A screen printing alignment film and preparation method thereof

By using optimized proportional pressure-sensitive adhesive and preparation process in the screen printing alignment film, the problems of low bonding performance and high residual adhesive rate in the prior art are solved, and the stability and efficient cleaning of high-precision screen printing are achieved. sex.

CN118372569BActive Publication Date: 2024-11-22SHENZHEN LIJIN TECH ENTERPRISES MATERLALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410512483.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-11-22
Estimated Expiration
2044-04-26

Smart Images

  • Figure CN118372569B_ABST
    Figure CN118372569B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of screen printing, and in particular to a screen printing alignment film and a preparation method thereof. The preparation method of the screen printing alignment film of the present invention comprises the following steps: uniformly coating the screen printing alignment film with a pressure-sensitive adhesive on a PE film, with a coating amount of 10-50 g / m 2 ; UV curing machine for 30-60 seconds, light energy of 200-600mJ / cm 2 ; Corona treatment, treatment voltage 10000-20000V, treatment time 10-30 seconds, to prepare the screen printing alignment film. The screen printing alignment film of the present invention adopts a carefully selected pressure-sensitive adhesive and optimizes the preparation process to provide excellent adhesion and stability to meet the requirements of high-precision screen printing. After UV curing and corona treatment, the alignment film can quickly and firmly adhere to the PE film to ensure accurate alignment. Its 180° peel strength shows good adhesion, and the low residual glue rate simplifies cleaning work, improves work efficiency, reduces printing defects, ensures the quality of printed products, and meets the needs of high-end screen printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of screen printing, and in particular to a screen printing alignment film and a preparation method thereof. Background Art

[0002] Screen printing is a widely used technology for printing graphics and texts. It uses a fabric mesh to transfer ink to a substrate to achieve the reproduction of patterns. Although this technology has a wide range of applications in multiple industries, such as clothing printing, electronic product identification and billboard production, there are still some challenges in actual operation, especially in terms of accurate alignment and pattern positioning. In order to improve printing accuracy and efficiency, a special alignment auxiliary material for the screen printing process, the screen printing alignment film, has been developed.

[0003] Although this technology has many advantages, the existing technology still faces some significant challenges in terms of the need for precise alignment, especially when using silk screen alignment film for multi-color printing or fine pattern printing, the shortcomings of the existing technology are particularly prominent.

[0004] In the existing screen printing alignment technology, there are mainly the following two disadvantages:

[0005] (1) Low adhesion and peel strength: Existing screen printing alignment films have insufficient adhesion in some application scenarios. This results in the alignment film being unable to be stably fixed during the printing process and being easily displaced during the printing or drying process, affecting the accuracy and consistency of the printed pattern. Although low peel strength facilitates the removal of the film, it is not sufficient to ensure positional stability during printing, which is particularly critical in fine or multi-color printing.

[0006] (2) It is not easy to completely peel off, and the residual adhesive rate is high: Another key problem is that the existing alignment film often leaves residual adhesive after peeling. This not only affects the appearance and quality of the printed product, but also increases the difficulty and cost of post-processing. The high residual adhesive rate means that an additional cleaning step is required, which is not only time-consuming, but may also cause damage to the material due to the use of solvents or detergents, especially on sensitive materials.

[0007] In view of the above shortcomings, it is urgent to develop a new type of screen printing alignment film, which should have improved bonding properties, and can ensure accurate alignment and stability during the printing process while ensuring peeling strength. At the same time, the new alignment film should be able to achieve clean peeling without leaving residual glue, thereby reducing the workload of post-processing and improving production efficiency and printing quality. Summary of the invention

[0008] The present invention aims to solve the problems existing in the prior art by optimizing the material composition and production process of the alignment film, and to provide a more reliable solution for high-quality screen printing. The technical problem to be solved by the present invention is to provide a screen printing alignment film and a preparation method thereof.

[0009] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0010] The invention discloses a method for preparing a screen printing alignment film, comprising the following steps:

[0011] Step 1: Apply the screen printing alignment film evenly to the PE film with pressure-sensitive adhesive;

[0012] Step 2: UV curing;

[0013] Step 3: Corona treatment.

[0014] Preferably, a method for preparing a screen printing alignment film comprises the following steps:

[0015] Step 1: Apply the screen printing alignment film evenly to the PE film with pressure-sensitive adhesive, with a coating amount of 10-50g / m 2 ;

[0016] Step 2: Expose the film to UV light for 30-60 seconds with a light energy of 200-600mJ / cm 2 ;

[0017] Step 3: corona treatment, with a treatment voltage of 10000-20000V and a treatment time of 10-30 seconds, to prepare the screen printing alignment film.

[0018] Preferably, the pressure-sensitive adhesive for screen printing alignment film is prepared from the following raw materials in parts by weight using a conventional method;

[0019] 10-20 parts of methyl methacrylate;

[0020] 10-20 parts of vinyl acetate;

[0021] Epoxy acrylate 20-25 parts;

[0022] 2-Ethylhexyl acrylate 15-25 parts;

[0023] 2-isocyanatoethyl acrylate 10-15 parts;

[0024] 10-15 parts of hydroxyethyl methacrylate;

[0025] 1-2 parts of azobisisobutyronitrile;

[0026] 80-120 parts of ethyl acetate;

[0027] 2-8 parts of mercaptan chain transfer agent.

[0028] The mercaptan-based chain transfer agent is at least one of n-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, 1,10-decandithiolan and dipropyltrimercaptan.

[0029] Preferably, the pressure-sensitive adhesive for the screen printing alignment film is prepared by the following method:

[0030] Methyl methacrylate, vinyl acetate, epoxy acrylate, 2-ethylhexyl acrylate, 2-isocyanoethyl acrylate, hydroxyethyl methacrylate, part of azobisisobutyronitrile, part of ethyl acetate and a thiol chain transfer agent are mixed uniformly to obtain a mixed solution A;

[0031] dissolving the remaining azobisisobutyronitrile in the remaining ethyl acetate to obtain a mixed solution B;

[0032] Under nitrogen atmosphere, the mixed solution B was uniformly added dropwise to the mixed solution A, and the mixture was stirred for reaction for 2-6 hours.

[0033] Preferably, the pressure-sensitive adhesive for the screen printing alignment film is prepared by the following method:

[0034] Methyl methacrylate, vinyl acetate, epoxy acrylate, 2-ethylhexyl acrylate, 2-isocyanatoethyl acrylate, hydroxyethyl methacrylate, 40-80 wt % of azobisisobutyronitrile, 30-70 wt % of ethyl acetate and a thiol chain transfer agent are uniformly mixed to obtain a mixed solution A;

[0035] dissolving the remaining azobisisobutyronitrile in the remaining ethyl acetate to obtain a mixed solution B;

[0036] Under nitrogen atmosphere, the mixed solution A is heated to 70-78° C., and the mixed solution B is added dropwise to the mixed solution A at a uniform rate of 1-5 drops / second. After the addition is completed, the mixture is stirred at 40-100 rpm for 2-6 hours.

[0037] The invention also discloses a silk-screen alignment film, which is prepared by adopting the method.

[0038] The screen printing alignment film of the present invention adopts a carefully selected pressure-sensitive adhesive and optimizes the preparation process to provide excellent adhesion and stability to meet the requirements of high-precision screen printing. After UV curing and corona treatment, the alignment film can quickly and firmly adhere to the PE film to ensure accurate alignment. Its 180° peel strength shows good adhesion, and the low residual adhesive rate simplifies cleaning work, improves work efficiency, reduces printing defects, ensures the quality of printed products, and meets the needs of high-end screen printing. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1This is a photo of the screen printing alignment film prepared by the present invention. DETAILED DESCRIPTION

[0040] A pressure-sensitive adhesive for a silk-screen alignment film is prepared from the following raw materials in parts by weight:

[0041] 10-20 parts of methyl methacrylate;

[0042] 10-20 parts of vinyl acetate;

[0043] Epoxy acrylate 20-25 parts;

[0044] 2-Ethylhexyl acrylate 15-25 parts;

[0045] 2-isocyanatoethyl acrylate 10-15 parts;

[0046] 10-15 parts of hydroxyethyl methacrylate;

[0047] 1-2 parts of azobisisobutyronitrile;

[0048] 80-120 parts of ethyl acetate;

[0049] 2-8 parts of mercaptan chain transfer agent.

[0050] The thiol-based chain transfer agent is at least one of n-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, 1,10-decandithiolan and dipropyltrimercaptan. Preferably, the thiol-based chain transfer agent at least comprises 1,10-decandithiolan. Further preferably, the thiol-based chain transfer agent is composed of 1,10-decandithiolan and n-dodecyl mercaptan in a mass ratio of 1:(0.5-2).

[0051] In the present invention, methyl methacrylate is a widely used hard monomer, and its main contribution is to improve the hardness and strength of the polymer. When methyl methacrylate monomer is converted into polymethyl methacrylate in the polymerization reaction, since polymethyl methacrylate has a high Tg (glass transition temperature), this makes the obtained polymer show hard and brittle properties at room temperature. This hardness is determined by the strong rigidity of the polymethyl methacrylate molecular chain, and the rigid chain is difficult to move at low temperatures, thereby giving the material a higher hardness. In the application of the pressure-sensitive adhesive of the present invention, adding an appropriate amount of methyl methacrylate can significantly improve the wear resistance of the adhesive film. This is because the enhanced hardness can reduce the damage to the adhesive film caused by physical wear, especially in application scenarios that require long-term adhesion or frequent contact. The chemical structure of polymethyl methacrylate determines its excellent chemical resistance. Since the methyl ester group contained in the methyl methacrylate molecule shows strong resistance to most organic solvents and chemicals, this enables the pressure-sensitive adhesive based on methyl methacrylate to maintain its structure and performance stability when facing chemical pollution or corrosive environments.

[0052] Vinyl acetate, as another hard monomer, can effectively adjust the glass transition temperature of the pressure-sensitive adhesive when copolymerized with methyl methacrylate. This is because the introduction of vinyl acetate provides a certain flexibility to the polymer chain, although it is also classified as a hard monomer. The polymer of vinyl acetate has a low Tg, and the copolymer formed with polymethyl methacrylate can achieve a subtle adjustment of Tg, which is very important for balancing the adhesion performance and physical stability of the pressure-sensitive adhesive. In the present invention, by adjusting the ratio of methyl methacrylate and vinyl acetate, while maintaining good hardness, it is ensured that the adhesive film maintains appropriate flexibility and toughness within the application temperature range.

[0053] Epoxy acrylate is an acrylate monomer containing epoxy groups, which provides unique chemical reactivity through its epoxy groups. These epoxy groups can participate in further chemical reactions in the polymer after polymerization, such as cross-linking reactions with amines, acids or alcohols to form a three-dimensional network structure. The cross-linking reaction of epoxy groups increases the interaction between molecules, and this enhanced intermolecular interaction improves the adhesion of pressure-sensitive adhesives to various surfaces. Especially for substrates with low surface energy (such as certain plastics and metals), epoxy acrylate can significantly improve the bonding effect of pressure-sensitive adhesives. The network structure formed by the cross-linking reaction of epoxy groups not only improves the mechanical strength of the polymer, but also effectively blocks the penetration of moisture and chemicals. This feature allows pressure-sensitive adhesives to maintain good performance in humid environments or when in contact with chemicals, expanding their application range.

[0054] 2-Ethylhexyl acrylate is a long-chain acrylate monomer whose long alkyl side chains give the polymer excellent flexibility and adhesion. The long alkyl side chains introduce a large steric hindrance into the polymer, which reduces the interaction between molecules and increases the freedom of movement of the polymer chain. This structural feature allows the pressure-sensitive adhesive to maintain good flexibility at low temperatures and avoids the degradation of bonding performance due to hardening. The long-chain structure of 2-ethylhexyl acrylate also helps to enhance the wettability of the polymer and the substrate surface, improving the contact area and quality of the pressure-sensitive adhesive with the substrate. This improved wettability allows the pressure-sensitive adhesive to better penetrate into the microstructure of the substrate surface, thereby improving the bonding strength.

[0055] The use of these two soft monomers, epoxy acrylate and 2-ethylhexyl acrylate, in the pressure-sensitive adhesive formula not only improves the bonding performance of the pressure-sensitive adhesive through their unique chemical structure and properties, but also enhances its durability in a variety of usage environments.

[0056] As functional monomers, 2-isocyanatoethyl acrylate and hydroxyethyl methacrylate play a vital role in the preparation of pressure-sensitive adhesives. By introducing specific chemical functional groups into the polymer, these monomers can not only improve the basic properties of pressure-sensitive adhesives, but also give them special physical and chemical properties to meet specific application requirements.

[0057] 2-Isocyanoethyl acrylate (CAS: 13641-96-8) contains active isocyanate groups (-NCO), which can react with compounds containing active hydrogen atoms (such as alcohols, amines or water) to form urea or urea ether structures, thereby forming crosslinking points within the polymer or between the polymer and other components. By introducing 2-isocyanoethyl acrylate, the crosslinked network formed in the pressure-sensitive adhesive significantly enhances the mechanical strength of the material. This enhancement effect comes from the fact that the crosslinked structure can more effectively disperse stress when subjected to external forces, reducing deformation and breakage of the material. At the same time, the crosslinked network also improves the temperature resistance of the pressure-sensitive adhesive. Under high temperature conditions, uncrosslinked polymers may soften or flow due to increased molecular motion, while the crosslinked structure can maintain the stability of the polymer and keep its performance unaffected by temperature.

[0058] Hydroxyethyl methacrylate contains active hydroxyl groups (-OH), which can participate in cross-linking reactions or react with other chemical functional groups to form stable chemical bonds. The introduction of hydroxyl groups is conducive to increasing the attraction between molecules through non-covalent interactions such as hydrogen bonds, thereby improving the cohesion of the polymer. Enhanced cohesion means that the pressure-sensitive adhesive has better structural integrity and shear resistance. In complex application environments, such as wet or greasy surfaces, enhanced cohesion ensures that the pressure-sensitive adhesive maintains good bonding properties. The chemical bonds formed by the cross-linking reaction involving hydroxyl groups are less susceptible to hydrolysis than physical entanglement or hydrophobic interactions, thereby improving the stability of the pressure-sensitive adhesive in humid environments. This hydrolysis resistance is particularly important for outdoor applications or applications that require long-term water contact, and can ensure the long-term stability of the pressure-sensitive adhesive performance.

[0059] The combined effect of 2-isocyanatoethyl acrylate and hydroxyethyl methacrylate significantly improves the mechanical properties, temperature resistance, cohesion and hydrolysis resistance of the pressure-sensitive adhesive, which can meet the application requirements of screen printing alignment films and ensure the accuracy of the printing process and the high quality of printed products.

[0060] In the present invention, the role of azobisisobutyronitrile (AIBN) as a free radical initiator is crucial, especially in the preparation of pressure-sensitive adhesives for screen printing alignment films. AIBN generates free radicals by decomposing at moderate temperatures, initiating the polymerization reaction of various monomers including methyl methacrylate, vinyl acetate, epoxy acrylate, etc. This process not only ensures that the molecular weight and structure of the polymer are formed as expected, but also further achieves fine-tuning of polymer properties, such as adhesion, strength, and resistance to environmental factors, by precisely controlling the amount of AIBN. In the pressure-sensitive adhesive of the present invention, the use of AIBN enables the final product to have excellent bonding properties and suitable mechanical strength, meeting the application requirements of screen printing alignment films in different printing environments, while ensuring the accuracy of the printing process and the high quality of the printed products.

[0061] As a solvent with good volatility and good solubility for many polymers, ethyl acetate provides a uniform reaction environment for various monomers and functional components such as methyl methacrylate and vinyl acetate, ensuring that they can be effectively mixed and polymerized. This process is not only crucial for achieving uniformity and high performance of polymers, but also facilitates fine control of the viscosity of polymer solutions by adjusting the solvent content to meet different coating and film-forming requirements. During the coating and curing stages of the pressure-sensitive adhesive, the volatilization of ethyl acetate also helps to form a uniform and continuous film layer, thereby ensuring the high quality and printing accuracy of the screen printing alignment film.

[0062] n-Butyl mercaptan, CAS No. 109-79-5. n-Octyl mercaptan, CAS No. 111-88-6. n-Dodecyl mercaptan, CAS No. 7773-83-3. 1,10-Decanedithiol, CAS No. 1191-67-9. Dipropyltrimercaptan, CAS No. 3069-40-7.

[0063] Compounds such as n-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, 1,10-decanedithiol, and dipropyltrithiol can be used as effective thiol chain transfer agents to control the molecular weight and molecular weight distribution of polymers in free radical polymerization reactions because their chemical structures contain thiol groups (-SH) that can react with free radicals. In the polymerization reaction, they terminate the growth of the current polymer chain and start the growth of new chains, thereby achieving the purpose of regulating the molecular weight of the polymer.

[0064] Specifically, the method for preparing the pressure-sensitive adhesive for the screen printing alignment film comprises the following steps:

[0065] Methyl methacrylate, vinyl acetate, epoxy acrylate, 2-ethylhexyl acrylate, 2-isocyanatoethyl acrylate, hydroxyethyl methacrylate, 40-80 wt % of azobisisobutyronitrile, 30-70 wt % of ethyl acetate and a thiol chain transfer agent are uniformly mixed to obtain a mixed solution A;

[0066] Different monomer components are copolymerized to form polymers with specific properties. Azobisisobutyronitrile is added as an initiator to start the polymerization reaction, while ethyl acetate is used as a solvent to adjust the viscosity of the reaction mixture, and a thiol-based chain transfer agent is used as a chain transfer agent to control the polymer molecular weight.

[0067] dissolving the remaining azobisisobutyronitrile in the remaining ethyl acetate to obtain a mixed solution B;

[0068] The gradual addition of initiator allows the polymerization rate and the molecular weight of the polymer to be precisely adjusted as needed. In the polymerization reaction, the concentration of the initiator directly affects the generation rate of free radicals, which in turn determines the polymerization rate and the growth rate of the molecular chain. By controlling the dripping rate of the mixed solution B, the reaction rate and heat generation can be balanced to prevent the quality of the polymer from being affected by local overheating.

[0069] Under nitrogen atmosphere, the mixed solution A is heated to 70-78° C., and the mixed solution B is added dropwise to the mixed solution A at a uniform rate of 1-5 drops / second. After the addition is completed, the mixture is stirred at 40-100 rpm for 2-6 hours.

[0070] The polymerization reaction is carried out under a nitrogen atmosphere to exclude oxygen and avoid undesired chain termination reactions caused by oxygen, thereby improving the quality of the polymer. Heating to 70-78°C is to ensure that azobisisobutyronitrile is effectively decomposed to generate free radicals to start the polymerization reaction. By uniformly adding mixed solution B to mixed solution A at a rate of 1-5 drops / second, the rate of polymerization reaction can be controlled to ensure the uniformity of polymerization reaction and the molecular weight distribution of polymer. Continuous stirring after the addition (40-100rpm, 2-6 hours) ensures the complete progress of the polymerization reaction, helps eliminate the temperature gradient and concentration gradient that may exist in the reaction system, and promotes the uniform growth of polymer chains.

[0071] A screen printing alignment film and a preparation method thereof, comprising the following steps:

[0072] Step 1: Apply the above-mentioned screen printing alignment film evenly to the PE film with pressure-sensitive adhesive, with a coating amount of 10-50g / m 2 ;

[0073] Step 2: Expose the film to UV light for 30-60 seconds with a light energy of 200-600mJ / cm 2 ;

[0074] The PE film coated with pressure-sensitive adhesive is subjected to light treatment on a UV light curing machine in order to promote the cross-linking reaction of the photosensitive components in the pressure-sensitive adhesive through the energy of UV light, thereby quickly curing to form a stable adhesive layer.

[0075] Step 3: corona treatment, with a treatment voltage of 10000-20000V and a treatment time of 10-30 seconds, to prepare the screen printing alignment film.

[0076] Corona treatment generates tiny discharges on the film surface through a high-voltage electric field, instantly changing the surface properties and increasing the polarity and roughness of the surface. This surface modification technology can significantly increase the surface energy of the PE film, thereby enhancing the adhesion between the film and other substances, improving wear resistance, and making the alignment film show better performance during the screen printing process.

[0077] The screen printing alignment film of the present invention utilizes a pressure-sensitive adhesive with a unique formula and, after a carefully designed preparation process, exhibits significant performance advantages and provides ideal support for high-precision screen printing. First, by selecting a specific proportion of monomers such as methyl methacrylate, vinyl acetate, epoxy acrylate, and combining the functional monomers of 2-isocyanatoethyl acrylate and hydroxyethyl methacrylate, the prepared pressure-sensitive adhesive not only performs well in adhesion, but also has good environmental resistance and stability. In particular, through the UV curing and corona treatment steps, this alignment film can be quickly cured and firmly adhered to the PE film in practical applications, ensuring accurate alignment during the printing process. The screen printing alignment film of the present invention has a high 180° peeling strength, showing its excellent adhesion; the residual glue rate is low, indicating that the alignment film is easy to clean after use, leaving very little residual glue, which greatly reduces the burden of subsequent cleaning work. These characteristics not only improve work efficiency and reduce printing defects, but also ensure the neatness and beauty of printed products, meeting the needs of high-quality screen printing.

[0078] The PE film in the specific implementation manner is provided by Shenzhen Lijin Technology Electronic Materials Co., Ltd.

[0079] Example 1

[0080] A pressure-sensitive adhesive for a silk-screen alignment film is prepared from the following raw materials in parts by weight:

[0081] 15 parts of methyl methacrylate;

[0082] 15 parts of vinyl acetate;

[0083] Epoxy acrylate 22.5 parts;

[0084] 20 parts of 2-ethylhexyl acrylate;

[0085] 2-isocyanatoethyl acrylate 12.5 parts;

[0086] 12.5 parts of hydroxyethyl methacrylate;

[0087] 1.5 parts of azobisisobutyronitrile;

[0088] 100 parts of ethyl acetate;

[0089] 5 parts of mercaptan chain transfer agent n-butyl mercaptan.

[0090] The method for preparing the pressure-sensitive adhesive for the screen printing alignment film comprises the following steps:

[0091] At room temperature, methyl methacrylate, vinyl acetate, epoxy acrylate, 2-ethylhexyl acrylate, 2-isocyanatoethyl acrylate, hydroxyethyl methacrylate, 60% of azobisisobutyronitrile, 50% of ethyl acetate and thiol chain transfer agent n-butyl mercaptan are mixed uniformly to obtain a mixed solution A;

[0092] At room temperature, dissolving the remaining 40% of the azobisisobutyronitrile in the remaining 50% of the ethyl acetate to obtain a mixed solution B;

[0093] Under nitrogen atmosphere, the mixed solution A was heated to 73°C and stirred at 60 rpm. The mixed solution B was added to the mixed solution A at a rate of 2 drops per second. After the addition was completed, the mixture was stirred at 60 rpm for 4 hours.

[0094] Specifically control the total amount of all raw materials in the pressure-sensitive adhesive for screen printing alignment film to be 200 grams.

[0095] A screen printing alignment film and a preparation method thereof, comprising the following steps:

[0096] Step 1: Apply the above-mentioned screen printing alignment film evenly to the PE film with pressure-sensitive adhesive, with a coating amount of 30g / m 2 ;

[0097] Step 2: Expose the film on a UV curing machine for 40 seconds with an energy of 400mJ / cm 2 ;

[0098] Step 3: corona treatment, with a treatment voltage of 15000 V and a treatment time of 20 seconds, to prepare the screen printing alignment film.

[0099] Example 2

[0100] The mercaptan-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of n-octyl mercaptan.

[0101] Example 3

[0102] The mercaptan-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of dipropyltrimercaptan.

[0103] Example 4

[0104] The mercaptan-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of n-dodecyl mercaptan.

[0105] Example 5

[0106] The mercaptan-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of 1,10-decanedithiol.

[0107] Example 6

[0108] The thiol-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of a mixed thiol-based chain transfer agent consisting of n-dodecyl mercaptan and 1,10-decanedithiol in a mass ratio of 1:1.

[0109] Comparative Example 1

[0110] The mercaptan-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of French Arkema polyether polyol Dianol 285.

[0111] Comparative Example 2

[0112] The mercaptan-based chain transfer agent n-butyl mercaptan in Example 1 was replaced by an equal weight of Dow polyether polyol VORANOL 2070.

[0113] Test Example 1

[0114] According to the test method of method 1 (180° peel strength between adhesive tape and stainless steel) in standard GB / T2792-2014, the 180° peel strength of the screen printing alignment film was tested.

[0115] Table 1 Peel strength test results

[0116] 180° peel strength, N / cm Example 1 4.8 Example 2 5.0 Example 3 5.1 Example 4 5.3 Example 5 6.4 Example 6 7.3 Comparative Example 1 2.5 Comparative Example 2 2.1

[0117] Test Example 2:

[0118] Residual adhesive rate test: paste the screen printing alignment film on the stainless steel plate, and roll it with a roller at a pressure of 80kPa for 3 times. Place it in a 90℃ oven for 24 hours, take it out and cool it to room temperature, peel it off in a 180° direction at a speed of 250mm / min, and calculate the residual adhesive rate.

[0119] The residual glue rate is calculated by comparing the residual glue area left on the stainless steel plate with the area of ​​the original fully pasted screen printing alignment film. Specifically, the percentage of the residual glue area to the original pasted area is the residual glue rate.

[0120] Table 2 Test results of residual glue rate

[0121] Residual glue rate, % Example 1 2.7 Example 2 2.5 Example 3 2.9 Example 4 2.0 Example 5 1.1 Example 6 0.6 Comparative Example 1 4.5 Comparative Example 2 4.9

[0122] In the present invention, by comparing Examples 1-5 with Comparative Examples 1-2 in detail, it can be clearly observed that the use of thiol chain transfer agents has significant advantages over other types of chain transfer agents. The essence of this advantage is not only due to the unique chemical structure and reactivity of the thiol chain transfer agent itself, but also closely related to the specific combination of soft and hard monomers and functional monomers carefully selected in the present invention. The thiol group has a high reactivity---the active sulfur-hydrogen bond (-SH) can quickly react with the growing polymer chain free radicals, effectively terminate the growth of the current chain and trigger new chain growth, thereby showing unique efficiency in regulating the molecular weight and molecular weight distribution of the polymer. This regulation mechanism, especially when combined with hard monomers such as methyl methacrylate, vinyl acetate, and soft monomers such as epoxy acrylate and 2-ethylhexyl acrylate selected by the present invention, can significantly optimize the comprehensive performance of the pressure-sensitive adhesive, including improving its adhesion, temperature resistance, chemical resistance and mechanical strength.

[0123] Further, the combination of mercaptan chain transfer agent and functional monomers in the present invention, such as 2-isocyanatoethyl acrylate and hydroxyethyl methacrylate, can form a stable cross-linked network in the polymer, and enhance the cohesion and cross-linking density of the material. The specific reactive groups introduced by these functional monomers, such as isocyanate groups and hydroxyl groups, not only participate in the polymerization reaction to enhance the structural strength of the polymer, but also promote the synergistic effect with the mercaptan chain transfer agent, and jointly optimize the formation of the polymer network, so that the final silk screen alignment film has better physical and chemical properties, and a lower residual glue rate during the stripping process. The advantage of the mercaptan chain transfer agent is also reflected in its microscopic regulation of the polymerization process. By accurately controlling the conditions of the polymerization reaction, a fine regulation of the polymer molecular weight is achieved. This regulation is not only crucial to improving the bonding performance of the silk screen alignment film, but also has a direct impact on reducing residual glue and improving the accuracy and repeatability of the printing process. Therefore, the use of thiol-based chain transfer agents in the present invention, combined with a combination of specific soft and hard monomers and functional monomers, not only effectively improves the comprehensive performance of the pressure-sensitive adhesive, but also optimizes the performance of the screen printing alignment film in high-precision printing applications, ensures the consistency and reliability of printing quality, and meets the high requirements for accuracy and durability in screen printing.

[0124] Further, in Examples 1-5, the performance of the screen printing alignment film was optimized by using different thiol chain transfer agents, and it was found that 1,10-decanedithiol was more effective than other thiol chain transfer agents. The root of this difference lies in the differences in the specific chemical structures between thiol chain transfer agents and how these structural differences affect their behavior in polymerization reactions. The thiol group can effectively react with the growing polymer chain free radicals due to its active sulfur-hydrogen bond (-SH), terminate the growth of the current chain and start the growth of a new chain, thereby controlling the molecular weight and molecular weight distribution of the polymer. 1,10-decanedithiol is unique in that its molecular structure contains two active thiol groups located at both ends of the molecule. This bifunctional structure enables it to not only participate in the reaction as a chain transfer agent in the polymerization reaction, but also promote crosslinking or form a more complex polymer structure through the double-terminal thiol groups. In addition, the longer alkyl chain of 1,10-decanedithiol can introduce more flexible segments into the polymer, thereby affecting the physical properties of the polymer, such as improving its flexibility and adhesion. The introduction of this flexible chain segment helps the polymer to better wet the bonded surface, forming a more uniform and tight bonding interface, thereby improving the bonding strength. At the same time, the introduction of long-chain alkyl groups may also affect the compatibility and microphase structure of the polymer through hydrophobic interactions, further optimizing its performance. In contrast, other thiol-based chain transfer agents have different effects on polymerization reactions and contributions to polymer properties due to the monofunctional characteristics of their structures and different chain lengths or structural complexities. Therefore, the unique effect of 1,10-decanedithiol in the polymerization reaction is due to both the structural characteristics of its dithiol group and its longer alkyl chain. These characteristics work together on the polymerization process and the final properties of the polymer, making it show excellent effects in regulating the molecular weight and molecular weight distribution of the polymer and optimizing the physical and chemical properties of the polymer.

[0125] Furthermore, comparing Example 5 with Example 4, the main structural differences between 1,10-decanedithiol and n-dodecyl mercaptan are reflected in the number of functional groups and the configuration of the molecular structure, and these differences directly affect their performance as chain transfer agents. 1,10-Decanedithiol has two thiol groups, located at both ends of the molecule, while n-dodecyl mercaptan contains only one thiol group. This structural difference means that 1,10-decanedithiol can participate in the chain transfer reaction from two directions in the polymerization reaction, which can theoretically more effectively control the molecular weight and molecular weight distribution of the polymer, and may also promote a certain degree of cross-linking reaction, thereby changing the network structure and properties of the final polymer. Due to the thiol groups at both ends of 1,10-decanedithiol, a more complex structure can be formed in the polymer, which may have an important effect on the physical properties of the polymer, such as improving its flexibility, adhesion and mechanical strength. Although the monothiol group of n-dodecyl mercaptan can also effectively carry out chain transfer reactions, its regulatory effect on the structure and properties of the polymer is relatively limited, mainly reflected in regulating the molecular weight and molecular weight distribution. 1,10-Decanedithiol, due to its unique dithiol group structure, shows great advantages in improving the adhesion of polymers, reducing residual glue, and improving temperature resistance and chemical resistance. This may be because the dithiol group structure can not only regulate the polymerization reaction more effectively, but also optimize the performance of the polymer by cross-linking or forming specific structural features. In contrast, although n-dodecyl mercaptan can also be used as an effective chain transfer agent, its single thiol group and relatively simple molecular structure limit its potential in performance regulation. Therefore, from a structural point of view, the difference between 1,10-decanedithiol and n-dodecyl mercaptan leads to obvious differences in their performance as chain transfer agents, especially in improving the comprehensive performance of polymers, 1,10-decanedithiol shows a more significant effect.

[0126] In Example 6, a unique synergistic effect was created by mixing n-dodecyl mercaptan and 1,10-decyl dithiol as chain transfer agents, significantly optimizing the performance of the screen printing alignment film. The reason may be that n-dodecyl mercaptan provides stable chain transfer efficiency, while the bifunctional structure of 1,10-decyl dithiol enhances the crosslinking density and flexibility of the polymer. In this way, the mixed chain transfer agent can not only effectively control the molecular weight of the polymer, but also improve its cohesion and adhesion, resulting in a comprehensive improvement in polymer performance in multiple aspects, reflecting a more significant synergistic effect than when used alone.

[0127] Figure 1The following is a photo of the screen printing alignment film prepared by the present invention. The screen printing alignment film of the present invention has significantly improved adhesion and environmental stability through an original pressure-sensitive adhesive formula and a sophisticated production process, and is particularly suitable for high-precision screen printing. Specific monomers and functional monomers are selected, combined with UV curing and corona treatment, to achieve fast and firm adhesion and precise alignment. Its excellent 180° peel strength and low residual adhesive rate greatly simplify cleaning work, improve efficiency, reduce defects, ensure the quality of printed products, and meet high-end printing standards.

Claims

1. A method for preparing a screen printing alignment film, characterized in that: The steps include: Step 1: Apply the screen printing alignment film evenly to the PE film with pressure-sensitive adhesive; Step 2: UV curing; Step 3: corona treatment; The pressure-sensitive adhesive for screen printing alignment film is prepared from the following raw materials in parts by weight using a conventional method; 10-20 parts of methyl methacrylate; 10-20 parts of vinyl acetate; Epoxy acrylate 20-25 parts; 2-Ethylhexyl acrylate 15-25 parts; 2-isocyanatoethyl acrylate 10-15 parts; 10-15 parts of hydroxyethyl methacrylate; 1-2 parts of azobisisobutyronitrile; 80-120 parts of ethyl acetate; 2-8 parts of mercaptan chain transfer agent.

2. The method for preparing the screen printing alignment film according to claim 1, characterized in that: The steps include: Step 1: Apply the screen printing alignment film evenly to the PE film with pressure-sensitive adhesive, with a coating amount of 10-50g / m 2 ; Step 2: Expose the film to UV light for 30-60 seconds with a light energy of 200-600mJ / cm 2 ; Step 3: corona treatment, with a treatment voltage of 10000-20000V and a treatment time of 10-30 seconds, to prepare the screen printing alignment film.

3. The method for preparing the screen printing alignment film according to claim 2, characterized in that: The mercaptan-based chain transfer agent is at least one of n-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, 1,10-decandithiolan and dipropyltrimercaptan.

4. The method for preparing the screen printing alignment film according to claim 3, characterized in that: The pressure-sensitive adhesive for the silk-screen alignment film is prepared by the following method: Methyl methacrylate, vinyl acetate, epoxy acrylate, 2-ethylhexyl acrylate, 2-isocyanoethyl acrylate, hydroxyethyl methacrylate, part of azobisisobutyronitrile, part of ethyl acetate and a thiol chain transfer agent are mixed uniformly to obtain a mixed solution A; dissolving the remaining azobisisobutyronitrile in the remaining ethyl acetate to obtain a mixed solution B; Under nitrogen atmosphere, the mixed solution B was uniformly added dropwise to the mixed solution A, and the mixture was stirred for reaction for 2-6 hours.

5. The method for preparing the screen printing alignment film according to claim 4, characterized in that: The pressure-sensitive adhesive for the silk-screen alignment film is prepared by the following method: Methyl methacrylate, vinyl acetate, epoxy acrylate, 2-ethylhexyl acrylate, 2-isocyanatoethyl acrylate, hydroxyethyl methacrylate, 40-80 wt % of azobisisobutyronitrile, 30-70 wt % of ethyl acetate and a thiol chain transfer agent are uniformly mixed to obtain a mixed solution A; dissolving the remaining azobisisobutyronitrile in the remaining ethyl acetate to obtain a mixed solution B; Under nitrogen atmosphere, the mixed solution A is heated to 70-78° C., and the mixed solution B is added dropwise to the mixed solution A at a uniform rate of 1-5 drops / second. After the addition is completed, the mixture is stirred at 40-100 rpm for 2-6 hours.

6. A screen printing alignment film, characterized in that: The method is prepared by any one of claims 1 to 5.