and benzophenone, and synergistically acts with the rare earth structure in the adsorbent, and has a high efficiency of anti-photooxidation aging function.

[0032] (4) The anti-PID EVA encapsulation film provided by the present invention has a synergistic effect of various raw material components in the formula system, has long-lasting acid binding and anti-PID functions, and has excellent anti-aging functions, and can also improve the photoelectric conversion efficiency of the film.

[0033] (5) The anti-PID EVA encapsulation film provided by the present invention has a zeolite matrix as the adsorbent in the formulation system. Zeolite is widely available and is green and environmentally friendly. It is highly operable for the industrialization of the product of the present invention and has practical significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a comparison chart of free acetic acid inventory / PID power attenuation of Example 1 and Comparative Examples 1-13. DETAILED DESCRIPTION

[0035] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0036] In order to solve the problems of aging and PID effect of EVA packaging film in the prior art due to long-term use, the present invention provides an anti-PID EVA packaging film, comprising the following raw materials in parts by weight:

[0037]

[0038]

[0039] EVA (ethylene-vinyl acetate copolymer) is the mainstream photovoltaic module packaging material on the market. As part of solar cells, EVA film is used outdoors for a long time and is exposed to extreme high and low temperatures, wind and rain, and thermal, light and oxygen aging. The aging of EVA film begins with the decomposition of its molecular chain. More precisely, it comes from the decomposition of the side groups of EVA molecules, which release small molecules of acetic acid. The presence of free acetic acid will form a weakly acidic environment, which will catalyze further decomposition. The whole process is "automatically accelerated". If the formation of free acetic acid is not effectively intervened, it will directly affect the failure of EVA materials and affect their service life.

[0040] Currently, most of the existing technologies use the addition of inorganic alkaline fillers to neutralize free acetic acid. However, this method has the problems of poor dispersibility of inorganic fillers and poor acid binding effect, which affects the mechanical properties, light transmittance and aging resistance of the material.

[0041] In addition, another issue that affects the service life of photovoltaic modules is the potential induced degradation (PID) effect of photovoltaic modules. The PID effect can cause catastrophic failure of photovoltaic modules under field conditions. The causes of the PID effect are relatively complex, mainly including the following: (1) installation method; (2) climatic conditions at the site where the photovoltaic modules are installed and used; (3) the type of photovoltaic module cells; (4) the materials used in photovoltaic modules: photovoltaic modules contain glass, encapsulation film, cells and backplanes, etc. The module materials cause Na to decay to varying degrees in actual applications. + Migration, thus triggering the PID effect.

[0042] From the perspective of materials, the research on anti-PID effect is mainly focused on Na +The mechanism of migration-induced PID effect of crystalline silicon modules is to reduce the internal ion mobility of EVA encapsulation film to prevent Na + Therefore, it is necessary to develop effective additives and formula-modified EVA encapsulation films to improve the aging and PID resistance of EVA encapsulation films.

[0043] Considering the problem of free acid in EVA film, the adsorption of zeolite is one of the first choice materials to consider. Zeolite is a general term for aluminosilicate minerals containing porous materials. Compared with organic materials, it has excellent high temperature resistance and can be subjected to conventional heat processing. During the exchange process of cations and other metal cations in zeolite, its structure will not be changed. By utilizing the ion exchange characteristics of zeolite, ion exchange can be carried out for modification. Zeolite is rich in tiny pores, and its structure is more complex than that of a honeycomb, with a huge specific surface area. These characteristics enable it to be used in many fields such as petrochemicals, military aviation, and water treatment.

[0044] The purpose of the present invention is to develop an EVA encapsulation film with acid removal and anti-PID functions to meet its use in the photovoltaic field under extreme weather. The idea of ​​implementation is: to make a self-made auxiliary agent with the function of adsorbing free acetic acid and resisting PID, while ensuring its compatibility and dispersibility in EVA. The theoretical basis for implementation is that natural zeolite has a porous structure, thus having a high specific surface area, and its porous structure has the function of adsorbing small molecules and ions. Phosphate has a good adsorption effect on sodium ions. Therefore, it has a good effect on the adsorption of amine structure after alkali treatment of natural zeolite, but the adsorption of phosphate structure is weak. Rare earth metal (lanthanide metal) ion exchange can form a complex with phosphate, thereby improving the adsorption of phosphate by zeolite; then the zeolite modified by absorption, amine and phosphate is silane-coupled to improve its compatibility and dispersibility in EVA. So far, the preparation of the adsorbent has been completed, which has the functions of efficient free acetic acid adsorption, anti-PID, anti-photooxidation aging and improving the photoelectric conversion efficiency.

[0045] The anti-PID EVA encapsulation film provided by the present invention has a self-made adsorbent in its formula system. The adsorbent is based on zeolite and is modified with phosphate, amine, rare earth structure, and a silane coupling agent. First, zeolite is a porous aluminate structure, an inorganic mineral, and can withstand high-temperature processing; at the same time, it has excellent small molecule, gas and ion adsorption, and can effectively adsorb free acetic acid produced by the decomposition of EVA; second, the amino structure adsorbed in the zeolite is alkaline, and can be neutralized with free acetic acid to form salts to reduce the content of free acetic acid in the system; third, after the rare earth metal and zeolite undergo ion exchange, on the one hand, it can effectively adsorb phosphates; on the other hand, the rare earth metal ions can form coordination with free acetic acid, further adsorb free acetic acid, and inhibit the decomposition of EVA. effect; Fourth, rare earth can absorb ultraviolet rays, slow down aging, and has photostability; Fifth, after absorbing ultraviolet rays, rare earth undergoes electron orbit energy level transition, releases visible light, and improves photoelectric conversion efficiency; Sixth, the phosphate structure in zeolite can effectively capture sodium ions and has anti-PID effect; Seventh, silane-modified zeolite has excellent dispersibility, low mobility, and long-term effects such as anti-ultraviolet aging, acid binding, anti-PID, and improved photoelectric conversion efficiency; Eighth, the adsorbent is a zeolite structure with a high specific surface area and a synergistic function.

[0046] The present invention preferably prepares the above-mentioned adsorbent according to the following method:

[0047] (1) Blending zeolite and rare earth metal solution, adjusting the pH to 9-11 with potassium hydroxide, shaking at 20-40° C. and 250 r / min for 8-12 h; after the reaction, centrifuging in a centrifuge, filtering, taking out insoluble matter, washing with deionized water until the supernatant is neutral, and drying at 50-60° C. for 12-14 h to obtain modified zeolite I;

[0048] Further, the concentration of the rare earth metal solution is preferably 1.5-3.5wt%, which may be 1.5wt%, 2.0wt%, 2.5wt%, 3.0wt%, 3.5wt%, or a range of any two values; the preferred ratio of zeolite to rare earth metal solution is 1g: 25-50mL;

[0049] (2) adding the modified zeolite I to the amine solution and the phosphate solution, respectively, at 20-30° C. and a rotation speed of 250-260 r / min, shaking for 4-6 hours, filtering, and taking the insoluble matter; obtaining the modified zeolite II;

[0050] Further, the preferred concentration of the amine solution is 100-150 mg / L, which can be 100 mg / L, 110 mg / L, 120 mg / L, 130 mg / L, 140 mg / L, 150 mg / L, or a range consisting of any two values; the preferred concentration of the phosphate solution is 10-20 mg / L, which can be 10 mg / L, 12 mg / L, 14 mg / L, 15 mg / L, 16 mg / L, 18 mg / L, 20 mg / L, or a range consisting of any two values; the preferred usage ratio of the modified zeolite to the amine solution and the phosphate solution is 0.6-2.0 g: 100 mL: 100 mL;

[0051] (3) Adding modified zeolite II and silane coupling agent to an alcohol solvent, ultrasonically oscillating for 0.5-1 h, standing at room temperature for 2-3 h, reacting at 40-80° C. for 2-12 h, filtering, taking insoluble matter, and drying at 50-60° C. for 12-14 h to obtain modified zeolite III, i.e., adsorbent.

[0052] Furthermore, it is preferred that the usage ratio of the modified zeolite II, the silane coupling agent, and the alcohol solvent is 1 g: 3.0-5.0 g: 80 mL.

[0053] The preferred zeolite of the present invention is natural zeolite;

[0054] In the present invention, the rare earth metal solution is preferably a lanthanide metal aqueous solution, and the metal ions in the lanthanide metal aqueous solution may be europium ions, lanthanum ions, erbium ions, cerium ions, holmium ions, terbium ions, gadolinium ions or yttrium ions, etc.; further, the metal ions in the lanthanide metal aqueous solution are preferably europium ions.

[0055] In the present invention, the anion in the rare earth metal salt is preferably a sulfate, a nitrate, a chloride or an acetate, etc.; further, the anion in the rare earth metal salt is preferably a chloride.

[0056] The preferred amine solution of the present invention is an aqueous solution of acrylamide, an aqueous solution of dopamine, an aqueous solution of 2-methylimidazole, an aqueous solution of diethylenetriamine, etc.; acrylamide is a reactive amine source, which can self-polymerize and copolymerize into a macromolecular structure, has low mobility, and can adsorb free acids well; dopamine, 2-methylimidazole, and diethylenetriamine are multipolar amine sources, which have good adsorption in the zeolite structure, low mobility, and adsorption of free acids; further, the preferred amine solution is an aqueous solution of acrylamide.

[0057] The preferred phosphate solution of the present invention is ammonium dihydrogen phosphate, potassium dihydrogen phosphate, ammonium monohydrogen phosphate or potassium monohydrogen phosphate; phosphate eradication has a good complexing effect on transition metals and rare earth metals, and also has an excellent capture effect on sodium ions, and its capture mechanism is as follows:

[0058] H2PO4 - +Na+ →NaHPO4 - +H +

[0059] HPO4 2- +Na + →NaPO4 2- +H + .

[0060] By capturing free sodium ions, the PID phenomenon of the EVA film can be effectively reduced; further, the preferred phosphate solution is potassium dihydrogen phosphate.

[0061] The preferred silane coupling agent of the present invention is selected from one or more of a mercaptosilane coupling agent, a vinylsilane coupling agent, an acryloxysilane coupling agent or a long-chain hydrocarbon silane coupling agent; wherein the mercapto, vinyl and acryloxy structures in the mercaptosilane coupling agent, the vinylsilane coupling agent and the acryloxysilane coupling agent are groups that can react and bond with EVA; and the long-chain hydrocarbon structure in the long-chain hydrocarbon silane coupling agent has good compatibility due to its high similarity with the PE segment in the EVA macromolecular chain.

[0062] In the present invention, the mercaptosilane coupling agent is preferably selected from KH580 or KH590; further, the mercaptosilane coupling agent is preferably KH590; the vinylsilane coupling agent is preferably selected from KH151 or KH171; further, the vinylsilane coupling agent is preferably KH171; the acryloxysilane coupling agent is preferably selected from KH570, KH571 or KH670; further, the acryloxysilane coupling agent is preferably KH570; the long-chain hydrocarbon silane coupling agent is preferably hexadecyltrimethoxysilane.

[0063] In the present invention, the preferred alcohol solvent is selected from one or more of anhydrous methanol, anhydrous ethanol, and anhydrous isopropanol; further, the preferred alcohol solvent is anhydrous ethanol.

[0064] The preferred crosslinking agent of the present invention is an organic peroxide crosslinking agent; the preferred crosslinking agent is selected from one or more of benzoyl peroxide, 2,5-dimethyl-2,5-bis(benzoyl peroxide)hexane, tert-butyl peroxycarbonate-2-ethylhexyl ester, cyclohexanone peroxide, dicyclohexyl peroxycarbonate or diisopropylbenzene peroxide; further, the preferred crosslinking agent is 2,5-dimethyl-2,5-bis(benzoyl peroxide)hexane.

[0065] The preferred auxiliary crosslinking agent of the present invention is allyl and / or acryloxy; the preferred allyl auxiliary crosslinking agent is selected from triallyl cyanurate or triallyl isocyanurate; the preferred acryloxy auxiliary crosslinking agent is selected from one or more of trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, propoxylated neopentyl glycol diacrylate, and pentaerythritol triacrylate.

[0066] The invention adopts a crosslinking agent and an auxiliary crosslinking agent through formula design to improve the crosslinking density of the EVA film, which has a positive effect on limiting the diffusion of free acetic acid and metal ions (mainly sodium ions), slowing down the aggregation of ions on the surface of EVA and glass to the surface of the battery, and reducing the aging rate.

[0067] In the present invention, the preferred antioxidant is a compound antioxidant of hindered phenols and phosphites; wherein the hindered phenol antioxidant is selected from antioxidant 1010, antioxidant 1076, antioxidant 264 or antioxidant 2246; further, the preferred hindered phenol antioxidant is antioxidant 1010; the phosphite antioxidant is selected from antioxidant 168, antioxidant 242 or antioxidant TPP; further, the preferred phosphite antioxidant is antioxidant 168.

[0068] The antioxidant in the present invention is a compound of hindered phenols and phosphites, which can play a role in different oxidation processes according to its antioxidant mechanism and has an excellent antioxidant effect.

[0069] The preferred light stabilizer of the present invention is a composite light stabilizer of hindered amines and benzophenones; wherein the hindered amine light stabilizer is selected from UV-292, UV-770 or GW540; further, the preferred hindered amine light stabilizer is UV-292; the benzophenone light stabilizer is selected from UV-0, UV-9, UV-24 or UV-531; further, the preferred benzophenone light stabilizer is UV-531.

[0070] The light stabilizer in the present invention is a hindered amine structure compounded with benzophenones, and synergistically acts with the rare earth structure in the adsorbent, and has a high-efficiency anti-photooxidation aging function.

[0071] Another object of the present invention is to provide a method for preparing the anti-PID EVA packaging film as described above, comprising the following steps:

[0072] S1: Mixing: Add raw materials according to the formula ratio into a mixer, mix and stir for 2-3 hours at a temperature of 40-50°C and a rotation speed of 80-90rpm to obtain a mixed raw material;

[0073] S2: Extrusion: Place the mixed raw materials in S1 in a twin-screw extruder, melt blend and extrude at a temperature of 80-82°C in zone 1, 90-92°C in zone 2, and 85-87°C in zone 3 at a rotation speed of 50-60rpm, discharge through a cast film die, and cool through a cast roller;

[0074] S3: Film forming: After thickness measurement, edge pressing, shaping, edge cutting and winding, the PIDEVA-resistant packaging film with a thickness of 500-550 μm is obtained.

[0075] The preparation method of the anti-PID EVA encapsulation film provided by the present invention can effectively achieve long-term acid binding and anti-PID functions through the synergistic effect of each raw material component in the formula system, and also has excellent anti-aging function and photoelectric conversion efficiency, thereby effectively extending the service life of the solar cell module; in addition, the adsorbent in the formula system uses zeolite as a matrix, and zeolite has a wide range of sources and is green and environmentally friendly, which makes the prepared anti-PID EVA encapsulation film have higher operability and feasibility in the industrial production process. Therefore, the preparation method of the anti-PID EVA encapsulation film provided by the present invention has important practical significance in industrial applications, and can bring more stable and reliable encapsulation materials to the solar photovoltaic industry, thereby promoting the sustainable development of the solar industry.

[0076] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0077] Unless otherwise specified, the antioxidants in the embodiments of the present invention and the comparative examples are antioxidant 1010 and antioxidant 168 added in a mass ratio of 1:2; the light stabilizers are UV-292 and UV-531 added in a mass ratio of 1:2; the coupling agent is silane coupling agent KH570; the EVA resin has a VA content of 28-33%; in the embodiments of the present invention, the EVA resin with a VA content of 33% and a melt index (MI) of 31 is preferably purchased from DuPont of the United States;

[0078] Example 1

[0079] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0080] EVA resin 100 parts;

[0081] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0082] Triallyl isocyanurate 0.5 parts;

[0083] 0.3 parts of trimethylolpropane trimethacrylate;

[0084] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0085] Pentaerythritol triacrylate 0.4 parts;

[0086] 3.0 parts of adsorbent;

[0087] 0.2 parts of antioxidant;

[0088] Light stabilizer 0.2 parts;

[0089] Silane coupling agent KH570 0.4 parts.

[0090] Wherein, the adsorbent is prepared according to the following method:

[0091] (1) Natural zeolite and europium chloride solution are mixed, potassium hydroxide is used to adjust the pH to 10, and the mixture is shaken at 35° C. and 250 r / min for 10 h. After the reaction is completed, the mixture is centrifuged and filtered to remove insoluble matter, which is washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain modified zeolite I.

[0092] Specifically, the concentration of the europium chloride solution is 2.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:40mL;

[0093] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0094] (2) adding modified zeolite I to acrylamide solution and potassium dihydrogen phosphate solution, respectively, at 25° C. and 250 r / min, shaking for 5 h, filtering, and taking insoluble matter; obtaining modified zeolite II;

[0095] Specifically, the concentration of the acrylamide solution is 120 mg / L; the concentration of the potassium dihydrogen phosphate solution is 15 mg / L; the usage ratio of the modified zeolite to the acrylamide solution and the potassium dihydrogen phosphate solution is 1.0 g: 100 mL: 100 mL;

[0096] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1:Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0097] (3) Add modified zeolite II and silane coupling agent KH570 to anhydrous ethanol, ultrasonically vibrate for 0.5 h, stand at room temperature for 2 h, react at 60° C. for 5 h, filter, take out the insoluble matter, and dry at 60° C. for 12 h to obtain modified zeolite III, i.e., adsorbent.

[0098] Specifically, the usage ratio of modified zeolite II, silane coupling agent KH570, and anhydrous ethanol is 1 g: 4.0 g: 80 mL;

[0099] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 1735cm -1 : Ester-C=O exists; 1603cm -1 、810cm -1 :-C=C- exists;

[0100] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+ The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0101] Example 2

[0102] The raw material components of the anti-PID EVA packaging film provided in this embodiment are the same as those in specific embodiment 1.

[0103] Wherein, the adsorbent is prepared according to the following method:

[0104] (1) Natural zeolite and europium chloride solution are mixed, potassium hydroxide is used to adjust the pH to 11, and the mixture is shaken at 20° C. and 250 r / min for 12 h. After the reaction is completed, the mixture is centrifuged in a centrifuge, filtered, and the insoluble matter is taken out and washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain modified zeolite I.

[0105] Specifically, the concentration of the europium chloride solution is 1.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:50mL;

[0106] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0107] (2) adding the modified zeolite I to an acrylamide solution and a potassium dihydrogen phosphate solution, respectively, at 30° C. and a rotation speed of 250 r / min, shaking for 6 h, filtering, and taking the insoluble matter; obtaining the modified zeolite II;

[0108] Specifically, the concentration of the acrylamide solution is 100 mg / L; the concentration of the potassium dihydrogen phosphate solution is 10 mg / L; the usage ratio of the modified zeolite to the acrylamide solution and the potassium dihydrogen phosphate solution is 0.6 g: 100 mL: 100 mL;

[0109] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0110] (3) Add modified zeolite II and silane coupling agent KH570 to anhydrous ethanol, ultrasonically vibrate for 0.5 h, stand at room temperature for 2 h, react at 40° C. for 12 h, filter, take out the insoluble matter, and dry at 60° C. for 12 h to obtain modified zeolite III, i.e., adsorbent.

[0111] Specifically, the usage ratio of modified zeolite II, silane coupling agent KH570, and anhydrous ethanol is 1 g: 3.0 g: 80 mL;

[0112] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 1735cm -1 : Ester-C=O exists; 1603cm -1 、810cm -1 :-C=C- exists;

[0113] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+ The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0114] Example 3

[0115] The raw material components of the anti-PID EVA packaging film provided in this embodiment are the same as those in specific embodiment 1.

[0116] Wherein, the adsorbent is prepared according to the following method:

[0117] (1) Natural zeolite and europium chloride solution are mixed, potassium hydroxide is used to adjust the pH to 9, and the mixture is shaken at 40° C. and 250 r / min for 8 h. After the reaction is completed, the mixture is centrifuged and filtered to remove insoluble matter, which is washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain modified zeolite I.

[0118] Specifically, the concentration of the europium chloride solution is 3.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:25mL;

[0119] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0120] (2) adding the modified zeolite I to an acrylamide solution and a potassium dihydrogen phosphate solution, respectively, at 30° C. and a rotation speed of 250 r / min, shaking for 4 h, filtering, and taking the insoluble matter to obtain the modified zeolite II;

[0121] Specifically, the concentration of the acrylamide solution is 150 mg / L; the concentration of the potassium dihydrogen phosphate solution is 20 mg / L; the usage ratio of the modified zeolite to the acrylamide solution and the potassium dihydrogen phosphate solution is 2.0 g: 100 mL: 100 mL;

[0122] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0123] (3) Add modified zeolite II and silane coupling agent KH570 to anhydrous ethanol, ultrasonically vibrate for 0.5 h, stand at room temperature for 2 h, react at 80° C. for 2 h, filter, take out the insoluble matter, and dry at 60° C. for 12 h to obtain modified zeolite III, i.e., adsorbent.

[0124] Specifically, the usage ratio of modified zeolite II, silane coupling agent KH570, and anhydrous ethanol is 1 g: 5.0 g: 80 mL;

[0125] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1:-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 :Silicon-oxygen tetrahedron -Si-O-Si-, aluminum-oxygen octahedron -Al-O-Si-; 1735cm -1 : Ester-C=O exists; 1603cm -1 、810cm -1 :-C=C- exists;

[0126] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+ The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0127] Example 4

[0128] The raw material components of the anti-PID EVA packaging film provided in this embodiment are the same as those in specific embodiment 1.

[0129] The preparation method of the adsorbent is the same as that of the specific embodiment 1, except that the silane coupling agent KH570 is replaced by KH171.

[0130] Example 5

[0131] The raw material components of the anti-PID EVA packaging film provided in this embodiment are the same as those in specific embodiment 1.

[0132] The preparation method of the adsorbent is the same as that of the specific embodiment 1, except that the silane coupling agent KH570 is replaced by KH590.

[0133] Example 6

[0134] The raw material components of the anti-PID EVA packaging film provided in this embodiment are the same as those in specific embodiment 1.

[0135] The preparation method of the adsorbent is the same as that of the specific embodiment 1, except that the silane coupling agent KH570 is replaced by hexadecyltrimethoxysilane.

[0136] Example 7

[0137] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0138] EVA resin 100 parts;

[0139] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0140] Triallyl isocyanurate 0.5 parts;

[0141] 0.3 parts of trimethylolpropane trimethacrylate;

[0142] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0143] Pentaerythritol triacrylate 0.4 parts;

[0144] 2.0 parts of adsorbent;

[0145] 0.2 parts of antioxidant;

[0146] Light stabilizer 0.2 parts;

[0147] Silane coupling agent KH570 0.4 parts.

[0148] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0149] Example 8

[0150] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0151] EVA resin 100 parts;

[0152] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0153] Triallyl isocyanurate 0.5 parts;

[0154] 0.3 parts of trimethylolpropane trimethacrylate;

[0155] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0156] Pentaerythritol triacrylate 0.4 parts;

[0157] Adsorbent 4.0 parts;

[0158] 0.2 parts of antioxidant;

[0159] Light stabilizer 0.2 parts;

[0160] Silane coupling agent KH570 0.4 parts.

[0161] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0162] Example 9

[0163] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0164] EVA resin 100 parts;

[0165] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0166] Triallyl isocyanurate 0.5 parts;

[0167] 0.3 parts of trimethylolpropane trimethacrylate;

[0168] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0169] Pentaerythritol triacrylate 0.4 parts;

[0170] 3.0 parts of adsorbent;

[0171] Antioxidant 0.1 part;

[0172] Light stabilizer 0.3 parts;

[0173] Silane coupling agent KH570 0.4 parts.

[0174] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0175] Example 10

[0176] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0177] EVA resin 100 parts;

[0178] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0179] Triallyl isocyanurate 0.5 parts;

[0180] 0.3 parts of trimethylolpropane trimethacrylate;

[0181] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0182] Pentaerythritol triacrylate 0.4 parts;

[0183] 3.0 parts of adsorbent;

[0184] 0.3 parts of antioxidant;

[0185] Light stabilizer 0.1 part;

[0186] Silane coupling agent KH570 0.4 parts.

[0187] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0188] Embodiment 11

[0189] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0190] EVA resin 100 parts;

[0191] 0.5 parts of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0192] Triallyl isocyanurate 0.67 parts;

[0193] 0.4 parts of trimethylolpropane trimethacrylate;

[0194] 0.4 parts of trimethylolpropane propoxide triacrylate;

[0195] Pentaerythritol triacrylate 0.53 parts;

[0196] 3.0 parts of adsorbent;

[0197] 0.2 parts of antioxidant;

[0198] Light stabilizer 0.2 parts;

[0199] Silane coupling agent KH570 0.4 parts.

[0200] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0201] Example 12

[0202] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0203] EVA resin 100 parts;

[0204] 1.5 parts of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0205] Triallyl isocyanurate 0.33 parts;

[0206] 0.2 parts of trimethylolpropane trimethacrylate;

[0207] 0.2 parts of trimethylolpropane propoxide triacrylate;

[0208] Pentaerythritol triacrylate 0.27 parts;

[0209] 3.0 parts of adsorbent;

[0210] 0.2 parts of antioxidant;

[0211] Light stabilizer 0.2 parts;

[0212] Silane coupling agent KH570 0.4 parts.

[0213] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0214] Example 13

[0215] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0216] EVA resin 100 parts;

[0217] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0218] 1.5 parts of triallyl isocyanurate;

[0219] 3.0 parts of adsorbent;

[0220] 0.2 parts of antioxidant;

[0221] Light stabilizer 0.2 parts;

[0222] Silane coupling agent KH570 0.4 parts.

[0223] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0224] Embodiment 14

[0225] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0226] EVA resin 100 parts;

[0227] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0228] 0.45 parts of trimethylolpropane trimethacrylate;

[0229] 0.45 parts of trimethylolpropane propoxide triacrylate;

[0230] Pentaerythritol triacrylate 0.6 parts;

[0231] 3.0 parts of adsorbent;

[0232] 0.2 parts of antioxidant;

[0233] Light stabilizer 0.2 parts;

[0234] Silane coupling agent KH570 0.4 parts.

[0235] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0236] Embodiment 15

[0237] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0238] EVA resin 100 parts;

[0239] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0240] Triallyl isocyanurate 0.5 parts;

[0241] 0.3 parts of trimethylolpropane trimethacrylate;

[0242] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0243] Pentaerythritol triacrylate 0.4 parts;

[0244] 3.0 parts of adsorbent;

[0245] 0.2 parts of antioxidant;

[0246] Light stabilizer 0.2 parts;

[0247] Silane coupling agent KH570 0.3 parts.

[0248] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0249] Example 16

[0250] The anti-PID EVA packaging film provided in this embodiment includes the following raw materials in parts by weight:

[0251] EVA resin 100 parts;

[0252] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0253] Triallyl isocyanurate 0.5 parts;

[0254] 0.3 parts of trimethylolpropane trimethacrylate;

[0255] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0256] Pentaerythritol triacrylate 0.4 parts;

[0257] 3.0 parts of adsorbent;

[0258] 0.2 parts of antioxidant;

[0259] Light stabilizer 0.2 parts;

[0260] Silane coupling agent KH570 0.5 parts.

[0261] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0262] The anti-PID EVA packaging films of comparative examples 1-13 were all compared with example 1.

[0263] Comparative Example 1

[0264] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0265] EVA resin 100 parts;

[0266] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0267] Triallyl isocyanurate 0.5 parts;

[0268] 0.3 parts of trimethylolpropane trimethacrylate;

[0269] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0270] Pentaerythritol triacrylate 0.4 parts;

[0271] 0.2 parts of antioxidant;

[0272] Light stabilizer 0.2 parts;

[0273] Silane coupling agent KH570 0.4 parts.

[0274] Comparative Example 2

[0275] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0276] EVA resin 100 parts;

[0277] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0278] Triallyl isocyanurate 0.5 parts;

[0279] 0.3 parts of trimethylolpropane trimethacrylate;

[0280] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0281] Pentaerythritol triacrylate 0.4 parts;

[0282] 3.0 parts of natural zeolite;

[0283] 0.2 parts of antioxidant;

[0284] Light stabilizer 0.2 parts;

[0285] Silane coupling agent KH570 0.4 parts.

[0286] Comparative Example 3

[0287] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0288] EVA resin 100 parts;

[0289] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0290] Triallyl isocyanurate 0.5 parts;

[0291] 0.3 parts of trimethylolpropane trimethacrylate;

[0292] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0293] Pentaerythritol triacrylate 0.4 parts;

[0294] 3.0 parts of adsorbent;

[0295] 0.2 parts of antioxidant;

[0296] Light stabilizer 0.2 parts;

[0297] Silane coupling agent KH570 0.4 parts.

[0298] Wherein, the adsorbent is prepared according to the following method:

[0299] Natural zeolite and europium chloride solution were mixed, potassium hydroxide was used to adjust the pH to 10, and the mixture was shaken at 35°C and 250 r / min for 10 hours. After the reaction was completed, the mixture was centrifuged and filtered to obtain insoluble matter, which was washed with deionized water until the supernatant was neutral, and dried at 60°C for 12 hours to obtain modified zeolite I, i.e., the adsorbent.

[0300] Specifically, the concentration of the europium chloride solution is 2.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:40mL;

[0301] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm-1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-;

[0302] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+ The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0303] Comparative Example 4

[0304] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0305] EVA resin 100 parts;

[0306] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0307] Triallyl isocyanurate 0.5 parts;

[0308] 0.3 parts of trimethylolpropane trimethacrylate;

[0309] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0310] Pentaerythritol triacrylate 0.4 parts;

[0311] 3.0 parts of adsorbent;

[0312] 0.2 parts of antioxidant;

[0313] Light stabilizer 0.2 parts;

[0314] Silane coupling agent KH570 0.4 parts.

[0315] Wherein, the adsorbent is prepared according to the following method:

[0316] (1) Natural zeolite and europium chloride solution are mixed, potassium hydroxide is used to adjust the pH to 10, and the mixture is shaken at 35° C. and 250 r / min for 10 h. After the reaction is completed, the mixture is centrifuged and filtered to remove insoluble matter, which is washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain modified zeolite I.

[0317] Specifically, the concentration of the europium chloride solution is 2.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:40mL;

[0318] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm-1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0319] (2) adding modified zeolite I to acrylamide solution, shaking at 25° C. and 250 r / min for 5 h, filtering, and taking insoluble matter; obtaining modified zeolite II, i.e., adsorbent;

[0320] Specifically, the concentration of the acrylamide solution is 120 mg / L; the usage ratio of the modified zeolite to the acrylamide solution is 1.0 g: 100 mL: 100 mL;

[0321] Its infrared data is as follows: 3441cm -1 、1637cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-;

[0322] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+ The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0323] Comparative Example 5

[0324] This comparative example provides an anti-PID EVA packaging film, including the following raw materials in parts by weight:

[0325] EVA resin 100 parts;

[0326] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0327] Triallyl isocyanurate 0.5 parts;

[0328] 0.3 parts of trimethylolpropane trimethacrylate;

[0329] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0330] Pentaerythritol triacrylate 0.4 parts;

[0331] 3.0 parts of adsorbent;

[0332] 0.2 parts of antioxidant;

[0333] Light stabilizer 0.2 parts;

[0334] Silane coupling agent KH570 0.4 parts.

[0335] Wherein, the adsorbent is prepared according to the following method:

[0336] (1) Natural zeolite and europium chloride solution are mixed, potassium hydroxide is used to adjust the pH to 10, and the mixture is shaken at 35° C. and 250 r / min for 10 h. After the reaction is completed, the mixture is centrifuged and filtered to remove insoluble matter, which is washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain modified zeolite I.

[0337] Specifically, the concentration of the europium chloride solution is 2.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:40mL;

[0338] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0339] (2) adding modified zeolite I to potassium dihydrogen phosphate solution, shaking at 25° C. and 250 r / min for 5 h, filtering and taking insoluble matter; obtaining modified zeolite II, i.e., adsorbent;

[0340] Specifically, the concentration of potassium dihydrogen phosphate solution is 15 mg / L; the usage ratio of modified zeolite to potassium dihydrogen phosphate solution is 1.0 g:100 mL;

[0341] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-;

[0342] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0343] Comparative Example 6

[0344] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0345] EVA resin 100 parts;

[0346] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0347] Triallyl isocyanurate 0.5 parts;

[0348] 0.3 parts of trimethylolpropane trimethacrylate;

[0349] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0350] Pentaerythritol triacrylate 0.4 parts;

[0351] 3.0 parts of adsorbent;

[0352] 0.2 parts of antioxidant;

[0353] Light stabilizer 0.2 parts;

[0354] Silane coupling agent KH570 0.4 parts.

[0355] Wherein, the adsorbent is prepared according to the following method:

[0356] (1) Natural zeolite and europium chloride solution are mixed, potassium hydroxide is used to adjust the pH to 10, and the mixture is shaken at 35° C. and 250 r / min for 10 h. After the reaction is completed, the mixture is centrifuged and filtered to remove insoluble matter, which is washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain modified zeolite I.

[0357] Specifically, the concentration of the europium chloride solution is 2.5wt%; the usage ratio of the natural zeolite to the europium chloride solution is 1g:40mL;

[0358] Its infrared data is as follows: 3441cm -1 、1637cm -1 : -OH (coordinated with europium) broad peak exists; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-.

[0359] (2) adding modified zeolite I to an acrylamide solution and a potassium dihydrogen phosphate solution, respectively, at 25° C. and a rotation speed of 250 r / min, shaking for 5 h, filtering, and taking insoluble matter; obtaining modified zeolite II, i.e., an adsorbent;

[0360] Specifically, the concentration of the acrylamide solution is 120 mg / L; the concentration of the potassium dihydrogen phosphate solution is 15 mg / L; the usage ratio of the modified zeolite to the acrylamide solution and the potassium dihydrogen phosphate solution is 1.0 g: 100 mL: 100 mL;

[0361] Its infrared data is as follows: 3442cm -1 、1640cm -1 :-OH (coordinated with europium) exists; 3312cm -1 :-NH2 sharp peak exists; 1690cm -1 :Amide-C=O exists; 1621cm -1 :-C=C- exists; 1132cm -1 :-P=O (coordinated with europium) exists; 1076cm -1 :-PO-existence; 1048cm -1 :-Si-O-Si- exists; 794cm -1 、724cm -1 : Silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-;

[0362] Fluorescence excitation emission spectrum: 590nm, 615nm for Eu 3+ The characteristic spectral line of 615nm is the strongest characteristic emission peak.

[0363] Comparative Example 7

[0364] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0365] EVA resin 100 parts;

[0366] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0367] Triallyl isocyanurate 0.5 parts;

[0368] 0.3 parts of trimethylolpropane trimethacrylate;

[0369] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0370] Pentaerythritol triacrylate 0.4 parts;

[0371] 3.0 parts of adsorbent;

[0372] 0.2 parts of antioxidant;

[0373] Light stabilizer 0.2 parts;

[0374] Silane coupling agent KH570 0.4 parts.

[0375] Wherein, the adsorbent is prepared according to the following method:

[0376] (1) acrylamide, europium chloride and potassium dihydrogen phosphate are mixed and added to deionized water, potassium hydroxide is used to adjust the pH to 10, and the mixture is shaken at 35° C. and 250 r / min for 10 h. After the reaction is completed, the mixture is centrifuged and filtered to obtain insoluble matter, which is washed with deionized water until the supernatant is neutral, and dried at 60° C. for 12 h to obtain the target product.

[0377] Specifically, the usage ratio of acrylamide, europium chloride and potassium dihydrogen phosphate is 24g:1000g:3g.

[0378] Comparative Example 8

[0379] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0380] EVA resin 100 parts;

[0381] 0.2 parts of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0382] Triallyl isocyanurate 0.5 parts;

[0383] 0.3 parts of trimethylolpropane trimethacrylate;

[0384] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0385] Pentaerythritol triacrylate 0.4 parts;

[0386] 3.0 parts of adsorbent;

[0387] 0.2 parts of antioxidant;

[0388] Light stabilizer 0.2 parts;

[0389] Silane coupling agent KH570 0.4 parts.

[0390] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0391] Comparative Example 9

[0392] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0393] EVA resin 100 parts;

[0394] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0395] Triallyl isocyanurate 0.17 parts;

[0396] 0.1 parts of trimethylolpropane trimethacrylate;

[0397] 0.1 part of trimethylolpropane propoxide triacrylate;

[0398] Pentaerythritol triacrylate 0.13 parts;

[0399] 3.0 parts of adsorbent;

[0400] 0.2 parts of antioxidant;

[0401] Light stabilizer 0.2 parts;

[0402] Silane coupling agent KH570 0.4 parts.

[0403] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0404] Comparative Example 10

[0405] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0406] EVA resin 100 parts;

[0407] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0408] Triallyl isocyanurate 0.5 parts;

[0409] 0.3 parts of trimethylolpropane trimethacrylate;

[0410] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0411] Pentaerythritol triacrylate 0.4 parts;

[0412] 3.0 parts of adsorbent;

[0413] Antioxidant 1010 0.2 parts;

[0414] Light stabilizer 0.2 parts;

[0415] Silane coupling agent KH570 0.4 parts.

[0416] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0417] Comparative Example 11

[0418] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0419] EVA resin 100 parts;

[0420] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0421] Triallyl isocyanurate 0.5 parts;

[0422] 0.3 parts of trimethylolpropane trimethacrylate;

[0423] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0424] Pentaerythritol triacrylate 0.4 parts;

[0425] 3.0 parts of adsorbent;

[0426] Antioxidant 168 0.2 parts;

[0427] Light stabilizer 0.2 parts;

[0428] Silane coupling agent KH570 0.4 parts.

[0429] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0430] Comparative Example 12

[0431] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0432] EVA resin 100 parts;

[0433] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0434] Triallyl isocyanurate 0.5 parts;

[0435] 0.3 parts of trimethylolpropane trimethacrylate;

[0436] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0437] Pentaerythritol triacrylate 0.4 parts;

[0438] 3.0 parts of adsorbent;

[0439] 0.2 parts of antioxidant;

[0440] UV-292 0.2 parts;

[0441] Silane coupling agent KH570 0.4 parts.

[0442] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0443] Comparative Example 13

[0444] The anti-PID EVA packaging film provided in this comparative example includes the following raw materials in parts by weight:

[0445] EVA resin 100 parts;

[0446] 1.0 part of 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane;

[0447] Triallyl isocyanurate 0.5 parts;

[0448] 0.3 parts of trimethylolpropane trimethacrylate;

[0449] 0.3 parts of trimethylolpropane propoxide triacrylate;

[0450] Pentaerythritol triacrylate 0.4 parts;

[0451] 3.0 parts of adsorbent;

[0452] 0.2 parts of antioxidant;

[0453] UV-531 0.2 parts;

[0454] Silane coupling agent KH570 0.4 parts.

[0455] Wherein, the preparation method of the adsorbent is the same as that in specific embodiment 1.

[0456] According to the formula amount, the physical properties of the anti-PID EVA encapsulation films prepared in Examples 1-16 and Comparative Examples 1-13 of the present invention were tested. The specific testing method is as follows:

[0457] (1) Free acid content: The ratio of the peak area of ​​the carbonyl group to the carboxyl group is measured by ATR, P = A2 (1760 cm -1 :-C=O free acetic acid) / A1(1760cm -1 :-C=O free acetic acid); "A1" represents before aging test; "A2" represents after aging test. Aging conditions are: +85℃, relative humidity 85%, and test time is 720hr.

[0458] (2) Cross-linking degree: After the EVA film undergoes cross-linking reaction, the cross-linking degree is determined by xylene extraction. The EVA film is cut into 1 mm pieces, weighed as m0, and placed in a stainless steel mesh bag. It is immersed in boiling xylene and extracted for 4 hours. The uncross-linked EVA will be extracted into the xylene, and the remaining undissolved EVA is the cross-linked EVA film m1.

[0459] Crosslinking degree = crosslinked EVA film m1 / EVA total weight m0×100%.

[0460] (3) Resistance to humidity and heat aging: The EVA film was subjected to a humidity and heat aging test. Conditions: Test conditions: +85°C, relative humidity 85%, test time 1000 hours.

[0461] The visible light transmittance before and after the test was measured, and the visible light transmittance retention rate was calculated according to the following formula:

[0462] Retention rate of visible light transmittance=average light transmittance after the test / average light transmittance before the test×100%.

[0463] The yellowing index (△YI) before and after the test was measured according to GB 2409.

[0464] (4) UV aging resistance: The obtained EVA film was subjected to UV irradiation aging test according to the requirements of the International Electrotechnical Commission standard IEC61345. Test conditions: the surface temperature of the test piece is 60±5℃, the UV wavelength range is 280-400nm, and the irradiation intensity is 15kW·h / m 2 , the UV irradiation test time is 2000hr.

[0465] The visible light transmittance before and after the test was measured, and the visible light transmittance retention rate was calculated according to the following formula:

[0466] Retention rate of visible light transmittance=average light transmittance after the test / average light transmittance before the test×100%.

[0467] The yellowing index (△YI) before and after the test was measured according to GB 2409.

[0468] (5) Photoelectric conversion power gain: Measured using an EL tester. Stack the photovoltaic glass, film, cell, film and photovoltaic backplane neatly from top to bottom, laminate at 140°C for 15 minutes, take out and cool, first test the bare chip power and record it as P 0.1 ; The power of the component obtained by laminating the EVA film without adding adsorbent is tested and recorded as P1; the power of the new bare chip is tested and recorded as P 0.2 , the EVA film of the present invention is used for lamination, and its power is tested and recorded as P2, then the power gain P m=(P2 / P 0.2 ) / (P1 / P 0.1 ).

[0469] (6) PID power attenuation: The PID of the photovoltaic module is tested according to the industry standard IEC-62804. The test conditions are: 1000V voltage, 85°C, 85% relative humidity, and 192h.

[0470] The test results are shown in Table 1:

[0471] Table 1

[0472]

[0473] First, it can be concluded from Examples 1-16 in Table 1 that the anti-PID EVA encapsulation film of the present invention has obvious advantages in adsorbing free acetic acid and resisting PID, and also has advantages in anti-oxidation, anti-yellowing and photoelectric conversion efficiency.

[0474] Second, it can be observed from Example 1 and Comparative Examples 1-6 that the EVA film of the present invention uses a self-made adsorbent with excellent free acetic acid adsorption, i.e., anti-PID and other properties. It can be observed from Example 1 and Comparative Examples 1-5 that the self-made adsorbent of the present invention is based on zeolite, and the porous structure of zeolite has excellent free acid adsorption; it can also be observed that the presence of amine source also plays an important role in the adsorption of free acid; in addition, the presence of rare earth, i.e., phosphate, has a positive effect on improving the anti-PID performance; it can be observed from Example 1 and Comparative Example 5 that the dispersibility of modified zeolite has an important influence on the performance of the most red.

[0475] Third, it can be observed from Example 1 and Comparative Example 7 that the high specific surface area formed by the porous structure of zeolite has a synergistic effect.

[0476] Fourth, it can be observed from Example 1 and Comparative Examples 8-13 that, through formulation optimization, reasonable crosslinking density, the ratio and dosage of antioxidants and light stabilizers have a positive effect on improving the performance of the product.

[0477] In summary, the anti-PID EVA encapsulation film of the present invention has excellent acid removal, anti-PID performance and excellent resistance to light, heat and oxygen aging through the synergistic effect of the homemade adsorbent and other components, while also being able to effectively improve the photoelectric conversion efficiency.

[0478] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. Anti-PID EVA packaging film, characterized in that: The invention comprises the following raw materials in parts by weight: EVA resin 100 parts; Cross-linking agent 0.5-1.5 parts; 1.0-2.0 parts of auxiliary cross-linking agent; Adsorbent 2.0-4.0 parts; Antioxidant 0.1-0.3 parts; Light stabilizer 0.1-0.3 parts; Coupling agent 0.3-0.5 parts; The adsorbent is prepared according to the following method: (1) zeolite and rare earth metal solution are subjected to ion exchange reaction under alkaline conditions to obtain modified zeolite I; (2) placing the modified zeolite I in an amine solution and then a phosphate solution to obtain a modified zeolite II; (3) placing the modified zeolite II and the silane coupling agent in an alcohol solvent for silylation coupling reaction to obtain the modified zeolite III, i.e., the adsorbent; The rare earth metal solution is a lanthanide metal aqueous solution; the concentration is 1.5-3.5wt%; The dosage ratio of the zeolite to the rare earth metal solution is 1g:25-50mL.

2. The anti-PID EVA packaging film according to claim 1, characterized in that: The concentration of the amine solution is 100-150 mg / L; the concentration of the phosphate solution is 10-20 mg / L.

3. The anti-PID EVA packaging film according to claim 1, characterized in that: The usage ratio of the modified zeolite to the amine solution and the phosphate solution is 0.6-2.0 g:100 mL:100 mL.

4. The anti-PID EVA packaging film according to claim 1, characterized in that: The silane coupling agent is selected from one or more of a mercaptosilane coupling agent, a vinylsilane coupling agent, an acryloxysilane coupling agent or a long-chain hydrocarbon silane coupling agent.

5. The anti-PID EVA packaging film according to claim 1, characterized in that: The usage ratio of the modified zeolite II, the silane coupling agent and the alcohol solvent is 1g:3.0-5.0g:80mL.

6. The anti-PID EVA packaging film according to claim 1, characterized in that: The crosslinking agent is an organic peroxide crosslinking agent; the auxiliary crosslinking agent is an allyl type and / or an acryloxy type; the antioxidant is a hindered phenol and phosphite type compound antioxidant; and the light stabilizer is a hindered amine and benzophenone type compound light stabilizer.

7. The method for preparing the anti-PID EVA packaging film according to any one of claims 1 to 6, characterized in that: The steps include: S1: Mixing: Mixing the raw materials according to the formula ratio to obtain a mixed raw material; S2: Extrusion: melt blending, extrusion, casting, and cooling the mixed raw materials in step S1 in sequence to obtain an intermediate product; S3: Film formation: The intermediate product in step S2 is subjected to thickness measurement, edge pressing, shaping, edge cutting and winding to obtain the PIDEVA-resistant packaging film.

Citation Information

Patent Citations

  • Fluorine compound-modified ethylene-vinyl acetate (EVA) packaging film and preparation method thereof

    CN103756578A

  • EVA composite adhesive film used for photovoltaic packaging and having anti-PID performance

    CN105820764A

  • Water-blocking packaging adhesive film and preparation method thereof

    CN112920722A

  • Heat-conducting composite EVA photovoltaic packaging adhesive film and preparation method thereof

    CN117467365A

  • Composite photovoltaic cell packaging adhesive film material and preparation method thereof

    CN117625069A