Iridium single atom / iridium nanocluster anchored CoMoO4 material and its preparation method and application
By preparing iridium single atoms/iridium nanoclusters to anchor CoMoO4 materials, the problems of high cost and insufficient activity of noble metal catalysts are solved, efficient electrocatalytic water splitting is achieved, and low-cost commercial hydrogen energy application prospects are provided.
Patent Information
- Application Number
- CN202410574823.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-05-10
AI Technical Summary
In the existing electrocatalytic water splitting technology, the scarcity and high cost of precious metal catalysts hinder its large-scale application in commercial electrolyzers, and research mainly focuses on single-functional catalysts, which increases the cost and cost of assembling total water splitting electrolyzers. Complexity.
The iridium single atom/iridium nanocluster-anchored CoMoO4 material was prepared through hydrothermal and low-temperature thermal reduction processes, achieving low Ir noble metal loading and high atomic utilization. The strong coupling of Ir metal sites and CoMoO4 improved the electrocatalytic performance.
A bifunctional electrocatalyst with high activity, high stability and low precious metal loading was obtained, which significantly improved the hydrogen evolution and oxygen evolution performance in electrocatalytic water splitting, reduced the overvoltage required for the reaction, and was superior to commercial IrO2 and Pt/ C catalyst.
Smart Images

Figure CN118142548B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functionalized materials and electrocatalytic water decomposition, and in particular to an iridium single atom / iridium nanocluster anchored CoMoO4 material and a preparation method and application thereof. Background Art
[0002] Electrocatalytic water splitting technology represented by proton exchange membrane produces hydrogen energy with high energy density, high purity, green and sustainable, providing an ideal solution to the current energy shortage and environmental pollution problems. Electrocatalytic water splitting is divided into anode oxygen evolution reaction (OER) and cathode hydrogen evolution reaction (HER), and the kinetics of OER and HER determine the efficiency of hydrogen production. At present, the water splitting catalysts with the best catalytic activity are still precious metal catalysts such as Pt / C, IrO2, and RuO2, but the scarcity and high cost of these materials seriously hinder their large-scale application in commercial electrolyzers. In addition, most studies focus on monofunctional catalysts (HER or OER catalysts), which increases the cost and complexity of assembling commercial full water splitting electrolyzers. Therefore, it is urgent to reduce the loading of precious metals and design a bifunctional electrocatalyst. Metal oxides can provide abundant anchoring sites for highly active precious metal sites, and there will be strong interactions between the oxide matrix and the precious metals, which improves the electronic structure of the material and optimizes the kinetics of oxygen and hydrogen evolution reactions. Summary of the invention
[0003] In order to solve the above problems, the purpose of the present invention is to provide an iridium single atom / iridium nanocluster anchored CoMoO4 material and its preparation method and application. The present invention successfully prepares an iridium single atom / iridium nanocluster anchored CoMoO4 material through a simple hydrothermal and low-temperature thermal reduction process. The low Ir noble metal loading and the obtained Ir single atom / Ir nanocluster achieve ultra-high atomic utilization, and the strong coupling between the Ir metal site and CoMoO4 effectively improves the electrocatalytic performance; it can improve the high cost of noble metal catalysts, low atomic utilization and insufficient intrinsic activity of single metal active sites, reduce the noble metal coating and increase the catalytic activity.
[0004] In order to achieve the above object, the present invention discloses a method for preparing an iridium single atom / iridium nanocluster anchored CoMoO4 material, comprising the following steps:
[0005] (1) Dissolve cobalt salt in deionized water to obtain solution A; dissolve molybdenum salt in deionized water to obtain solution B; dissolve anhydrous sodium acetate in deionized water to obtain solution C; drop solution B and solution C into solution A respectively, stir evenly, and obtain a uniform pink solution D; then add iridium source to solution D, stir and react at room temperature for a certain time, and after the reaction is completed, obtain a mixed solution E for standby use;
[0006] (2) Soaking the nickel foam in hydrochloric acid, then washing it in deionized water and anhydrous ethanol alternately with ultrasonic for multiple times, drying it at room temperature, and setting it aside;
[0007] (3) placing the nickel foam treated in step (2) into the mixed solution E obtained in step (1), and transferring the mixture to a reaction kettle lined with polytetrafluoroethylene, placing the reaction kettle in a forced air drying oven, heating it to a certain temperature, and performing a hydrothermal reaction at the temperature; washing the product obtained after the reaction, and then vacuum drying it to obtain an off-white sample;
[0008] (4) The off-white sample obtained in step (3) is placed in a tube furnace and calcined at low temperature under a reducing atmosphere to obtain an iridium single atom / iridium nanocluster anchored CoMoO4 material.
[0009] Furthermore, in step (1), the cobalt salt is cobalt nitrate hexahydrate (Co(NO3)2•6H2O), the molybdenum salt is sodium molybdate dihydrate (Na2MoO4•2H2O), and the iridium source is iridium trichloride (IrCl3).
[0010] Furthermore, in step (1), the amount of the cobalt salt is 0.1-1 mmol; the amount of the molybdenum salt is 0.1-1 mmol; the amount of anhydrous sodium acetate is 1-10 mmol; and the amount of the iridium source is 0.005-0.05 mmol.
[0011] Furthermore, in step (1), the volumes of deionized water in solution A, solution B, and solution C are 5 to 15 mL, respectively, and the sum of the volumes of solution A, solution B, and solution C is 30 mL.
[0012] Furthermore, in step (1), the molar ratio of the cobalt salt, the molybdenum salt and the anhydrous sodium acetate is 1:1:2-10.
[0013] Furthermore, in step (1), the stirring reaction time is 2 to 6 h.
[0014] Furthermore, in step (2), the size of the nickel foam is 1 cm×3 cm×1 cm, the pore size is 230 nm, the hydrochloric acid concentration is 2-6 mol / L, and the immersion time is 15-30 min.
[0015] Furthermore, in step (3), the temperature of the hydrothermal reaction is 150-200°C, and the hydrothermal reaction time is 8-24h;
[0016] Furthermore, in step (3), the product obtained after the reaction is rinsed with deionized water for 3 to 6 times, the vacuum drying temperature is 50 to 80 °C, and the drying time is 5 to 12 h;
[0017] Furthermore, in step (4), the reducing atmosphere is a H2 / N2 or H2 / Ar mixed gas with a hydrogen gas volume fraction of 5% to 100%, and the gas flow rate is 3 to 30 mL / min; the calcination temperature is 300 to 500 °C, the heating rate is 2 to 8 °C / min, and the insulation time is 2 to 5 h; after the calcination is completed, the iridium single atom / iridium nanocluster anchored CoMoO4 material is obtained after natural cooling.
[0018] The present invention also aims to provide an iridium single atom / iridium nanocluster anchored CoMoO4 material prepared according to the above method and the use of the iridium single atom / iridium nanocluster anchored CoMoO4 material in electrocatalytic water splitting.
[0019] Furthermore, the iridium single atom / iridium nanocluster anchored CoMoO4 material is a nanosheet structure, and the Ir single atom and the Ir nanocluster are jointly anchored on the CoMoO4 surface.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention utilizes the unique sheet structure and surface characteristics of CoMoO4 nanosheets to obtain highly dispersed Ir single atoms / Ir nanoclusters, greatly improving the utilization rate of metal atoms and obtaining excellent electrocatalytic hydrogen evolution (HER) and oxygen evolution (OER) performance. The CoMoO4 carrier not only effectively disperses and stabilizes the Ir metal sites, but also interacts strongly with the Ir single atoms / Ir nanoclusters, which improves the electronic structure of the material and promotes the kinetics of hydrogen and oxygen evolution. In addition, the unique nanosheet structure of CoMoO4 optimizes the hydrophilicity and gas repellency of the material, accelerates the precipitation of bubbles during the reaction, and avoids the poisoning phenomenon caused by the long-term occupation of active sites by bubbles. Based on this, the current density of the catalyst in the OER reaction reaches 20 mA / cm 2 When the overvoltage is only 251 mV, it is significantly improved compared with commercial IrO2 catalysts. In HER, the current density reaches 10 mA / cm 2 When the overvoltage is 30 mV, it is comparable to the activity of commercial Pt / C catalysts. Importantly, the OER and HER activities of the catalyst proposed in the present invention surpass those of most electrocatalysts in this field under alkaline conditions, showing good prospects for industrial application.
[0022] (2) The present invention prepares a bifunctional electrocatalyst with high activity, high stability and low precious metal loading, which can realize low-cost commercial hydrogen energy applications. The Ir single atoms and Ir nanoclusters supported by CoMoO4 nanosheets greatly improve the utilization of active sites, and the strong interaction between Ir sites and CoMoO4 significantly enhances the hydrogen and oxygen evolution activities in electrocatalytic water splitting. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The XRD pattern of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0024] Figure 2 This is a SEM image of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0025] Figure 3 TEM image of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0026] Figure 4 This is a spherical aberration corrected TEM image of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0027] Figure 5 This is the XPS spectrum of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0028] Figure 6 The OER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0029] Figure 7 HER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1;
[0030] Figure 8 This is the OER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 2;
[0031] Fig. 9 HER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 2;
[0032] Fig.10 This is the OER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 3;
[0033] Fig.11 This is the HER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 3. DETAILED DESCRIPTION
[0034] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. The following embodiments are implemented based on the technology of the present invention, and detailed implementation methods and operating steps are given, but the protection scope of the present invention is not limited to the following embodiments.
[0035] Embodiment 1:
[0036] (1) Take 3 portions of deionized water, each with a volume of 10 mL, dissolve 0.3 mmol of Co(NO3)2•6H2O in one portion of deionized water to obtain solution A; dissolve 0.3 mmol of Na2MoO4•2H2O in another portion of deionized water to obtain solution B; dissolve 3 mmol of anhydrous sodium acetate in the last portion of deionized water to obtain solution C; then drop solution B and solution C into solution A respectively, stir evenly to obtain a uniform pink solution D, add 0.0178 mmol of IrCl3 to solution D, and stir at room temperature for 3 h. After the reaction is completed, a light yellow mixed solution E is obtained for use;
[0037] (2) Place nickel foam with a size of 1 cm × 3 cm × 1 cm and a pore size of about 230 nm in a 3 mol / L hydrochloric acid solution and soak for 25 min. Then, alternately ultrasonically wash it in deionized water and anhydrous ethanol for 3 times, each ultrasonic time for 5 minutes. Finally, dry it at room temperature and set aside.
[0038] (3) The nickel foam treated in step (2) is placed in the mixed solution E obtained in step (1), and the mixture is transferred together to a reaction kettle lined with polytetrafluoroethylene. The reaction kettle is placed in a forced air drying oven and heated to 180°C, and subjected to a hydrothermal reaction at this temperature for 12 h. The product obtained after the reaction is rinsed with deionized water three times to remove residual solvent and reactants, and then vacuum dried at 60°C for 10 h to obtain an off-white sample.
[0039] (4) The off-white sample obtained in step (3) was placed in a tubular furnace, and a H2 / Ar mixed atmosphere with a H2 volume fraction of 10% was used as a reducing atmosphere. The flow rate of the H2 / Ar mixed atmosphere was 12 mL / min, and the mixture was heated to 400°C at a heating rate of 5°C / min. The mixture was kept at 400°C for 2 h, and after natural cooling, an iridium single atom / iridium nanocluster anchored CoMoO4 material was obtained, which was recorded as Ir-CoMoO4.
[0040] Embodiment 2:
[0041] (1) Take 3 portions of deionized water, each with a volume of 10 mL, dissolve 0.3 mmol of Co(NO3)2•6H2O in one portion of deionized water to obtain solution A; dissolve 0.3 mmol of Na2MoO4•2H2O in another portion of deionized water to obtain solution B; dissolve 3 mmol of anhydrous sodium acetate in the last portion of deionized water to obtain solution C; then drop solution B and solution C into solution A respectively, stir evenly to obtain a uniform pink solution D, add 0.0089 mmol of IrCl3 to solution D, and stir at room temperature for 3 h. After the reaction is completed, a light yellow mixed solution E is obtained for use;
[0042] (2) Place nickel foam with a size of 1 cm × 3 cm × 1 cm and a pore size of about 230 nm in a 3 mol / L hydrochloric acid solution and soak for 25 min. Then, alternately ultrasonically wash it in deionized water and anhydrous ethanol for 3 times, each ultrasonic time for 5 minutes. Finally, dry it at room temperature and set aside.
[0043] (3) The nickel foam treated in step (2) is placed in the mixed solution E obtained in step (1), and the mixture is transferred together to a reactor lined with polytetrafluoroethylene. The reactor is placed in a forced air drying oven and heated to 180°C, and subjected to a hydrothermal reaction at this temperature for 24 hours. The product obtained after the reaction is rinsed with deionized water three times to remove residual solvent and reactants, and then vacuum dried at 60°C for 10 hours to obtain an off-white sample.
[0044] (4) The off-white sample obtained in step (3) was placed in a tubular furnace, and a H2 / Ar mixed atmosphere with a H2 volume fraction of 10% was used as a reducing atmosphere. The flow rate of the H2 / Ar mixed atmosphere was 12 mL / min, and the mixture was heated to 400°C at a heating rate of 5°C / min. The mixture was kept at 400°C for 2 h, and after natural cooling, an iridium single atom / iridium nanocluster anchored CoMoO4 material was obtained, which was recorded as Ir-CoMoO4-2.
[0045] Embodiment 3:
[0046] (1) Take 3 portions of deionized water, each with a volume of 10 mL, dissolve 0.3 mmol of Co(NO3)2•6H2O in one portion of deionized water to obtain solution A; dissolve 0.3 mmol of Na2MoO4•2H2O in another portion of deionized water to obtain solution B; dissolve 3 mmol of anhydrous sodium acetate in the last portion of deionized water to obtain solution C; then drop solution B and solution C into solution A respectively, stir evenly to obtain a uniform pink solution D, add 0.0356 mmol of IrCl3 to solution D, and stir at room temperature for 3 h. After the reaction is completed, a yellow mixed solution E is obtained for use;
[0047] (2) Place nickel foam with a size of 1 cm × 3 cm × 1 cm and a pore size of about 230 nm in a 3 mol / L hydrochloric acid solution and soak for 25 min. Then, alternately ultrasonically wash it in deionized water and anhydrous ethanol for 3 times, each ultrasonic time for 5 minutes. Finally, dry it at room temperature and set aside.
[0048] (3) The nickel foam treated in step (2) is placed in the mixed solution E obtained in step (1), and the mixture is transferred together to a reaction kettle lined with polytetrafluoroethylene. The reaction kettle is placed in a forced air drying oven and heated to 200°C, and subjected to a hydrothermal reaction at this temperature for 8 h. The product obtained after the reaction is rinsed with deionized water for 3 times to remove residual solvent and reactants, and then vacuum dried at 60°C for 10 h to obtain an off-white sample.
[0049] (4) The off-white sample obtained in step (3) was placed in a tubular furnace, and a H2 / Ar mixed atmosphere with a H2 volume fraction of 10% was used as a reducing atmosphere. The flow rate of the H2 / Ar mixed atmosphere was 12 mL / min, and the mixture was heated to 400°C at a heating rate of 5°C / min. The mixture was kept at 400°C for 2 h, and after natural cooling, an iridium single atom / iridium nanocluster anchored CoMoO4 material was obtained, which was recorded as Ir-CoMoO4-3.
[0050] The phase composition and crystal structure of the sample obtained in Example 1 were analyzed using Rigaku SmartLab SE type X-ray diffraction. Figure 1 The signal peak of CoMoO4 is shown, but no Ir-related peak is found, which reveals that iridium may exist in the form of single atoms or small-sized nanoclusters at the atomic level.
[0051] SEM testing was performed using a ZEISS Gemini 300 field emission scanning electron microscope. Some samples obtained in Example 1 were cut and prepared for SEM testing after gold spraying. Figure 2It shows that the sample has a perfect nanosheet structure, which optimizes the hydrophilicity and gas repellency of the material and promotes the diffusion of ions and the precipitation of bubbles during the reaction.
[0052] The TEM test was performed using JEM 2100F to further analyze the microstructure of the catalyst. Figure 3 The lamellar structure of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1 was verified again.
[0053] Aberration-corrected TEM was performed using a Thermo Themis Z to reveal the existence form of Ir. Figure 4 It is proved that there are Ir single atoms and Ir nanoclusters in the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1, and the Ir single atoms and Ir nanoclusters are jointly anchored on the CoMoO4 surface.
[0054] XPS (Thermo Scientific ESCALAB Xi+) was used to analyze the valence of the Ir element in the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1. Figure 5 It is shown that Ir has 0-valent, 3-valent and 4-valent states, which verifies the existence of Ir single atoms / Ir nanoclusters.
[0055] An electrochemical workstation (CHI760E, Shanghai Chenhua Instrument Co. Ltd.) was used to carry out polarization curve (LSV) tests of OER and HER. The polarization curve tests were all carried out in 1 mol / L KOH solution with a test scan rate of 5 mV / s. The difference was that the HER scan range was -0.85~-1.4 V (vs. MMO) and the OER scan range was 0~0.9 V (vs. MMO).
[0056] Figure 6 This is the OER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1. Figure 6 The results show that the OER performance of Ir-CoMoO4 is significantly better than that of commercial IrO2 catalyst, with a current density of 20 mA / cm 2 When the overvoltage is only 251 mV,
[0057] Figure 7 HER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 1, Figure 7 It is revealed that Ir-CoMoO4 has comparable HER activity to commercial Pt / C at a current density of 10 mA / cm 2The overvoltage is only 30mV. The excellent catalytic activity mainly comes from the strong interaction between the highly dispersed Ir single atoms / Ir nanoclusters and the CoMoO4 substrate, which optimizes the electronic structure of the material, promotes the adsorption and desorption of the reaction intermediates on the active sites, and significantly reduces the energy barrier required for the reaction. Secondly, the unique nanosheet structure of CoMoO4 promotes the mass transfer process and bubble precipitation during the reaction, accelerating the reaction kinetics.
[0058] Figure 8 This is the OER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 2. Fig. 9 HER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 2; Figure 8 , 9 It can be seen that the current density reaches 20 mA / cm 2 When the OER overvoltage of Ir-CoMoO4-2 is 267 mV, the HER reaction can overcome the 10 mA / cm 2 The overvoltage required for the current density is 32 mV, showing electrochemical performance similar to that of Ir-CoMoO4 obtained in Example 1.
[0059] Fig.10 This is the OER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 3; Fig.11 HER polarization curve of the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 3; Fig.10 and Fig.11 The current density was 20 mA / cm 2 The OER overpotential is 287 mV and the current density is 10 mA / cm 2 The HER overvoltage is 29 mV, which proves that the iridium single atom / iridium nanocluster anchored CoMoO4 material prepared in Example 3 also has excellent HER and OER performance.
[0060] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. An iridium single atom / iridium nanocluster anchoring CoMoO 4 Methods of preparing materials, Features The specific steps include: (1) Dissolve cobalt salt, molybdenum salt and anhydrous sodium acetate in deionized water to obtain solution A, solution B and solution C respectively; drop solution B and solution C into solution A respectively, stir evenly to obtain a uniform pink solution D; then add iridium source to solution D, stir and react at room temperature for a certain time, and after the reaction is completed, obtain a mixed solution E for standby use; (2) Soaking the nickel foam in hydrochloric acid, then washing it in deionized water and anhydrous ethanol alternately with ultrasonic for multiple times, drying it at room temperature, and setting it aside; (3) placing the nickel foam treated in step (2) into the mixed solution E obtained in step (1), and transferring the mixture to a reaction kettle lined with polytetrafluoroethylene, placing the reaction kettle in a forced air drying oven, heating it to a certain temperature, and performing a hydrothermal reaction at the temperature; washing the product obtained after the reaction, and then vacuum drying it to obtain an off-white sample; (4) The off-white sample obtained in step (3) is placed in a tube furnace and calcined at low temperature under a reducing atmosphere to obtain iridium single atom / iridium nanocluster anchored CoMoO 4 Material; In step (1), the amount of the cobalt salt is 0.1-1 mmol; the amount of the molybdenum salt is 0.1-1 mmol; the amount of the anhydrous sodium acetate is 1-10 mmol; the amount of the iridium source is 0.005-0.0356 mmol; the molar ratio of the cobalt salt, the molybdenum salt and the anhydrous sodium acetate is 1:1:2-10; the volume of deionized water in the solution A, solution B and solution C is 5-15 mL respectively, and the sum of the volumes of solution A, solution B and solution C is 30 mL; In step (3), the temperature of the hydrothermal reaction is 150-200 °C, and the hydrothermal reaction time is 8-24 h; In step (4), the calcination temperature is 300-500°C, the heating rate is 2-8°C / min, and the holding time is 2-5 h. After the calcination is completed, the iridium single atom / iridium nanocluster anchored CoMoO is obtained after natural cooling. 4 Material.
2. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 1 4 Methods of preparing materials, Features: In step (1), the cobalt salt is cobalt nitrate hexahydrate, the molybdenum salt is sodium molybdate dihydrate, and the iridium source is iridium trichloride.
3. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 1 4 Methods of preparing materials, Features: In step (1), the stirring reaction time is 2 to 6 h.
4. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 1 4 Methods of preparing materials, Features: In step (2), the size of the nickel foam is 1 cm×3 cm×1 cm, the pore size is 230 nm, the hydrochloric acid concentration is 2-6 mol / L, and the immersion time is 15-30 min.
5. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 1 4 Methods of preparing materials, Features: In step (3), the product obtained after the reaction is rinsed with deionized water for 3 to 6 times, the vacuum drying temperature is 50 to 80 °C, and the drying time is 5 to 12 h.
6. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 1 4 Methods of preparing materials, Features: In step (4), the reducing atmosphere is a hydrogen gas with a volume fraction of 5% to 100% H 2 / N 2 or H 2 / Ar mixed gas, the gas flow rate is 3~30 mL / min.
7. Iridium single atom / iridium nanocluster anchored CoMoO prepared by the preparation method according to any one of claims 1 to 6 4 Material.
8. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 7 4 Material, Features: The material is a nanosheet structure, with Ir single atoms and Ir nanoclusters anchored on CoMoO 4 surface.
9. The iridium single atom / iridium nanocluster anchored CoMoO as claimed in claim 7 4 Application of materials in electrocatalytic water splitting.
Citation Information
Patent Citations
Preparation method of graphene iridium nanometer conductive catalytic film
CN103147051A
Cobalt-molybdenum composite metal multifunctional carbon-based catalyst, and preparation method and application thereof
CN106475113A
Preparation method and application of core-shell-structured nickel molybdate / manganese dioxide composite material
CN106683896A
Preparation method and application of core-shell structured cobalt molybdate@ nickel cobaltate material
CN107068420A
Preparation method of cobalt molybdate hollow microsphere electrocatalyst
CN109012683A