Composite material for promoting periosteum repair and preparation method thereof
The modified polycaprolactone/hydroxyapatite-Ag composite fiber membrane was prepared by electrospinning technology and combined with bioactive glass and modified chitosan, which solved the problem of mismatch between the degradation rate of periosteal repair materials and the formation of bone tissue. It achieves the activation of bone cells and bone regeneration, provides strength and antibacterial effect, and is suitable for the repair of complex anatomical structures.
Patent Information
- Application Number
- CN202410891210.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The existing periosteal repair materials suffer from a mismatch between the degradation rate and the formation rate of new bone tissue, resulting in poor bone regeneration and difficulty in providing sufficient initial strength and flexibility to adapt to complex anatomical structures.
A composite ultrafine fiber membrane of modified polycaprolactone and hydroxyapatite nanoparticles surface-modified and grafted with metal ions Ag was prepared by electrospinning technology, and carboxylated-modified chitosan was cross-linked on its surface. and bioactive glass to form a hierarchical structure composite material, ensuring stable loading and uniform distribution of metal ions, and enhancing the bioactivity and mechanical properties of the material.
It achieves the maturation and mineralization of bone cells, promotes bone regeneration, provides good antibacterial effects and biodegradability, and at the same time improves the strength and toughness of the material, making it suitable for the repair of complex anatomical structures.
Smart Images

Figure CN118403220B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tissue repair materials, and in particular relates to a composite material for promoting periosteum repair and a preparation method thereof. Background Art
[0002] Periosteum, as the connective tissue wrapping the outer layer of bones, plays an indispensable role in the growth, repair and maintenance of bones. When the periosteum is damaged by trauma, surgery or disease, the bone regeneration ability will be significantly reduced, which may lead to delayed or incomplete healing. Periosteum repair materials have emerged to simulate and promote the recovery of natural periosteum function and accelerate the bone tissue repair process. Such materials are usually composed of biocompatible materials, such as natural or synthetic polymers, inorganic minerals, or a composite of these materials, designed to provide temporary structural support while inducing the proliferation and differentiation of bone cells and promoting new bone formation.
[0003] Current periosteum repair material technology covers a variety of innovative solutions, mainly including bio-derived materials: such as collagen membranes, which use animal-derived collagen to simulate the biological properties of natural periosteum, provide a matrix for cell adhesion, and promote cell growth; inorganic bioactive materials: such as membranes or particles made of hydroxyapatite (HA) and tricalcium phosphate (TCP), which can directly participate in the formation of bone minerals and provide bone conduction; composite materials: combining organic (such as polymers) and inorganic (such as HA) components to optimize mechanical properties and bioactivity, such as a double-layer mineralized collagen membrane, which provides a barrier with pure collagen facing the muscle side and mineralized collagen facing the bone defect side to promote osteogenesis; functional materials: such as sustained-release materials containing growth factors (such as BMPs), or bionic periosteum that can regulate the immune-neurovascular microenvironment, which accelerate bone regeneration by releasing bioactive molecules or improving the local microenvironment. Although the technology of periosteal repair materials has made significant progress, it still faces a series of problems: the degradation rate of biomaterials needs to match the speed of new bone tissue formation. Too fast or too slow will affect the repair effect. The repair material needs to provide sufficient initial strength to support the damaged area while maintaining a certain flexibility to adapt to complex anatomical structures. Based on the above problems, it is extremely necessary to develop a composite material that promotes periosteal repair with good biocompatibility, strong degradability and sufficient strength. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a composite material for promoting periosteum repair and a preparation method thereof. By means of electrospinning technology, a mixed solution of modified polycaprolactone and hydroxyapatite nanoparticles that have been surface-modified and grafted with metal ions Ag is directly spun to form a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane with a porous structure, thereby ensuring the stable loading and uniform distribution of Ag in the fiber network; then, utilizing the porous structure of the ultrafine fiber membrane, the activity of the material is further enhanced by embedding bioactive glass; finally, carboxyl-modified chitosan is cross-linked on the surface of the modified polycaprolactone ultrafine fiber membrane to form a hierarchical structure.
[0005] The technical effect described in the present invention is achieved through the following technical scheme: a composite material for promoting periosteum repair, consisting of a matrix support layer and a functional coating, wherein the matrix support layer is a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane, which is composed of modified polycaprolactone and hydroxyapatite nanoparticles grafted with Ag metal ions; the functional coating is composed of bioactive glass and modified chitosan.
[0006] A method for preparing a composite material for promoting periosteum repair, specifically comprising the following steps:
[0007] S1: Preparation of modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane; modified polycaprolactone was combined with Ag-grafted hydroxyapatite nanoparticles using electrospinning technology;
[0008] S2: Preparation of modified chitosan; Preparation of carboxymethylated modified chitosan using chloroacetic acid method;
[0009] S3: adding the bioactive glass to a PBS buffer solution with a pH of 7.4, treating it with ultrasonic oscillation at a frequency of 20 to 50 kHz for 15 to 60 minutes, filtering it with a 0.45 μm microporous membrane, adding 0.2 wt % of Tween-80, mixing it evenly, and obtaining a suspension;
[0010] S4: Gently wash the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in step S1 with deionized water, then spread it flat in a container, slowly add the suspension prepared in step S3, immerse for 6 to 12 hours, and after the immersion, vacuum dry at 50° C. to obtain an embedded composite fiber membrane;
[0011] S5: dissolving the modified chitosan prepared in step S2 into deionized water, stirring evenly, adding 0.1 M NaOH solution to adjust the pH to 8-9, and then adding 0.3 wt % glutaraldehyde to obtain a modified chitosan solution;
[0012] S6: Coat the modified chitosan solution prepared in step S5 onto the embedded composite fiber membrane prepared in step S4 with a coating thickness of 10 to 50 μm, then place the coated embedded composite fiber membrane in a constant temperature and humidity chamber with a set temperature of 30 to 40°C and a humidity of 50 to 80%. After reacting for 4 to 8 hours, repeat the above coating and drying operations to coat and dry the second side. After all coating reactions are completed, wash with deionized water and dry in vacuo at 35°C to obtain a composite material.
[0013] Preferably, the preparation steps of the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane in step S1 are as follows:
[0014] A1: Hydroxyapatite nanoparticles were dispersed in 50 times the mass volume of deionized water, ultrasonically dispersed evenly, a coupling agent was added, stirred at 4-10°C for 1-2 hours, and then 1wt% succinimide solution was slowly added dropwise within 10 minutes, and the reaction was continued at 4-10°C with stirring for 1-2 hours, centrifuged, and the precipitate was taken, washed three times with deionized water, and vacuum freeze-dried to obtain modified hydroxyapatite nanoparticles;
[0015] A2: Dissolve polycaprolactone in dichloromethane, stir and mix evenly, add polyethylene glycol, dicyclohexylcarbodiimide and 4-dimethylaminopyridine under nitrogen protection, stir at 60-70°C for 8-12h, centrifuge, filter, wash with deionized water, and dry in vacuum at 60°C to obtain modified polycaprolactone;
[0016] A3: The modified hydroxyapatite nanoparticles prepared in step A1 are dispersed in 30 to 50 times the mass volume of deionized water, subjected to 30W ultrasonic treatment for 15 to 30 minutes, and then a 0.1M AgNO3 solution is slowly added dropwise, and stirring is continued for 5 to 10 minutes. Then, in an ice bath, a 0.2M NaBH4 solution is slowly added dropwise, and stirring is continued for 1 to 2 hours. After the reaction is completed, centrifugation is performed, and the precipitate is taken, washed three times with deionized water, and vacuum dried at 60°C to obtain a modified hydroxyapatite-Ag composite material;
[0017] A4: After uniformly mixing the modified polycaprolactone and polyvinyl pyrrolidone prepared in step A2, slowly add dichloromethane, heat in a water bath to control the temperature at 60-70°C, and continue stirring until the solution is transparent; then slowly add the modified hydroxyapatite-Ag composite material prepared in step A3, control the temperature at 40-60°C, continue stirring to react for 30-60 minutes, and after the reaction is completed, quickly cool to room temperature in an ice bath, filter with a 0.22 μm filter membrane, and obtain a composite spinning solution;
[0018] A5: The composite spinning solution prepared in step A4 is transferred to a syringe and electrospinning is performed at room temperature. The parameter voltage is set to 5-15 kV, the solution propulsion speed is set to 200-500 μL / min, and the receiving distance is set to 10-30 cm to obtain a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane.
[0019] Preferably, the coupling agent described in step A1 is 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide prepared in a mass ratio of 1.5:1; the usage ratio of the hydroxyapatite nanoparticles, the coupling agent and the succinimide solution is 1g:10-20mg:2mL.
[0020] Preferably, the ratio of the amount of polycaprolactone, dichloromethane, polyethylene glycol, dicyclohexylcarbodiimide and 4-dimethylaminopyridine used in step A2 is 1 g:10 mL:0.3-0.5 g:5-10 mg:1 mg.
[0021] Preferably, all operations after the dropwise addition of the AgNO3 solution in step A3 are performed under nitrogen protection, and the ratio of the amount of the modified hydroxyapatite nanoparticles, the AgNO3 solution and the NaBH4 solution is 1 g: 1-1.5 mL: 1 mL.
[0022] Preferably, in step A4, the ratio of the amount of the modified polycaprolactone, polyvinyl pyrrolidone, dichloromethane and the modified hydroxyapatite-Ag composite material is 1 g: 0.15-0.25 g: 5 mL: 0.2-0.5 g.
[0023] Preferably, the preparation steps of the modified chitosan in step S2 are as follows:
[0024] B1: Add chitosan powder to 0.5wt% acetic acid solution, stir and mix evenly at room temperature, filter, and centrifuge to obtain a 3wt% pretreated chitosan solution;
[0025] B2: Slowly add chloroacetic acid to the pretreated chitosan solution prepared in step B1, and control the pH to 4-6 with glacial acetic acid, heat in a water bath to 50-60°C, react for 2-6 hours, adjust the NaOH solution to neutral, cool naturally to room temperature, dialyze at 30 kDa, centrifuge, take the precipitate, wash with anhydrous ethanol, and vacuum freeze-dry to obtain modified chitosan.
[0026] Preferably, the ratio of the amount of chloroacetic acid to the pretreated chitosan solution in step B2 is 1.5-3 g:100 mL.
[0027] Preferably, the diameter of the bioactive glass in step S3 is 50 μm; the ratio of the amount of the bioactive glass to the amount of PBS buffer is 1-3 g:100 mL.
[0028] Preferably, the ratio of the modified chitosan and deionized water used in step S5 is 2-5 g:100 mL.
[0029] Preferably, the coating operation in step S6 is double-sided coating, and the coating and drying are performed on the second side after the coating and drying on the first side.
[0030] The beneficial effects of the present invention are as follows:
[0031] The present invention introduces an active group carboxyl (-COOH) by surface modification of hydroxyapatite nanoparticles to provide specific reaction sites for the coordination and binding of Ag metal ions. Then, Ag metal ions are grafted onto the active groups on the surface of hydroxyapatite nanoparticles by chemical reaction (coordination reaction) to form a stable chemical bond connection. After hydroxyapatite is grafted with Ag, the metal ions not only enhance the antibacterial properties of the material, but also further promote the deposition of bone minerals through ion exchange, and synergize with the porous structure of polycaprolactone fiber membrane to jointly promote the maturation and mineralization process of bone cells. Hydroxyapatite nanoparticles can promote the recognition and adhesion of bone cells due to their similarity to bone tissue components, thereby activating the signal pathways in the cells and promoting the expression of genes related to bone formation. The local release of Ag is crucial in controlling infection. It can effectively inhibit the growth of various bacteria and create a sterile environment that is conducive to tissue healing. In addition, the appropriate amount of Ag release can also indirectly promote the recruitment and activation of cells in the early stages of bone regeneration by stimulating inflammatory reactions. The hydroxyapatite nanoparticles grafted with metal ions were mixed into the polycaprolactone solution, and the fiber membrane was prepared together by electrospinning technology to ensure the stable existence of metal ions in the polycaprolactone fiber network. The porous structure of the polycaprolactone fiber membrane provides sufficient growth space for cells, laying the foundation for the initial adhesion and subsequent proliferation of bone cells. At the same time, by grafting hydrophilic polyethylene glycol, the hydrophilicity of polycaprolactone can be significantly improved, promoting cell adhesion and proliferation. The introduction of polyethylene glycol also helps the degradation of the material.
[0032] The introduction of carboxylated chitosan promotes the formation of extracellular matrix through its carboxyl group to enhance the hydrophilicity and wettability of the material, complements the hydrophobicity of polycaprolactone, and promotes cell adhesion, migration and differentiation. The Ca and P ions released by the bioactive glass can react with the carboxyl groups on the carboxylated chitosan to form a mineralization environment similar to the natural bone matrix, promoting the mineralization process of bone cells. The high hydrophilicity of carboxylated chitosan helps the rapid diffusion and effective utilization of bioactive glass ions, enhancing the biological activity of the material. In addition, the negative charge of carboxylated chitosan and the positive charge of Ag can form an electrostatic interaction, which helps to stabilize the distribution of Ag in the material, prevent its premature or uneven release, and achieve a lasting antibacterial effect. Modified chitosan not only enhances the hydrophilicity and cell adhesion of the material surface, but also promotes the stable attachment and efficient utilization of bioactive molecules. By utilizing its excellent biocompatibility and degradability, it complements polycaprolactone and hydroxyapatite nanoparticles, promotes the close integration of cells and materials, accelerates periosteum repair, and promotes the orderly arrangement of the extracellular matrix, thereby enhancing the mechanical stability of the interface and improving the overall strength and toughness of the composite material.
[0033] The addition of hydroxyapatite nanoparticles not only provides biological activity and promotes bone integration, but also, because hydroxyapatite is similar to the main inorganic components of bone matrix, they can be embedded in the polycaprolactone matrix as a reinforcing phase to form microscopic "reinforcement points", that is, under pressure, these dispersed hydroxyapatite particles can effectively disperse stress and enhance the hardness and compressive strength of the material; in addition, nanoscale particles can effectively hinder crack propagation, thereby improving the toughness of the material. Carboxylated chitosan has good biocompatibility and degradability, which complements the biodegradable properties of polycaprolactone, and together they build a gradually degradable repair environment, which is conducive to the regeneration of bone tissue. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 It is a cell culture test diagram of the composite materials prepared in Examples 1 to 4 of the present invention and Comparative Examples 1 to 4;
[0036] Figure 2 is a SEM scanning electron microscope image of the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in Example 2 of the present invention;
[0037] Figure 3is the FTIR infrared spectrum of the composite material prepared in Example 2 of the present invention;
[0038] Figure 4 is a graph of biodegradability of the composite materials prepared in Examples 2 and 3 of the present invention and Comparative Examples 1 to 4;
[0039] Figure 5 It is an antibacterial test diagram of the composite materials prepared in Examples 2 and 3 of the present invention and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. It should be noted that, unless otherwise specified, the raw materials involved in the present invention are purchased through conventional commercial channels.
[0041] Example 1: A composite material for promoting periosteum repair, consisting of a matrix support layer and a functional coating, wherein the matrix support layer is a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane, which is composed of modified polycaprolactone and hydroxyapatite nanoparticles grafted with Ag metal ions; the functional coating is composed of bioactive glass and modified chitosan.
[0042] A method for preparing a composite material for promoting periosteum repair, specifically comprising the following preparation steps:
[0043] S1: Preparation of modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane:
[0044] A1: 10 g of hydroxyapatite nanoparticles were dispersed in 500 mL of deionized water, and ultrasonically dispersed uniformly. 100 mg of a coupling agent prepared by 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in a mass ratio of 1.5:1 was added, and stirred at 4°C for 2 h. Then, 20 mL of a 1 wt% succinimide solution was slowly added dropwise within 10 min. The above stirring temperature was maintained, and the stirring reaction was continued for 1 h. The mixture was centrifuged, and the precipitate was taken, washed three times with deionized water, and vacuum freeze-dried to obtain modified hydroxyapatite nanoparticles.
[0045] A2: Dissolve 10 g of polycaprolactone in 100 mL of dichloromethane, stir and mix well, add 3 g of polyethylene glycol, 50 mg of dicyclohexylcarbodiimide and 10 mg of 4-dimethylaminopyridine under nitrogen protection, stir at 60 ° C for 12 h, centrifuge, filter, wash with deionized water, and dry in vacuo at 60 ° C to obtain modified polycaprolactone;
[0046] A3: 10 g of modified hydroxyapatite nanoparticles prepared in step A1 were dispersed in 300 mL of deionized water, subjected to 30 W ultrasonic treatment for 15 min, and then 10 mL of 0.1 M AgNO3 solution was slowly added dropwise, and stirring was continued for 5 min. Then, 10 mL of 0.2 M NaBH4 solution was slowly added dropwise under ice bath conditions, and stirring was continued for 1 h. After the reaction was completed, centrifugation was performed, and the precipitate was taken, washed three times with deionized water, and vacuum dried at 60 ° C to obtain a modified hydroxyapatite-Ag composite material;
[0047] A4: After uniformly mixing 10 g of modified polycaprolactone and 1.5 g of polyvinyl pyrrolidone prepared in step A2, slowly add 50 mL of dichloromethane, heat in a water bath to control the temperature at 60°C, and continue stirring until the solution is transparent; then slowly add 2 g of modified hydroxyapatite-Ag composite material prepared in step A3, control the temperature at 40°C, continue stirring and react for 60 min, and after the reaction is completed, quickly cool to room temperature in an ice bath, filter with a 0.22 μm filter membrane, and obtain a composite spinning solution;
[0048] A5: The composite spinning solution prepared in step A4 was transferred into a syringe, and electrospinning was performed at room temperature, with the parameter voltage set to 5 kV, the solution advancing speed to 200 μL / min, and the receiving distance to 10 cm, to obtain a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane;
[0049] S2: Preparation of modified chitosan:
[0050] B1: Add chitosan powder to 0.5wt% acetic acid solution, stir and mix evenly at room temperature, filter, and centrifuge to obtain a 3wt% pretreated chitosan solution;
[0051] B2: Slowly add 7.5 g of chloroacetic acid to 500 mL of the pretreated chitosan solution prepared in step B1, and control the pH to 6 with glacial acetic acid, heat to 50°C in a water bath, react for 6 h, adjust the solution to neutral with NaOH, cool naturally to room temperature, dialyze at 30 kDa, centrifuge, take the precipitate, wash with anhydrous ethanol, and freeze-dry in vacuum to obtain modified chitosan;
[0052] S3: 5 g of bioactive glass with a diameter of 50 μm was added to 500 mL of PBS buffer with a pH of 7.4, and the mixture was treated with ultrasonic oscillation at a frequency of 20 kHz for 60 min, filtered through a 0.45 μm microporous membrane, and 1 g of Tween-80 was added and mixed to obtain a suspension;
[0053] S4: 5 g of the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in step S1 was gently washed with deionized water, then spread flat in a container, 500 mL of the suspension prepared in step S3 was slowly added, and immersed for 6 h. After the immersion, vacuum dried at 50° C. to obtain an embedded composite fiber membrane;
[0054] S5: dissolving 10 g of the modified chitosan prepared in step S2 into 500 mL of deionized water, stirring evenly, adding 0.1 M NaOH solution to adjust the pH to 8, and then adding 1.5 g of glutaraldehyde, mixing evenly, to obtain a modified chitosan solution;
[0055] S6: Coat the modified chitosan solution prepared in step S5 onto the embedded composite fiber membrane prepared in step S4 with a coating thickness of 10 μm, then place the coated embedded composite fiber membrane in a constant temperature and humidity chamber, set the temperature to 30°C and the humidity to 50%, react for 8 hours, repeat the above operation to perform double-sided coating, and after all coating reactions are completed, wash with deionized water, and vacuum dry at 35°C to obtain a composite material.
[0056] Example 2: A composite material for promoting periosteum repair, consisting of a matrix support layer and a functional coating, wherein the matrix support layer is a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane, composed of modified polycaprolactone and hydroxyapatite nanoparticles grafted with Ag metal ions; the functional coating is composed of bioactive glass and modified chitosan.
[0057] A method for preparing a composite material for promoting periosteum repair, specifically comprising the following preparation steps:
[0058] S1: Preparation of modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane:
[0059] A1: 10 g of hydroxyapatite nanoparticles were dispersed in 500 mL of deionized water, and ultrasonically dispersed uniformly. 170 mg of a coupling agent prepared by 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in a mass ratio of 1.5:1 was added, and stirred at 10°C for 1.5 h. Then, 20 mL of a 1 wt% succinimide solution was slowly added dropwise within 10 min. The above stirring temperature was maintained, and the reaction was stirred for 2 h. The mixture was centrifuged, and the precipitate was taken, washed three times with deionized water, and vacuum freeze-dried to obtain modified hydroxyapatite nanoparticles.
[0060] A2: Dissolve 10 g of polycaprolactone in 100 mL of dichloromethane, stir and mix well, add 4.5 g of polyethylene glycol, 80 mg of dicyclohexylcarbodiimide and 10 mg of 4-dimethylaminopyridine under nitrogen protection, stir at 65 ° C for 10 h, centrifuge, filter, wash with deionized water, and dry in vacuo at 60 ° C to obtain modified polycaprolactone;
[0061] A3: 10 g of modified hydroxyapatite nanoparticles prepared in step A1 were dispersed in 400 mL of deionized water, subjected to 30 W ultrasonic treatment for 25 min, and then 14 mL of 0.1 M AgNO3 solution was slowly added dropwise, and stirring was continued for 8 min. Then, 10 mL of 0.2 M NaBH4 solution was slowly added dropwise under ice bath conditions, and stirring was continued for 1.5 h. After the reaction was completed, centrifugation was performed, and the precipitate was taken, washed three times with deionized water, and vacuum dried at 60 ° C to obtain a modified hydroxyapatite-Ag composite material;
[0062] A4: After uniformly mixing 10 g of modified polycaprolactone and 2.2 g of polyvinyl pyrrolidone prepared in step A2, slowly add 50 mL of dichloromethane, heat in a water bath to control the temperature at 65°C, and continue stirring until the solution is transparent; then slowly add 4 g of modified hydroxyapatite-Ag composite material prepared in step A3, control the temperature at 50°C, continue stirring and react for 45 minutes, and after the reaction is completed, quickly cool to room temperature in an ice bath, filter with a 0.22 μm filter membrane, and obtain a composite spinning solution;
[0063] A5: The composite spinning solution prepared in step A4 was transferred into a syringe, and electrospinning was performed at room temperature, with the parameter voltage set to 12 kV, the solution advancing speed to 300 μL / min, and the receiving distance to 20 cm, to obtain a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane;
[0064] S2: Preparation of modified chitosan:
[0065] B1: Add chitosan powder to 0.5wt% acetic acid solution, stir and mix evenly at room temperature, filter, and centrifuge to obtain a 3wt% pretreated chitosan solution;
[0066] B2: Slowly add 12 g of chloroacetic acid to 500 mL of the pretreated chitosan solution prepared in step B1, and control the pH to 4.5 with glacial acetic acid, heat to 55°C in a water bath, react for 4 h, adjust the solution to neutral with NaOH, cool naturally to room temperature, dialyze at 30 kDa, centrifuge, take the precipitate, wash with anhydrous ethanol, and freeze-dry in vacuum to obtain modified chitosan;
[0067] S3: 12 g of bioactive glass with a diameter of 50 μm was added to 500 mL of PBS buffer with a pH of 7.4, and ultrasonically vibrated for 30 min at a frequency of 40 kHz, filtered through a 0.45 μm microporous membrane, and 1 g of Tween-80 was added, mixed evenly, and a suspension was obtained;
[0068] S4: Gently wash the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in step S1 with deionized water, then spread it flat in a container, slowly add the suspension prepared in step S3, immerse for 10 hours, and after the immersion, vacuum dry at 50° C. to obtain an embedded composite fiber membrane;
[0069] S5: dissolving 20 g of the modified chitosan prepared in step S2 into 500 mL of deionized water, stirring evenly, adding 0.1 M NaOH solution to adjust the pH to 8.5, and then adding 1.5 g of glutaraldehyde, mixing evenly, to obtain a modified chitosan solution;
[0070] S6: Coat the modified chitosan solution prepared in step S5 onto the embedded composite fiber membrane prepared in step S4 with a coating thickness of 25 μm, then place the coated embedded composite fiber membrane in a constant temperature and humidity chamber with the temperature set to 37°C and the humidity set to 60%. After reacting for 5 hours, repeat the above operation to perform double-sided coating. After all coating reactions are completed, wash with deionized water and dry in vacuo at 35°C to obtain a composite material.
[0071] Example 3: A composite material for promoting periosteum repair, consisting of a matrix support layer and a functional coating, wherein the matrix support layer is a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane, composed of modified polycaprolactone and hydroxyapatite nanoparticles grafted with Ag metal ions; the functional coating is composed of bioactive glass and modified chitosan.
[0072] A method for preparing a composite material for promoting periosteum repair, specifically comprising the following preparation steps:
[0073] S1: Preparation of modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane:
[0074] A1: 10 g of hydroxyapatite nanoparticles were dispersed in 500 mL of deionized water, and ultrasonically dispersed uniformly. 140 mg of a coupling agent prepared by 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in a mass ratio of 1.5:1 was added, and stirred at 6°C for 2 h. Then, 20 mL of a 1 wt% succinimide solution was slowly added dropwise within 10 min. The above stirring temperature was maintained, and the stirring reaction was continued for 1.5 h. The mixture was centrifuged, and the precipitate was taken, washed three times with deionized water, and vacuum freeze-dried to obtain modified hydroxyapatite nanoparticles.
[0075] A2: Dissolve 10 g of polycaprolactone in 100 mL of dichloromethane, stir and mix well, add 4 g of polyethylene glycol, 70 mg of dicyclohexylcarbodiimide and 10 mg of 4-dimethylaminopyridine under nitrogen protection, stir at 62 ° C for 11 h, centrifuge, filter, wash with deionized water, and dry in vacuo at 60 ° C to obtain modified polycaprolactone;
[0076] A3: 10 g of modified hydroxyapatite nanoparticles prepared in step A1 were dispersed in 450 mL of deionized water, subjected to 30 W ultrasonic treatment for 25 min, and then 12 mL of 0.1 M AgNO3 solution was slowly added dropwise, and stirring was continued for 8 min. Then, 10 mL of 0.2 M NaBH4 solution was slowly added dropwise under ice bath conditions, and stirring was continued for 1.5 h. After the reaction was completed, centrifugation was performed, and the precipitate was taken, washed three times with deionized water, and vacuum dried at 60 ° C to obtain a modified hydroxyapatite-Ag composite material;
[0077] A4: After uniformly mixing 10 g of modified polycaprolactone and 1.8 g of polyvinyl pyrrolidone prepared in step A2, slowly add 50 mL of dichloromethane, heat in a water bath to control the temperature at 65°C, and continue stirring until the solution is transparent; then slowly add 3.5 g of modified hydroxyapatite-Ag composite material prepared in step A3, control the temperature at 55°C, continue stirring and react for 40 minutes, and after the reaction is completed, quickly cool to room temperature in an ice bath, filter with a 0.22 μm filter membrane, and obtain a composite spinning solution;
[0078] A5: The composite spinning solution prepared in step A4 was transferred into a syringe, and electrospinning was performed at room temperature, with the parameter voltage set to 10 kV, the solution propulsion speed to 400 μL / min, and the receiving distance to 25 cm, to obtain a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane;
[0079] S2: Preparation of modified chitosan:
[0080] B1: Add chitosan powder to 0.5wt% acetic acid solution, stir and mix evenly at room temperature, filter, and centrifuge to obtain a 3wt% pretreated chitosan solution;
[0081] B2: Slowly add 10 g of chloroacetic acid to 500 mL of the pretreated chitosan solution prepared in step B1, and use glacial acetic acid to control the pH to 5, heat in a water bath to 54°C, react for 5 h, adjust the solution to neutral with NaOH, cool naturally to room temperature, dialyze at 30 kDa, centrifuge, take the precipitate, wash with anhydrous ethanol, and freeze-dry in vacuum to obtain modified chitosan;
[0082] S3: 10 g of bioactive glass with a diameter of 50 μm was added to 500 mL of PBS buffer with a pH of 7.4, and treated with ultrasonic oscillation at a frequency of 40 kHz for 25 min, filtered with a 0.45 μm microporous membrane, and 1 g of Tween-80 was added, mixed evenly, and a suspension was obtained;
[0083] S4: Gently wash the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in step S1 with deionized water, then spread it flat in a container, slowly add the suspension prepared in step S3, immerse for 8 hours, and after the immersion, vacuum dry at 50° C. to obtain an embedded composite fiber membrane;
[0084] S5: dissolving 15 g of the modified chitosan prepared in step S2 into 500 mL of deionized water, stirring evenly, adding 0.1 M NaOH solution to adjust the pH to 8, and then adding 1.5 g of glutaraldehyde, mixing evenly, to obtain a modified chitosan solution;
[0085] S6: Coat the modified chitosan solution prepared in step S5 onto the embedded composite fiber membrane prepared in step S4 with a coating thickness of 40 μm, then place the coated embedded composite fiber membrane in a constant temperature and humidity chamber, set the temperature to 35°C and the humidity to 70%, react for 5 hours, repeat the above operation to perform double-sided coating, and after all coating reactions are completed, wash with deionized water, and vacuum dry at 35°C to obtain a composite material.
[0086] Example 4: A composite material for promoting periosteum repair, consisting of a matrix support layer and a functional coating, wherein the matrix support layer is a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane, composed of modified polycaprolactone and hydroxyapatite nanoparticles grafted with Ag metal ions; the functional coating is composed of bioactive glass and modified chitosan.
[0087] A method for preparing a composite material for promoting periosteum repair, specifically comprising the following preparation steps:
[0088] S1: Preparation of modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane:
[0089] A1: 10 g of hydroxyapatite nanoparticles were dispersed in 500 mL of deionized water, and ultrasonically dispersed uniformly. 200 mg of a coupling agent prepared by 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in a mass ratio of 1.5:1 was added, and stirred at 10°C for 1 h. Then, 20 mL of a 1 wt% succinimide solution was slowly added dropwise within 10 min. The above stirring temperature was maintained, and the reaction was stirred for 2 h. The mixture was centrifuged, and the precipitate was taken, washed three times with deionized water, and vacuum freeze-dried to obtain modified hydroxyapatite nanoparticles.
[0090] A2: Dissolve 10 g of polycaprolactone in 100 mL of dichloromethane, stir and mix well, add 5 g of polyethylene glycol, 100 mg of dicyclohexylcarbodiimide and 10 mg of 4-dimethylaminopyridine under nitrogen protection, stir at 70 ° C for 12 h, centrifuge, filter, wash with deionized water, and dry in vacuo at 60 ° C to obtain modified polycaprolactone;
[0091] A3: 10 g of modified hydroxyapatite nanoparticles prepared in step A1 were dispersed in 500 mL of deionized water, subjected to 30 W ultrasonic treatment for 30 min, and then 15 mL of 0.1 M AgNO3 solution was slowly added dropwise, and stirring was continued for 10 min. Then, 10 mL of 0.2 M NaBH4 solution was slowly added dropwise under ice bath conditions, and stirring was continued for 2 h. After the reaction was completed, centrifugation was performed, and the precipitate was taken, washed three times with deionized water, and vacuum dried at 60 ° C to obtain a modified hydroxyapatite-Ag composite material;
[0092] A4: After uniformly mixing 10 g of modified polycaprolactone and 2.5 g of polyvinyl pyrrolidone prepared in step A2, slowly add 50 mL of dichloromethane, heat in a water bath to control the temperature to 70°C, and continue stirring until the solution is transparent; then slowly add 5 g of modified hydroxyapatite-Ag composite material prepared in step A3, control the temperature to 60°C, continue stirring and react for 30 minutes, and after the reaction is completed, quickly cool to room temperature in an ice bath, filter with a 0.22 μm filter membrane, and obtain a composite spinning solution;
[0093] A5: The composite spinning solution prepared in step A4 was transferred into a syringe, and electrospinning was performed at room temperature, with the parameter voltage set to 15 kV, the solution propulsion speed to 500 μL / min, and the receiving distance to 30 cm, to obtain a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane;
[0094] S2: Preparation of modified chitosan:
[0095] B1: Add chitosan powder to 0.5wt% acetic acid solution, stir and mix evenly at room temperature, filter, and centrifuge to obtain a 3wt% pretreated chitosan solution;
[0096] B2: Slowly add 15 g of chloroacetic acid to 500 mL of the pretreated chitosan solution prepared in step B1, and control the pH to 4 with glacial acetic acid, heat to 60°C in a water bath, react for 2 h, adjust the solution to neutral with NaOH, cool naturally to room temperature, dialyze at 30 kDa, centrifuge, take the precipitate, wash with anhydrous ethanol, and freeze-dry in vacuum to obtain modified chitosan;
[0097] S3: 15 g of bioactive glass with a diameter of 50 μm was added to 500 mL of PBS buffer with a pH of 7.4, and ultrasonically vibrated at a frequency of 50 kHz for 15 min, filtered through a 0.45 μm microporous membrane, and 1 g of Tween-80 was added, mixed evenly, and a suspension was obtained;
[0098] S4: Gently wash the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in step S1 with deionized water, then spread it flat in a container, slowly add the suspension prepared in step S3, immerse for 12 hours, and after the immersion, vacuum dry at 50° C. to obtain an embedded composite fiber membrane;
[0099] S5: dissolving 15 g of the modified chitosan prepared in step S2 into 500 mL of deionized water, stirring evenly, adding 0.1 M NaOH solution to adjust the pH to 9, and then adding 1.5 g of glutaraldehyde, mixing evenly, to obtain a modified chitosan solution;
[0100] S6: Coat the modified chitosan solution prepared in step S5 onto the embedded composite fiber membrane prepared in step S4 with a coating thickness of 50 μm, then place the coated embedded composite fiber membrane in a constant temperature and humidity chamber with the temperature set to 40°C and the humidity set to 80%. After reacting for 4 hours, repeat the above operation to perform double-sided coating. After all coating reactions are completed, wash with deionized water and dry in vacuo at 35°C to obtain a composite material.
[0101] Comparative Example 1: The operation of Comparative Example 1 is basically the same as that of Example 2, except that chitosan is used in place of modified chitosan for the final coating in Comparative Example 1.
[0102] Comparative Example 2: The operation of Comparative Example 2 is basically the same as that of Example 2, except that Comparative Example 2 does not use bioactive glass for embedding.
[0103] Comparative Example 3: The operation of Comparative Example 3 is basically the same as that of Example 3, except that no Ag ions are grafted in Comparative Example 3.
[0104] Comparative Example 4: The operation of Comparative Example 4 is basically the same as that of Example 3, except that Comparative Example 4 does not use the hydroxyapatite part, but directly uses modified polycaprolactone for spinning operation.
[0105] Performance Test:
[0106] Cell culture test: The composite material samples for periosteum repair prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were cut and placed at the bottom of the culture plate, and 8 wells per group of samples were evenly distributed in a 96-well plate. 50 μL of DMEM medium was added to each well, and then mouse bone marrow mesenchymal stem cells were diluted to 1×10 4 / mL and then inoculate 50 μL in the wells added with samples. At the same time, 8 wells without samples were used as negative control groups, and 8 wells with bone marrow mesenchymal stem cell culture medium were used as positive control groups. The temperature was set at 37°C and the CO2 concentration was 5%. 5 μL of 5 mg / mL MTT solution was added after culturing for 24 h, 72 h, and 168 h, respectively. After further culturing for 4 h, the culture medium in the wells was aspirated, and 50 μL of dimethyl sulfoxide was added to the wells. The absorbance (OD value) was measured at 490 nm using a microplate reader, and the activity percentage was measured [cell survival rate (%) = (OD value of the embodiment - OD value of the negative control group) / (OD value of the positive control group - OD value of the negative control group) × 100%], blank control group: only containing culture medium and MTT solution; negative control group: untreated cells were used as control; each sample was processed and analyzed three times, and the results were averaged. The results are shown in Figure 1 shown.
[0107] Depend on Figure 1 The results show that the composite material for periosteum repair prepared by the present invention has excellent biological safety and has an excellent promoting effect on the growth activity of bone marrow mesenchymal stem cells; from the results of comparative example 1 and example 2, it can be seen that the cell activity is affected to a certain extent when chitosan replaces modified chitosan; from the results of comparative example 2 and example 2, it can be seen that the absence of bioactive glass significantly reduces the effectiveness of the material in promoting bone cell maturation and mineralization, and significantly affects the cell activity; from the results of comparative example 3 and example 3, it can be seen that the absence of Ag ions affects ion exchange and bone mineral deposition, and the cell activity is significantly affected; from the results of comparative example 3, comparative example 4 and example 3, it can be seen that the absence of hydroxyapatite seriously affects the bone inductivity and cell activity of the material, and the cell activity is most significantly affected.
[0108] Spectrum measurement: The spectrum of the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane sample prepared in Example 2 was tested using a scanning electron microscope. The results are as follows: Figure 2 The FTIR spectrometer tested the composite material sample spectrum as shown, and the results are as follows Figure 3 shown.
[0109] Depend on Figure 2 The results show that the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared by electrospinning is relatively uniform and has an elongated morphology. Obvious dots and particles are observed on the fiber, and hydroxyapatite and Ag are effectively deposited. Figure 3 The results show that at 1000-1100cm -1 The prominent peaks between 2800-2950 cm show the stretching vibrations of Si-O-Si and Si-OC chains in bioactive glass; -1 The peaks in between are the symmetric stretching vibrations of the methyl groups of polycaprolactone.
[0110] Biodegradability test: Three samples of the composite materials for periosteum repair prepared in Examples 2, 3 and Comparative Examples 1 to 4 were taken as samples, each sample was 1 g, and a total of 18 samples were added to 30 mL of PBS buffer with a pH of 7.4, placed in a constant temperature box at 42°C and a humidity of 55%, and samples were taken on the 1st, 3rd, 7th, and 14th days, and [biodegradation rate (%) = (initial weight - residual weight) / initial weight × 100%] was calculated. The results are as follows: Figure 4 shown.
[0111] Depend on Figure 4 The results show that the composite material for periosteum repair prepared by the present invention has good biodegradability, and can effectively achieve more than 50% efficient degradation after 14 days; from the results of Comparative Example 4 and Example 3, it can be seen that the biodegradability of the composite material is significantly affected by the lack of hydroxyapatite, and from the results of Comparative Example 2 and Example 2, it can be seen that the lack of bioactive glass also has a certain impact on biodegradability.
[0112] Antibacterial test: fresh bacterial suspensions of Staphylococcus aureus, Escherichia coli and Candida albicans were prepared at a concentration of 1×10 8 CFU / mL, add the composite material samples prepared in Examples 2 and 3 of the present invention and Comparative Examples 1 to 4 (0.1 g + 10 mL of deionized water) respectively, place the mixed bacterial solution in a constant temperature oscillator at 37°C for 48 h, record the total number of colonies in the bacterial solution by plate colony counting method, repeat the test 3 times, take the average value, take the bacterial solution without sample as the control (the strains used in this experiment are all purchased from the market), and calculate [antibacterial rate (%) = (1-the number of bacteria in the control sample / the number of bacteria in the experimental sample) × 100%], the results are as follows Figure 5 shown.
[0113] Depend on Figure 5 The results show that the composite material for periosteum repair prepared by the present invention has an excellent antibacterial effect. It can be seen from the results of Comparative Example 2 and Example 2 that the lack of Ag ions significantly affects the antibacterial performance. It can be seen from the results of Comparative Example 1, Comparative Example 3 and Example 2 that modified chitosan can effectively synergistically promote the antibacterial effect of Ag ions; it can be seen from the results of Comparative Example 4 and Example 3 that the antibacterial effect is significantly affected by the lack of hydroxyapatite and Ag ions.
[0114] Strength test: Tensile strength test: During the test, the samples of Examples 2, 3 and Comparative Examples 1 to 4 were installed on a universal material testing machine and stretched at a constant speed of 10 mm / min until they broke, and the maximum force (breaking strength) and the strain at break (elongation at break) were recorded; Compression strength test: During the test, axial pressure was applied to the composite material samples for periosteum repair prepared in Examples 2, 3 and Comparative Examples 1 to 4 until the samples were damaged, and the compressive strength and modulus were recorded. Each sample was tested three times and the average value was taken. The results are shown in the following table.
[0115] Table 1. Strength test results of composite materials.
[0116]
[0117] It can be seen from the results in Table 1 that the composite material for periosteum repair prepared by the present invention has excellent strength performance. It can be seen from the results of Comparative Example 4 and Example 3 that the lack of hydroxyapatite has the greatest impact on the strength of the composite material, among which the fracture strength and compression strength are significantly affected; it can be seen from the results of Comparative Example 1, Comparative Example 2 and Example 2 that modified chitosan and bioactive glass both effectively improve the strength of the composite material.
[0118] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a composite material for promoting periosteum repair, characterized in that: The composite material is composed of a matrix support layer and a functional coating, wherein the matrix support layer is a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane, which is composed of modified polycaprolactone and hydroxyapatite nanoparticles grafted with Ag metal ions; the functional coating is composed of bioactive glass and modified chitosan; The method for preparing the composite material for promoting periosteum repair specifically comprises the following steps: S1: Preparation of modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane; modified polycaprolactone was combined with Ag-grafted hydroxyapatite nanoparticles using electrospinning technology; S2: Preparation of modified chitosan; Preparation of carboxymethylated modified chitosan using chloroacetic acid method; S3: adding the bioactive glass to a PBS buffer solution with a pH of 7.4, subjecting the solution to ultrasonic oscillation, filtering the solution through a microporous membrane, adding Tween-80, and mixing the mixture evenly to obtain a suspension; S4: washing the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane prepared in step S1, then spreading it flat in a container, slowly adding the suspension prepared in step S3, and immersing it for 6 to 12 hours. After the immersion is completed, vacuum drying is performed to obtain an embedded composite fiber membrane; S5: dissolving the modified chitosan prepared in step S2 into deionized water, stirring evenly, adding NaOH solution to adjust the pH, and then adding glutaraldehyde, mixing evenly, to obtain a modified chitosan solution; S6: coating the modified chitosan solution prepared in step S5 onto the embedded composite fiber membrane prepared in step S4, and then placing the coated embedded composite fiber membrane in a constant temperature and humidity chamber for drying. After drying, repeat the above coating and drying operations to coat and dry the second side. After all coating reactions are completed, wash and vacuum dry to obtain a composite material. The preparation steps of the modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane in step S1 are as follows: A1: Hydroxyapatite nanoparticles are dispersed in deionized water, ultrasonically dispersed evenly, a coupling agent is added, stirred at 4-10°C for 1-2 hours, and then the succinimide solution is slowly added dropwise, and the stirring reaction is continued at 4-10°C for 1-2 hours. The precipitate is collected by centrifugation, washed three times with deionized water, and vacuum freeze-dried to obtain modified hydroxyapatite nanoparticles; A2: dissolving polycaprolactone in dichloromethane, stirring and mixing, adding polyethylene glycol, dicyclohexylcarbodiimide and 4-dimethylaminopyridine under nitrogen protection, stirring, centrifuging, filtering, washing with deionized water, and vacuum drying to obtain modified polycaprolactone; A3: The modified hydroxyapatite nanoparticles prepared in step A1 are dispersed in deionized water, subjected to ultrasonic treatment, and then the AgNO3 solution is slowly added dropwise, and the mixture is stirred for 5 to 10 minutes. Then, the NaBH4 solution is slowly added dropwise in an ice bath, and the mixture is stirred for 1 to 2 hours. After the reaction is completed, the mixture is centrifuged, the precipitate is collected, washed, and vacuum dried to obtain a modified hydroxyapatite-Ag composite material; A4: After the modified polycaprolactone and polyvinyl pyrrolidone prepared in step A2 are uniformly mixed, dichloromethane is added, and the temperature is controlled at 60-70° C. in a water bath, and stirring is continued until the solution is transparent; then the modified hydroxyapatite-Ag composite material prepared in step A3 is added, and the temperature is controlled and stirring is continued for reaction. After the reaction is completed, the solution is quickly cooled to room temperature in an ice bath, and filtered with a filter membrane to obtain a composite spinning solution; A5: transferring the composite spinning solution prepared in step A4 into a syringe, and performing electrospinning at room temperature to obtain a modified polycaprolactone / hydroxyapatite-Ag composite ultrafine fiber membrane; The coupling agent described in step A1 is 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide prepared in a mass ratio of 1.5:1; the ratio of the amount of hydroxyapatite nanoparticles, coupling agent, and succinimide solution is 1g:10-20mg:2mL; The ratio of the amount of polycaprolactone, dichloromethane, polyethylene glycol, dicyclohexylcarbodiimide and 4-dimethylaminopyridine used in step A2 is 1 g:10 mL:0.3-0.5 g:5-10 mg:1 mg; All operations after the dropwise addition of the AgNO3 solution in step A3 are performed under nitrogen protection, and the ratio of the amount of the modified hydroxyapatite nanoparticles, the AgNO3 solution and the NaBH4 solution is 1 g: 1-1.5 mL: 1 mL; The ratio of the modified polycaprolactone, polyvinyl pyrrolidone, dichloromethane and modified hydroxyapatite-Ag composite material used in step A4 is 1 g: 0.15-0.25 g: 5 mL: 0.2-0.5 g; The preparation steps of the modified chitosan in step S2 are as follows: B1: Add chitosan powder to 0.5wt% acetic acid solution, stir and mix evenly at room temperature, filter, and centrifuge to obtain a 3wt% pretreated chitosan solution; B2: slowly adding chloroacetic acid to the pretreated chitosan solution prepared in step B1, and controlling the pH with glacial acetic acid, heating the reaction in a water bath, adjusting the NaOH solution to neutral, naturally cooling to room temperature, dialyzing, centrifuging, taking the precipitate, washing, and vacuum freeze-drying to obtain modified chitosan; The ratio of the amount of chloroacetic acid to the pretreated chitosan solution in step B2 is 1.5-3 g:100 mL; The diameter of the bioactive glass in step S3 is 50 μm; the ratio of the amount of the bioactive glass to the amount of the PBS buffer is 1-3 g:100 mL; The ratio of the modified chitosan and deionized water used in step S5 is 2-5 g:100 mL.
Citation Information
Patent Citations
Anti hemorrhagic healing traumatic material of chitosan based fiber in water-solubility, preparation method and application
CN101049513A
Chemically collagen grafted hydroxyapatite implant materials
KR1020090043857A