A method for growing large-size calcium fluoride crystals and calcium fluoride crystals

By adjusting the top baffle of the crucible, crystal furnace temperature and argon convection, the problem of incomplete discharge of bubbles in the growth of large-sized calcium fluoride crystals was solved, and higher-quality calcium fluoride crystal growth was achieved, with the bubble content significantly reduced and the crystals Defects reduced.

CN118407130BActive Publication Date: 2024-09-27BEIJING QIFENG LANDA OPTICAL TECH DEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410865769.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-09-27
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

When growing large-sized calcium fluoride crystals in the existing technology, incomplete discharge of bubbles leads to an increase in crystal defects, high dislocation density, and even cracking of the crystal, which affects the quality of the crystal.

Method used

By adjusting the crucible top baffle, crystal furnace temperature and argon gas convection, the natural convection and surface tension convection of the melt are increased, combined with vacuum evacuation, to ensure full overflow of bubbles and reduce the bubble content in calcium fluoride crystals.

Benefits of technology

It significantly reduces the bubble content in calcium fluoride crystals, reduces defects, and improves crystal quality, making the obtained large-sized calcium fluoride crystals have a bubble content of less than 15/100cm3 and higher quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118407130B
    Figure CN118407130B
Patent Text Reader

Abstract

The present application relates to the field of crystal growth technology, and specifically discloses a method for growing large-sized calcium fluoride crystals and calcium fluoride crystals. The method for growing large-sized calcium fluoride crystals provided in the present application comprises the following steps: S1: loading calcium fluoride crystals into a crystal furnace crucible, heating the calcium fluoride crystals to melt them, and then opening the baffle on the top of the crucible; S2: then raising the temperature in the crystal furnace by 100-500°C, and waiting for the calcium fluoride crystals to melt all again, continuing to raise the temperature by 50-150°C; S3: then leaving the crystal furnace to stand for 10-72h, while filling the crystal furnace with argon gas, and evacuating the furnace to a pressure of 11-50kpa; the present application also provides calcium fluoride crystals obtained using the above-mentioned growth method. The method for growing large-sized calcium fluoride crystals provided in the present application can reduce the bubble content in the calcium fluoride crystals, reduce the defects of the calcium fluoride crystals, and effectively improve the quality of the calcium fluoride crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of crystal growth, and in particular to a growth method of large-sized calcium fluoride crystals and calcium fluoride crystals. Background Art

[0002] The Czochralski method is one of the most widely used single crystal growth methods. The advantage of this method is that the crystal will not contact the crucible wall during the growth process, and will not produce parasitic nucleation to form polycrystals. In addition, the crystal grows fast, has low stress birefringence, and has high integrity.

[0003] At present, the process of growing calcium fluoride crystals by the Czochralski method mainly includes: heating, constant temperature, seeding, shoulder release, equal diameter, cooling, etc. Among them, the main function of the constant temperature process is to expel bubbles in the raw material melt. However, when using the existing constant temperature process to prepare large-sized calcium fluoride crystals, bubbles cannot be completely eliminated due to the slow natural convection of the melt, large crystal size, and small thermal field temperature gradient. The bubbles that are not expelled will grow into the crystal with the convection of the melt, resulting in an increase in crystal defects and dislocation density. In severe cases, it will cause crystal cracking, thereby affecting the crystal quality. Summary of the invention

[0004] In order to overcome the problem of unclean bubble discharge during the growth of large-sized calcium fluoride crystals, the present application provides a growth method for large-sized calcium fluoride crystals and calcium fluoride crystals.

[0005] In the first aspect, the present application provides a method for growing large-sized calcium fluoride crystals, which adopts the following technical solution:

[0006] A method for growing large-sized calcium fluoride crystals comprises the following steps:

[0007] S1: Load calcium fluoride crystals into a crucible of a crystal furnace, heat up to melt the calcium fluoride crystals, and then open the baffle on the top of the crucible;

[0008] S2: then the temperature in the crystal furnace is raised by 100-500°C, and when all the calcium fluoride crystals are melted again, the temperature is further raised by 50-150°C;

[0009] S3: Then, the crystal furnace is left to stand for 10-72 hours, while argon is filled into the crystal furnace and the furnace is evacuated to a pressure of 11-50 kPa.

[0010] The present application provides a method for growing large-sized calcium fluoride crystals. In step S1 of the growth method, the temperature gradient of the melt in the crucible can be increased in the horizontal and vertical directions by opening a baffle, thereby increasing the natural convection of the melt and gradually discharging the bubbles in the melt. Step S2 can reduce the surface tension of the melt by overheating by 50-150°C, thereby strengthening the surface tension convection of the melt, thereby reducing the viscosity of the melt, strengthening the flow of the melt, and making it easy for bubbles to overflow. Step S3 adjusts the pressure in the furnace by evacuating the vacuum, so that the bubbles in the melt can fully overflow. Impurity gases (HF, CO, CO2, F2, gaseous or powdered CaF2, etc.) in the crystal furnace can be taken away by filling with flowing argon gas. In summary, the method for growing large-sized calcium fluoride crystals provided in the present application adjusts the temperature gradient of the inner cylinder of the crucible by adjusting the baffle on the top of the crucible, the temperature of the crystal furnace and the type of convection gas, thereby increasing the natural convection and surface tension convection of the melt, so that the bubbles in the melt are fully discharged, effectively reducing the bubble content in the obtained calcium fluoride crystals, reducing the defects of the calcium fluoride crystals, and improving the quality of the calcium fluoride crystals.

[0011] In the present application, since the Nusselt value of argon is large, the argon convection can take away the heat in the crystal furnace, so that the temperature gradient of the melt near the crucible increases. The increase in temperature gradient can enhance the natural convection of the melt, which is conducive to the small bubbles and large bubbles in the melt to collide with each other and aggregate to form large bubbles, and under the combined action of natural convection and buoyancy, they rupture at the liquid surface of the melt.

[0012] In some embodiments, in step S3, the pressure inside the furnace may be 11-20 kpa, 11-30 kpa, 11-40 kpa, 11-50 kpa, 20-30 kpa, 20-40 kpa, 20-50 kpa, 30-40 kpa, 30-50 kpa or 40-50 kpa.

[0013] In a specific embodiment, in step S3, the pressure inside the furnace can also be 11 kPa, 20 kPa, 30 kPa, 40 kPa or 50 kPa.

[0014] Optionally, in step S1, the opening rate of the baffle on the top of the crucible is 5-30 mm / min.

[0015] Optionally, in step S1, the temperature of the argon gas is 25±5° C., the purity is 5N, and the filling flow rate of the argon gas is 3-15 L / min.

[0016] In some embodiments, in step S3, the inflation flow rate of argon gas can be 3-5 L / min, 3-10 L / min, 3-15 L / min, 3-20 L / min, 5-10 L / min, 5-15 L / min, 5-20 L / min, 10-15 L / min, 10-20 L / min, or 15-20 L / min.

[0017] In a specific embodiment, in step S3, the filling flow rate of argon gas can also be 3 L / min, 5 L / min, 10 L / min, 15 L / min or 20 kPa.

[0018] Optionally, the heating rate in step S2 is 15-25° C. / h.

[0019] Optionally, the specific steps of melting the calcium fluoride crystal in step S1 are: first, evacuate the crystal furnace and increase the temperature to a vacuum degree of 1×10 -4 Pa, the temperature in the furnace is raised to 250-270℃, and kept at this temperature for 24-72h; stop evacuating, and slowly raise the temperature at a rate of 90-120℃ / h, and at the same time fill the furnace with argon. When the pressure in the furnace is about 112kPa-150kPa, stop filling with argon, and continue to raise the temperature at a rate of 140-160℃ / h until the temperature reaches 1400-1500℃, then start to keep the temperature constant until the calcium fluoride crystals melt.

[0020] Optionally, after step S3 is completed, the argon gas is turned off, and vacuuming is continued until the pressure in the furnace body reaches 50-80 kPa and the vacuum valve is closed.

[0021] Optionally, after closing the vacuum valve, close the top baffle at a rate of 13-18 mm / min, then cool to 1400-1500° C. at a rate of 10-50° C. / h, and keep at a constant temperature for 7-30 hours.

[0022] Optionally, the method for growing large-size calcium fluoride crystals further includes: seeding, shoulder release, equal-diameter growth and cooling.

[0023] In a second aspect, the present application provides a calcium fluoride crystal obtained by using a method for growing a large-sized calcium fluoride crystal.

[0024] Optionally, the diameter of the calcium fluoride crystal is 250-350 mm.

[0025] In some embodiments, the calcium fluoride crystals may have a diameter of 250-340 mm.

[0026] In a specific embodiment, the diameter of the calcium fluoride crystal may also be 250 mm or 340 mm.

[0027] In summary, this application has the following beneficial effects:

[0028] 1. The present application provides a method for growing large-sized calcium fluoride crystals. The method can fully overflow the bubbles in the calcium fluoride melt by adjusting the baffle on the top of the crucible, the temperature of the crystal furnace and using argon as a convection gas, thereby significantly reducing the bubble content in the calcium fluoride crystals and improving the quality of the calcium fluoride crystals.

[0029] 2. The present application further controls the argon gas filling flow rate in step S3 within the range of 3-15 L / min, and the pressure in the furnace body within the range of 20-50 kPa, and the bubble content of the obtained calcium fluoride crystal is less than 15 / 100cm 3 , the quality of calcium fluoride crystals is higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of the crystal furnace used in the embodiments of the present application; 1-furnace body, 2-seed rod, 3-top baffle, 4-push rod, 5-graphite plate, 6-heater, 7-graphite hard felt, 8-bottom graphite hard felt, 9-lower shaft, 10-crucible support, 11-outer crucible, 12-inner crucible, 13-calcium fluoride crystal, 14-calcium fluoride melt. DETAILED DESCRIPTION

[0031] The present application provides a method for growing large-sized calcium fluoride crystals, comprising the following steps:

[0032] (1) Place calcium fluoride crystals into a graphite crucible; then start the vacuum system to evacuate the crystal furnace to a vacuum degree of 1x10 -4 Pa, turn on the heater at the same time to raise the temperature in the furnace to 250-270℃, and then keep the temperature constant for 24-72h.

[0033] (2) After the constant temperature is completed, stop evacuating the vacuum, then slowly increase the temperature at a rate of 90-120℃ / h, and at the same time fill the furnace with argon. When the pressure in the furnace is about 112-150kPa, stop filling with argon; then continue to increase the temperature at a rate of 140-160℃ / h until the temperature reaches 1400-1500℃ and then start constant temperature.

[0034] (3) After the calcium fluoride crystals in the crucible become melt, open the baffle on the top of the crucible at a speed of 5-30 mm / min, and open the baffle to the maximum position (the distance between the two semicircles of the top plate is not less than the crystal diameter); appropriately adjust the temperature to 100-500℃ to melt all the melt in the crucible. Continue to increase the temperature by 50-150℃ to allow the bubbles in the melt to fully overflow; during the above two heating processes, control the heating rate to 15-25℃ / h.

[0035] (4) The equipment is left to stand for 10-72 hours. During the standing period, open the argon filling valve and the vacuum pump, adjust the argon filling flow rate of the flow meter to 3-15L / min, and control the pressure in the furnace to 11-50kPa, so that the bubbles in the solution can be fully overflowed with the argon gas; the argon gas is in a cold state, and the temperature is 25±5℃.

[0036] (5) After the standing time is over, close the vacuum valve and close the argon valve when the pressure inside the furnace is 50-80kPa.

[0037] (6) Close the top baffle at a rate of 13-18 mm / min, then cool to 1400-1500°C at a rate of 10-50°C / h, and keep it at a constant temperature for 7-30 hours.

[0038] (7) Then, process gas is charged according to the ratio of patent CN116676668B, and seeding, shoulder release and crystal growth are carried out according to the method of patent CN116716659B, and finally large-sized calcium fluoride crystals with a diameter of 250-350 mm are obtained.

[0039] In the present application, the particle size of calcium fluoride crystals is 3-7 mm, and the oxygen content is less than 0.00001%; ​​the remaining raw materials, reagents, etc. can be obtained commercially.

[0040] The present application is further described in detail below in conjunction with embodiments and performance testing experiments. Example 1

[0041] Embodiment 1 provides a method for growing large-sized calcium fluoride crystals, comprising the following steps:

[0042] (1) Place calcium fluoride crystals into a graphite crucible; then start the vacuum system to evacuate the crystal furnace to a vacuum degree of 5x10 -5 Pa, and at the same time turn on the heater to raise the temperature in the furnace to 260°C, and then keep the temperature constant for 24 hours.

[0043] (2) After the constant temperature is completed, stop evacuating the vacuum, then slowly increase the temperature at a rate of 100℃ / h, and at the same time fill the furnace with argon. When the pressure in the furnace reaches 131kPa, stop filling with argon; then continue to increase the temperature at a rate of 150℃ / h until the temperature reaches 1450℃ and then start constant temperature.

[0044] (3) After the calcium fluoride crystals in the crucible become melt, open the baffle on the top of the crucible at a speed of 20 mm / min (the baffle is opened and closed by the push rod on the side), and open the baffle to the maximum position; appropriately adjust the temperature to 200°C so that all the melt in the crucible is melted, and continue to heat up by 100°C; during the above two heating processes, control the heating rate to 20°C / h.

[0045] (4) The equipment was left to stand for 24 hours. During the standing period, the argon filling valve and vacuum pump were opened, and the argon filling flow rate of the flow meter was adjusted to 10L / min and the pressure inside the furnace was 30kPa.

[0046] (5) After the standing time is over, close the vacuum valve and close the argon valve when the pressure inside the furnace reaches 60kPa.

[0047] (6) Close the top baffle at a rate of 16 mm / min, then cool to 1450°C at 40°C / h and keep at this temperature for 12 h.

[0048] (7) Then, the process gas is filled in according to the ratio of patent CN116676668B, and the seeding, shoulder release and crystal growth are carried out according to the method of patent CN116716659B, and finally a large-sized calcium fluoride crystal with a diameter of 250 mm is obtained.

[0049] Embodiment 2-9

[0050] Examples 2-9 each provide a method for growing large-sized calcium fluoride crystals.

[0051] The difference between the above embodiment and embodiment 1 is that the argon filling flow rate and the pressure inside the furnace in step (4) are specifically shown in Table 1 below.

[0052] Table 1 Argon filling flow rate and furnace pressure in the growth method provided in Examples 1-9

[0053] Example 10

[0054] Example 10 provides a method for growing large-sized calcium fluoride crystals.

[0055] The difference between the above embodiment and embodiment 1 is that the diameter of the prepared calcium fluoride crystal is 340 mm. Comparative Example 1

[0056] Comparative Example 1 provides a method for growing large-sized calcium fluoride crystals.

[0057] The difference between the comparative example and Example 1 is that step (3) is as follows:

[0058] (3) After the calcium fluoride crystals in the crucible become a melt, continue to raise the temperature by 100°C. Comparative Example 2

[0059] Comparative Example 2 provides a method for growing large-sized calcium fluoride crystals.

[0060] The difference between the comparative example and Example 1 is that step (3) is as follows:

[0061] (3) After the calcium fluoride crystals in the crucible become melt, open the baffle on the top of the crucible at a speed of 20 mm / min and open the baffle to the maximum position; appropriately adjust the temperature to 200°C and control the heating rate to 20°C / h so that all the melt in the crucible is melted. Comparative Example 3

[0062] Comparative Example 3 provides a method for growing large-sized calcium fluoride crystals.

[0063] The difference between the comparative example and Example 1 is that the argon gas in step (2) and step (4) is replaced by helium. Comparative Example 4

[0064] Comparative Example 4 provides a method for growing large-sized calcium fluoride crystals.

[0065] The difference between the comparative example and Example 1 is that step (4-5) is as follows:

[0066] (4) Let the equipment stand for 24 hours. During this period, open the argon filling valve and adjust the argon filling flow rate of the flow meter to 10L / min.

[0067] (5) After the standing time is over, turn off the argon gas.

[0068] Performance testing

[0069] The number of bubbles in the calcium fluoride crystals obtained in Examples 1-10 and Comparative Examples 1-4 was detected, and the results are shown in Table 2 below.

[0070] The method for detecting the number of bubbles is: in total darkness, use a strong light source with a luminous flux of 2000lm (lumens) to illuminate the crystal, and observe the number of bubbles in the crystal with the naked eye. According to the volume of the crystal, calculate the number of bubbles per unit volume and take the integer.

[0071] Table 2 Results of the detection of the number of bubbles in the calcium fluoride crystals obtained in Examples 1-10 and Comparative Examples 1-4

[0072]

[0073] According to the test results in Table 2, the bubble content in the calcium fluoride crystals obtained in Examples 1-10 is 7-17 / 100cm 3 The bubble content in the calcium fluoride crystal obtained in Comparative Example 1 without opening the baffle was as high as 48 / 100cm 3 The bubble content in the calcium fluoride crystal obtained in Comparative Example 2 without overheating was as high as 35 / 100cm 3In Comparative Example 3, the bubble content of the calcium fluoride crystal obtained by using helium as the convection gas was as high as 42 / 100cm 3 The bubble content in the calcium fluoride crystal obtained in Comparative Example 4 without vacuuming after inflation was as high as 37 / 100cm 3 Therefore, it is shown that the method for growing large-sized calcium fluoride crystals provided in the present application can effectively reduce the bubble content in the obtained calcium fluoride crystals and improve the quality of the calcium fluoride crystals by adjusting the baffle plate on the top of the crucible, the temperature of the crystal furnace, the type of convection gas and related parameters.

[0074] The test results of Examples 1-5 show that with the increase of the argon gas flow rate, the bubble content in the obtained calcium fluoride crystals shows a trend of first decreasing and then increasing. Further comparison shows that when the argon gas flow rate is controlled to 3-15 L / min in Example 1-4, the bubble content in the obtained calcium fluoride crystals is 7-13 / 100 cm 3 (<15 / 100cm 3 ). Therefore, it is explained that the present application controls the argon gas filling flow rate within the range of 3-15 L / min, the bubble content of the obtained calcium fluoride crystals is small, and the quality of the calcium fluoride crystals is better.

[0075] The test results of Example 1 and Examples 6-9 show that, with the increase of the pressure in the furnace, the bubble content in the obtained calcium fluoride crystals first decreases and then remains basically unchanged. Further comparison shows that, when the pressure in the furnace is controlled at 20-50 kPa in Example 1 and Examples 7-9, the bubble content in the obtained calcium fluoride crystals is 7-12 / 100cm 3 (<15 / 100cm 3 ). Therefore, it is explained that the pressure in the furnace body is controlled within the range of 20-50 kPa in the present application, the bubble content of the obtained calcium fluoride crystals is small, and the quality of the calcium fluoride crystals is better.

[0076] The test results of Example 1 and Example 10 show that the growth method of calcium fluoride crystals provided by the present application can obtain large-sized calcium fluoride crystals with diameters of 250 mm and 340 mm, and the bubble content in the obtained calcium fluoride crystals is less than 20 / 100 cm 3 .

[0077] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for growing large-sized calcium fluoride crystals, characterized in that: The following steps are involved: S1: Load calcium fluoride crystals into a crucible of a crystal furnace, heat up to melt the calcium fluoride crystals, and then open the baffle on the top of the crucible; S2: then the temperature in the crystal furnace is raised by 100-500°C, and when all the calcium fluoride crystals are melted again, the temperature is further raised by 50-150°C; S3: Then, the crystal furnace is left to stand for 10-72 hours, while argon is filled into the crystal furnace and the furnace is evacuated to a pressure of 11-50 kPa.

2. The method for growing large-sized calcium fluoride crystals according to claim 1, characterized in that: In the step S1, the opening rate of the baffle plate on the top of the crucible is 5-30 mm / min.

3. The method for growing large-sized calcium fluoride crystals according to claim 1, characterized in that: In step S3, the temperature of the argon gas is 25±5° C., the purity is 5N, and the filling flow rate of the argon gas is 3-15 L / min.

4. The method for growing large-sized calcium fluoride crystals according to claim 1, characterized in that: The heating rate in step S2 is 15-25°C / h.

5. The method for growing large-sized calcium fluoride crystals according to claim 1, characterized in that: The specific steps of melting the calcium fluoride crystals in step S1 are: First, evacuate the crystal furnace and raise the temperature to a vacuum degree of 1x10 -4 Pa, the temperature in the furnace is raised to 250-270℃, and kept at this temperature for 24-72h; stop evacuating, and slowly raise the temperature at a rate of 90-120℃ / h, and at the same time fill the furnace with argon. When the pressure in the furnace reaches 112kPa-150kPa, stop filling with argon, and continue to raise the temperature at a rate of 140-160℃ / h until the temperature reaches 1400-1500℃, then start to keep the temperature constant until the calcium fluoride crystals melt.

6. The method for growing large-sized calcium fluoride crystals according to claim 1, characterized in that: After step S3 is completed, the vacuum valve is closed until the pressure in the furnace body reaches 50-80 kPa, and the argon valve is closed.

7. The method for growing large-sized calcium fluoride crystals according to claim 6, characterized in that: After closing the vacuum valve, close the top baffle at a rate of 13-18 mm / min, then cool down to 1400-1500°C at a rate of 10-50°C / h, and keep it at a constant temperature for 7-30 hours.

8. The method for growing large-sized calcium fluoride crystals according to claim 1, characterized in that: The method for growing large-size calcium fluoride crystals also includes: seeding, shoulder release, equal diameter growth and cooling.

Citation Information

Cited By

  • Impurity removal process for high-transmittance calcium fluoride crystals

    CN121629495A