A method for preparing precipitated hydrated white carbon black based on the production of silicon slag from anhydrous hydrogen fluoride
By beating, filtration, rinsing and grading reactions of the silicon slag produced in the anhydrous hydrogen fluoride production process, high-quality precipitated hydrated white carbon black was prepared, solving the problems of toxic gases and wastewater during the silicon slag treatment process, and realizing the Reuse of resources and reduction of costs.
Patent Information
- Application Number
- CN202410477503.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-19
AI Technical Summary
In the sulfuric acid decomposition method of anhydrous hydrogen fluoride, toxic gases and wastewater are generated during the treatment of silicon slag, resulting in high treatment costs and waste of resources.
Silicon standards-based slurry is prepared by precision filtration, rinsing, staging reaction and drying to prepare precipitated hydrated white carbon black to achieve harmless treatment and reuse of silicon slag.
The quality stability of precipitated hydrated white carbon black is improved, the treatment cost is reduced, the emission of toxic gases is avoided, and the utilization rate of raw materials is improved.
Smart Images

Figure CN118183631B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of harmless disposal and resource recovery of fluorine-containing industrial hazardous wastes, and in particular to a method for preparing precipitated hydrated white carbon black based on waste residues from anhydrous hydrogen fluoride production. Background Art
[0002] White carbon black, also known as precipitated silica or hydrated silica, is a colorless and odorless powder with excellent chemical stability and electrical insulation, as well as high specific surface area and adsorption properties. As an important raw material for the production of chemical products, white carbon black is usually used as a filler, thickener and brightener, and is widely used in rubber, plastics, ceramics, coatings, food and other fields.
[0003] Commonly used methods for synthesizing white carbon black include gas phase method and precipitation method. Among them, the precipitation method has attracted wide attention due to its significant cost advantage. The precipitation method is also called sodium silicate acidification method, which uses water glass solution to react with acid, and then precipitates, filters, washes, dries and calcines to produce white carbon black. According to different production processes, the precipitation method can be divided into carbonization method, sol method and acid method. The carbonization method is to pass carbon dioxide into a soluble silicate solution for carbonization operation to form precipitated hydrated white carbon black and sodium carbonate. This process has a large loss of sodium silicate and a low conversion rate; the sol method is to first react hydrochloric acid with sodium silicate to form a dilute sol of a certain concentration, and then add the dilute sodium silicate solution to the prepared sol under slight heating and stirring, and at the same time add a certain amount of sodium chloride solution, and form precipitated hydrated white carbon black by adjusting the pH value and keeping warm for aging. Although this process can produce relatively fine activated white carbon black, the process flow is long, the reaction process is complicated, and the conditions for preparing the sol are harsh; the acid method is to react soluble silicate with sulfuric acid (or other acids) together, stop the reaction after reaching a certain pH value, and then age. This process first converts the soluble silicate into monomer silicic acid, which is prone to aggregation or gelation, producing flocs or dense colloid particles, and the product differences are large.
[0004] Anhydrous hydrogen fluoride (AHF), as the most basic chemical raw material in the fluorine chemical industry, is widely used in the fields of chemical industry, electronics, metallurgy and atomic energy. The preparation processes of anhydrous hydrogen fluoride mainly include the fluorite method and the fluorosilicic acid method. The fluorite method uses a rotary kiln to prepare anhydrous hydrogen fluoride. This process has constraints such as low heat transfer and mass transfer efficiency and the difficulty in applying low-grade fluorite powder. The fluorosilicic acid method is divided into a direct method and an indirect method. The direct method is to directly pyrolyze fluorosilicic acid or decompose it with concentrated sulfuric acid (i.e., sulfuric acid decomposition method) to prepare anhydrous hydrogen fluoride; the indirect method is to first convert fluorosilicic acid into fluoride-containing salts such as calcium fluoride, calcium fluorosilicate, sodium fluorosilicate, magnesium fluorosilicate, potassium / sodium hydrogen fluoride and ammonium fluoride, and then pyrolyze the fluoride-containing salt or decompose it with concentrated sulfuric acid to prepare anhydrous hydrogen fluoride. At present, the sulfuric acid decomposition method has become the most mature method for preparing anhydrous hydrogen fluoride in industry due to its simple process and easy separation of products.
[0005] The main reactions involved in the sulfuric acid decomposition method are: (1) H2SiF6+H2SO4(concentrated)→SiF4↑+2HF↑+H2SO4(dilute); (2) 3SiF4+2H2O→2H2SiF6+SiO2↓; (3) SiO2+4HF→SiF4↑+2H2O. This method first utilizes the reaction between fluorosilicic acid and concentrated sulfuric acid to generate SiF4 and HF, then absorbs SiF4 with water to generate fluorosilicic acid and silicon slag, where fluorosilicic acid can react with concentrated sulfuric acid again to prepare HF. After the silicon slag is discharged from the system, it needs to consume HF for treatment, which not only reduces the yield of HF and increases the treatment cost, but also produces toxic gases such as SiF4 and a large amount of wastewater. Summary of the invention
[0006] Aiming at the technical problems that in the prior art, silicon slag produced in the process of preparing anhydrous hydrogen fluoride by sulfuric acid decomposition method using fluorosilicic acid as raw material generates toxic gas and wastewater during the treatment process and has high treatment cost, the present invention provides a method for preparing precipitated hydrated silica based on silicon slag produced by anhydrous hydrogen fluoride. The silicon slag produced in the process of anhydrous hydrogen fluoride production is used to prepare precipitated hydrated silica, thereby realizing harmless treatment and reuse of the silicon slag and improving the quality stability of the precipitated hydrated silica.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing precipitated hydrated silica based on the production of silicon slag from anhydrous hydrogen fluoride comprises the following steps:
[0009] Step 1: slurry the silicon slag with water to prepare a slurry, and filter the slurry with a precision filter to obtain a slurry;
[0010] Step 2: Primary filtering and rinsing the slurry to obtain a filter cake;
[0011] Step 3: slurry the filter cake into a dispersion, pass it into an overflow reaction tank, and perform graded reaction with an alkaline solution and a modifier to obtain a modified slurry;
[0012] Step 4: performing secondary filtration on the modified slurry to obtain a modified filter cake and a filtrate;
[0013] Step 5: Break up and dry the modified filter cake to obtain precipitated hydrated silica.
[0014] Furthermore, anhydrous hydrogen fluoride is prepared from fluorosilicic acid by decomposing it with sulfuric acid.
[0015] Furthermore, in step 2, the primary filtration is performed by filter pressing or filter pressing after centrifugation. The filter pressing is preferably a membrane plate and frame filter pressing device.
[0016] Furthermore, in step 3, the overflow reaction tank includes a first reaction tank, a second reaction tank, a third reaction tank and a fourth reaction tank connected in sequence, and the dispersion flows in the overflow reaction tank in a natural overflow manner. The overflow reaction tank is provided with a jacket or a coil, and overflow pipelines are provided between the first reaction tank and the second reaction tank, between the second reaction tank and the third reaction tank, and between the third reaction tank and the fourth reaction tank. An eccentric stirring device is provided in the first reaction tank, the second reaction tank, the third reaction tank and the fourth reaction tank.
[0017] Furthermore, the temperature of the first reaction tank is 90-92°C, and the pH value is 6.5-7; the temperature of the second reaction tank is 85-90°C, and the pH value is 6.8-7.2; the temperature of the third reaction tank is 83-88°C, and the pH value is 7.2-7.5; the temperature of the fourth reaction tank is 80-82°C, and the pH value is 7.2-8.0.
[0018] Furthermore, in step three, the alkaline solution is an aqueous solution of sodium carbonate or an aqueous solution of sodium hydroxide.
[0019] Further, in step three, the modifier is one or more of a coupling agent, a surfactant, an oligomer, an unsaturated organic acid, an organosilicon compound, and a water-soluble polymer. The amount of the modifier in the first reaction tank is 0.01wt%-0.015wt%, the amount of the modifier in the second reaction tank is 0.01wt%-0.02wt%, the amount of the modifier in the third reaction tank is 0.01wt%-0.015wt%, and the amount of the modifier in the fourth reaction tank is 0.001wt%-0.010wt%. The coupling agent is preferably silane or a polyethylene glycol with an average molecular weight greater than 1000, the surfactant is preferably anisole resin or isobutyl hydroxyphenyl ether, the oligomer is preferably oligofructose or sodium methyl silicate, the unsaturated organic acid is preferably linoleic acid or linolenic acid, the organosilicon compound is preferably silicone oil or silicone resin, and the water-soluble polymer is preferably PAM or hydroxymethyl cellulose. The modifier can modify the surface of the white carbon black, and the modifier can be selected according to the purpose of the white carbon black. The dispersion can be subjected to graded reactions with the same or different alkaline solutions and modifiers in the first reaction tank, the second reaction tank, the third reaction tank, and the fourth reaction tank, respectively.
[0020] Furthermore, in step 4, after the filtrate is concentrated and crystallized, solid-liquid separation and drying are carried out in sequence to obtain a fluoride salt product. The filtrate is concentrated using an MVR system or a triple-effect vacuum concentration system. The solid-liquid separation method is preferably centrifugation or filter pressing, the centrifugation using a horizontal centrifuge or a vertical centrifuge, and the filter pressing using a plate and frame filter press. The drying method is preferably spray drying or fluidized bed flash drying. The fluoride salt is a sodium fluoride crystalline substance.
[0021] Furthermore, the water removed by filtrate concentration and solid-liquid separation can be reused for silicon slag slurry, filter cake slurry, preparation of alkaline solution or production of anhydrous hydrogen fluoride.
[0022] Furthermore, in step 4, the secondary filtration is performed by filter pressing or centrifugal filtration. The filter pressing is preferably a membrane plate and frame filter pressing device.
[0023] The beneficial effects of the present invention are:
[0024] The method for preparing precipitated hydrated white carbon black based on the production of silicon slag with anhydrous hydrogen fluoride provided by the present invention comprises the following steps: slurrying silicon slag containing active silicon dioxide and filtering it with a precision filter having an automatic back-blowing function to remove most of the crystalline silicon dioxide; primary filtration is performed on the slurry and rinsed with water to remove residual hydrofluoric acid, sulfuric acid and fluorosilicic acid in the slurry; the dispersion is passed into an overflow reaction tank to perform graded reaction with an alkaline solution and a modifier, and during the graded reaction, neutralization and modification of the dispersion are simultaneously achieved, so that the neutralization reaction and modification of the active silicon dioxide are more sufficient and thorough, which is conducive to realizing the layer-by-layer modification of the active silicon dioxide to form a core-shell structure, and the overflow reaction tank can screen the silicon dioxide, and silicon dioxide with better dispersibility is more likely to overflow naturally with the dispersion; the modified slurry is sequentially subjected to secondary filtration and drying to achieve further purification.
[0025] The invention makes full use of silicon slag produced in the production process of anhydrous hydrogen fluoride, and prepares precipitated hydrated white carbon black with stable product quality by filtering, rinsing, graded reaction and drying the silicon slag, thereby improving the utilization rate of raw materials, reducing the processing cost of silicon slag and avoiding the emission of toxic gases. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 This is a process flow chart for preparing precipitated hydrated silica in Example 1. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0029] Example 1
[0030] A method for preparing precipitated hydrated silica based on the production of silicon slag from anhydrous hydrogen fluoride comprises the following steps:
[0031] Step 1: Use water to slurry the silicon slag to prepare a slurry with a concentration of 5wt%, and use a precision filter with a filtration accuracy of 5-10nm to filter the slurry to remove most of the crystalline silicon dioxide to obtain a slurry. The silicon slag is a by-product of the production of anhydrous hydrogen fluoride by the fluosilicic acid sulfuric acid decomposition method.
[0032] Step 2: Use F=100m 2 The slurry is filtered by a fully automatic diaphragm plate and frame filter press and rinsed with water to obtain a filter cake.
[0033] Step three: Beat the filter cake into a fully uniform dispersion without obvious visual particles, and pass it into the first reaction tank in the overflow reaction tank, and enter the second reaction tank, the third reaction tank and the fourth reaction tank in sequence through the overflow pipe in a natural overflow manner. The dispersion first enters the first reaction tank with a temperature controlled at 90-92°C, and the pH value of the liquid in the first reaction tank is adjusted to 6.5-7 with a sodium carbonate aqueous solution, and 0.01wt% of silane is added to the first reaction tank for a first-stage reaction; the liquid in the first reaction tank naturally overflows to the second reaction tank with a temperature controlled at 85-90°C, and the pH value of the liquid in the second reaction tank is adjusted to 6.8-7.2 with a sodium carbonate aqueous solution, and 0.015wt% of linoleic acid is added to the second reaction tank for a second-stage reaction; the liquid in the second reaction tank The liquid in the third reaction tank naturally overflows to the third reaction tank whose temperature is controlled at 83-88°C, and the pH value of the liquid in the third reaction tank is adjusted to 7.2-7.5 with sodium carbonate aqueous solution, and 0.01wt% PAM is added to the third reaction tank for the third stage reaction; the liquid in the third reaction tank naturally overflows to the fourth reaction tank whose temperature is controlled at 80-82°C, and the pH value of the liquid in the fourth reaction tank is adjusted to 7.2-8.0 with sodium carbonate aqueous solution, and 0.005wt% oligofructose is added to the fourth reaction tank for the fourth stage reaction to obtain the modified slurry. The volume of the overflow reaction tank is 2m 3 The height-to-diameter ratio is 1:1.15, a jacket is provided in the overflow reaction tank, and eccentric stirring devices are provided in the first reaction tank, the second reaction tank, the third reaction tank and the fourth reaction tank.
[0034] Step 4: Use a centrifuge to centrifuge the modified slurry, and then filter it to obtain the modified filter cake and filtrate. 3 The filtrate is concentrated and crystallized at a rate of 1000 rpm to a solid content of 20%, and then centrifuged in a horizontal centrifuge to obtain a material with a solid content of 55%. The material is flash dried in a fluidized bed to obtain a sodium fluoride product with a purity of 86% and a yield of 95.4%. The water removed by centrifugation can be used for silicon slag pulping, preparation of alkaline solution or production of anhydrous hydrogen fluoride. The water removed by filtrate concentration is reused for filter cake pulping, and the water removed by filtrate crystallization centrifugation is reused for silicon slag pulping. Among them, the MVR system was purchased from Huanruida Environmental Protection Technology Co., Ltd.
[0035] Step 5: Use a double-shaft crusher to break up the modified filter cake, then send it to a flash dryer for drying, collect the dried material into a cyclone dust collector, use positive pressure airflow to transport it to the packaging silo, and then automatically package and stack it under negative pressure to obtain the precipitated hydrated silica product. The double-shaft crusher was purchased from Kewei Machinery Co., Ltd.
[0036] Example 2
[0037] A method for preparing precipitated hydrated silica based on the production of silicon slag from anhydrous hydrogen fluoride comprises the following steps:
[0038] Step 1: Use water to slurry the silicon slag to prepare a slurry with a concentration of 5wt%, and use a precision filter with a filtration accuracy of 5-10nm to filter the slurry to remove most of the crystalline silicon dioxide to obtain a slurry. The silicon slag is a by-product of the production of anhydrous hydrogen fluoride by the fluosilicic acid sulfuric acid decomposition method.
[0039] Step 2: Use F=100m 2 The slurry is filtered by a fully automatic diaphragm plate and frame filter press and rinsed with water to obtain a filter cake.
[0040] Step three: Beat the filter cake into a fully uniform dispersion without obvious visual particles, pass it into the first reaction tank in the overflow reaction tank, and enter the second reaction tank, the third reaction tank and the fourth reaction tank in sequence through the overflow pipe in a natural overflow manner. The dispersion first enters the first reaction tank whose temperature is controlled at 90-92°C, and the pH value of the liquid in the first reaction tank is adjusted to 6.5-7 with sodium hydroxide aqueous solution, and 0.015wt% of isobutyl hydroxyphenyl ether is added to the first reaction tank for a first-stage reaction; the liquid in the first reaction tank naturally overflows to the second reaction tank whose temperature is controlled at 85-90°C, and the pH value of the liquid in the second reaction tank is adjusted to 6.8-7.2 with sodium hydroxide aqueous solution, and 0.01wt% of hydroxymethyl cellulose is added to the second reaction tank for a second-stage reaction; the second reaction tank The liquid in the third reaction tank naturally overflows to the third reaction tank whose temperature is controlled at 83-88°C, and the pH value of the liquid in the third reaction tank is adjusted to 7.2-7.5 with sodium hydroxide aqueous solution, and 0.012wt% of PAM is added to the third reaction tank for a third-stage reaction; the liquid in the third reaction tank naturally overflows to the fourth reaction tank whose temperature is controlled at 80-82°C, and the pH value of the liquid in the fourth reaction tank is adjusted to 7.2-8.0 with sodium hydroxide aqueous solution, and 0.004wt% of silicone resin is added to the fourth reaction tank for a fourth-stage reaction to obtain a modified slurry. The volume of the overflow reaction tank is 2m 3 The height-to-diameter ratio is 1:1.15, a coil is provided in the overflow reaction tank, and eccentric stirring devices are provided in the first reaction tank, the second reaction tank, the third reaction tank and the fourth reaction tank.
[0041] Step 4: Use a diaphragm plate and frame filter press to filter the modified slurry to obtain a modified filter cake and filtrate. The filtrate is concentrated and crystallized to a solid content of 22% using a triple-effect vacuum concentration system, and then input into a horizontal centrifuge for centrifugation to obtain a material with a solid content of 52%. The material is flash dried in a fluidized bed to obtain a sodium fluoride product with a purity of 84.7% and a yield of 96.4%. The water removed by centrifugation can be used for silicon slag pulping, preparation of alkaline solutions or production of anhydrous hydrogen fluoride. The water removed by filtrate concentration is reused for filter cake pulping, and the water removed by filtrate crystallization centrifugation is reused for silicon slag pulping.
[0042] Step 5: Use a double-shaft crusher to break up the modified filter cake, then send it into a horizontal drum dryer for drying, collect the dried material into a bag dust collector, use positive pressure airflow to transport it to the packaging silo, and then automatically package and stack it under negative pressure to obtain a precipitated hydrated silica product.
[0043] Example 3
[0044] A method for preparing precipitated hydrated silica based on the production of silicon slag from anhydrous hydrogen fluoride comprises the following steps:
[0045] Step 1: Use water to slurry the silicon slag to prepare a slurry with a concentration of 6wt%, and use a precision filter with a filtration accuracy of 5-10nm to filter the slurry to remove most of the crystalline silicon dioxide to obtain a slurry. The silicon slag is a by-product of the production of anhydrous hydrogen fluoride by the fluosilicic acid sulfuric acid decomposition method.
[0046] Step 2: Use F=100m 2 The slurry is filtered by a fully automatic diaphragm plate and frame filter press and rinsed with water to obtain a filter cake.
[0047] Step three: Beat the filter cake into a fully uniform dispersion without obvious visual particles, and pass it into the first reaction tank in the overflow reaction tank, and enter the second reaction tank, the third reaction tank and the fourth reaction tank in sequence through the overflow pipe in a natural overflow manner. The dispersion first enters the first reaction tank whose temperature is controlled at 90-92°C, and the pH value of the liquid in the first reaction tank is adjusted to 6.5-7 with sodium carbonate aqueous solution, and 0.012wt% of polyethylene glycol is added to the first reaction tank for a first-stage reaction, and the average molecular weight of polyethylene glycol is 2000; the liquid in the first reaction tank naturally overflows to the second reaction tank whose temperature is controlled at 85-90°C, and the pH value of the liquid in the second reaction tank is adjusted to 6.8-7.2 with sodium carbonate aqueous solution, and 0.013wt% of silane is added to the second reaction tank for a second-stage reaction; the second The liquid in the reaction tank naturally overflows to the third reaction tank whose temperature is controlled at 83-88°C, and the pH value of the liquid in the third reaction tank is adjusted to 7.2-7.5 with sodium carbonate aqueous solution, and 0.013wt% of hydroxymethyl cellulose is added to the third reaction tank for the third stage reaction; the liquid in the third reaction tank naturally overflows to the fourth reaction tank whose temperature is controlled at 80-82°C, and the pH value of the liquid in the fourth reaction tank is adjusted to 7.2-8.0 with sodium carbonate aqueous solution, and 0.006wt% of oligofructose is added to the fourth reaction tank for the fourth stage reaction to obtain the modified slurry. The volume of the overflow reaction tank is 2m 3 The height-to-diameter ratio is 1:1.15, a jacket is provided in the overflow reaction tank, and eccentric stirring devices are provided in the first reaction tank, the second reaction tank, the third reaction tank and the fourth reaction tank.
[0048] Step 4: Use a centrifuge to centrifuge the modified slurry, and then filter it to obtain the modified filter cake and filtrate. 3 The filtrate is concentrated and crystallized at a rate of 1.5447 W / h to a solid content of 23%, and then centrifuged in a horizontal centrifuge to obtain a material with a solid content of 51%. The material is flash dried in a fluidized bed to obtain a sodium fluoride product with a purity of 87.1% and a yield of 96.8%. The water removed by centrifugation can be used for silicon slag pulping, preparation of alkaline solution or production of anhydrous hydrogen fluoride. The water removed by filtrate concentration is reused for filter cake pulping, and the water removed by filtrate crystallization centrifugation is reused for silicon slag pulping. Among them, the MVR system was purchased from Huanruida Environmental Protection Technology Co., Ltd.
[0049] Step 5: Use a double-shaft crusher to break up the modified filter cake, then send it into a vibrating fluidized bed for drying, collect the dried material into an electrostatic precipitator, use positive pressure airflow to transport it to the packaging silo, and then automatically package and stack it under negative pressure to obtain a precipitated hydrated silica product.
[0050] Comparative Example 1
[0051] Comparative Example 1 is a commercially available precipitated silica product of Class D.
[0052] The specific surface area, loss on ignition, silica content, water-insoluble matter content, heating loss, pH value, oil absorption value, metal content and 45 μm sieve residue of the white carbon black products obtained in Examples 1-3 and Comparative Example 1 were tested respectively. The test results are shown in Table 1, and the test standard is HG / T3061-2020.
[0053] Table 1 Test results of white carbon black products obtained in Examples 1-3 and Comparative Example 1
[0054]
[0055] It can be seen from Table 1 that the white carbon black products prepared by the method provided by the present invention in Examples 1-3 have higher purity and specific surface area.
[0056] The heavy metal content and the harmful substance content in the white carbon black products obtained in Examples 1-3 and Comparative Example 1 were tested respectively. The test was carried out according to the revised Directive (EU) 2015 / 863 of Appendix II of EU ROHS Directive 2011 / 65 / EU. The test results are shown in Table 2.
[0057] Table 2 Detection results of harmful substances in the white carbon black products obtained in Examples 1-3 and Comparative Example 1
[0058]
[0059] As can be seen from Table 2, the heavy metal content and the harmful substance content of the white carbon black products obtained in Examples 1-3 all meet the test standards and are lower than those in Comparative Example 1, indicating that the products produced by the method provided by the present invention are safe and non-toxic.
[0060] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.
Claims
1. A method for preparing precipitated hydrated silica based on the production of silicon slag from anhydrous hydrogen fluoride, characterized in that: The steps include: Step 1: slurry the silicon slag with water to prepare a slurry, and filter the slurry with a precision filter to obtain a slurry; Step 2: Primary filtering and rinsing the slurry to obtain a filter cake; Step 3: slurry the filter cake into a dispersion, pass it into an overflow reaction tank, and perform graded reaction with an alkaline solution and a modifier to obtain a modified slurry; Step 4: performing secondary filtration on the modified slurry to obtain a modified filter cake and a filtrate; Step 5: breaking up and drying the modified filter cake to obtain precipitated hydrated silica; In step 3, the overflow reaction tank includes a first reaction tank, a second reaction tank, a third reaction tank and a fourth reaction tank connected in sequence, and the dispersion flows in the overflow reaction tank in an overflow manner; The temperature of the first reaction tank is 90-92°C, and the pH value is 6.5-7; the temperature of the second reaction tank is 85-90°C, and the pH value is 6.8-7.2; the temperature of the third reaction tank is 83-88°C, and the pH value is 7.2-7.5; the temperature of the fourth reaction tank is 80-82°C, and the pH value is 7.2-8.
0.
2. The method according to claim 1, characterized in that Anhydrous hydrogen fluoride is prepared from fluorosilicic acid by decomposition with sulfuric acid.
3. The method according to claim 1, characterized in that In step 2, the primary filtration method is filter pressing or filter pressing followed by centrifugation.
4. The method according to claim 1, characterized in that In step 3, the alkaline solution is an aqueous solution of sodium carbonate or an aqueous solution of sodium hydroxide.
5. The method according to claim 1, characterized in that In step three, the modifier is one or more of a coupling agent, a surfactant, an oligomer, an unsaturated organic acid, an organosilicon compound, and a water-soluble polymer.
6. The method according to claim 1, characterized in that In step 4, the filtrate is concentrated and crystallized, and then solid-liquid separation and drying are performed in sequence to obtain a fluoride salt product.
7. The method according to claim 6, characterized in that The water removed by filtrate concentration and solid-liquid separation can be reused for silicon slag slurry, filter cake slurry, preparation of alkaline solution or production of anhydrous hydrogen fluoride.
8. The method according to claim 1, characterized in that In step 4, the secondary filtration method is filter pressing or filtration after centrifugation.
Citation Information
Patent Citations
Method for preparing white carbon black from silicon slags containing fluorine
CN103663474A