A highly wear-resistant rubber composition for automobile tire tread
Through the grafting technology of modified ethylene propylene rubber and white carbon black, combined with other components, a high wear-resistant automotive tire rubber composition is formed, which solves the problem of low strength, poor wear resistance and easy oxidation and degradation of rubber materials in the prior art. The problem is that excellent mechanical properties, UV aging resistance and flame retardant properties are achieved, reducing energy consumption.
Patent Information
- Application Number
- CN202410784865.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The existing automotive tire rubber materials have problems such as low strength, poor wear resistance, easy yellowing and oxidative degradation during use, and the addition of a large number of flame retardants will affect the mechanical properties, resulting in the tire increasing rolling resistance and energy consumption during dynamic processes.
Using modified ethylene propylene ternary rubber and modified white carbon black, carboxylated nanotitanium dioxide and DOPO derivatives are grafted through chemical reactions, combining natural rubber, butyl rubber, nano zinc oxide, stearic acid, sulfur, promoters and Anti-aging agent forms a rubber composition for treads for high wear-resistant automotive tires.
It significantly improves the mechanical properties, UV aging resistance and flame retardant properties of the rubber composition, enhances the rebound rate, tensile strength and flame retardant effect of the rubber, and avoids the migration and exudation of flame retardant and the white carbon black. Self-aggregation reduces rolling resistance and energy consumption.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tire rubber, and in particular relates to a rubber composition for a highly wear-resistant automobile tire tread. Background Art
[0002] Tires are one of the important components of automobiles. Their main function is to support the entire weight of the vehicle, bear the load of the vehicle, transmit traction and braking torque, and ensure the adhesion between the wheel and the road surface. Rubber materials are the main materials for making tires. Natural rubber has high tensile strength and tear strength due to strain-induced crystallization. It is the most widely used base material in the tread of load-bearing tires. However, natural rubber itself has low strength. With the rapid development of the automobile industry, higher requirements are placed on the quality and performance of natural rubber.
[0003] Carbon black reinforcement can effectively improve the strength and wear resistance of rubber materials, but rubber and carbon black are mainly combined by blending. Since carbon black has a strong polarity, it has poor compatibility with rubber molecules and is not easy to disperse in the rubber, which limits its mechanical properties from being effectively exerted. In the dynamic process, the slippage of the rubber molecular chain on the surface of carbon black and the friction between the carbon black particles will produce hysteresis losses, resulting in increased rolling resistance and heat generation of the tire, and increased energy consumption. In addition, tire rubber is prone to yellowing and oxidative degradation when exposed to light for a long time, resulting in the breakage of the material molecular chain and destruction of the molecular structure. At the same time, a large amount of flame retardants are added to the existing tire rubber to achieve its flame retardant properties, but the addition of a large amount of flame retardants will affect the mechanical properties of the tire rubber, further limiting the application of rubber compositions in automobile tires. Summary of the invention
[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a highly wear-resistant rubber composition for automobile tire treads, which is endowed with excellent mechanical properties, UV aging resistance and flame retardant properties by adding modified EPDM rubber and modified silica.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A rubber composition for a highly wear-resistant automobile tire tread, comprising the following raw materials in parts by weight: 55-80 parts of natural rubber, 5-15 parts of modified EPDM rubber, 20-40 parts of butadiene rubber, 10-25 parts of modified white carbon black, 5-8 parts of nano zinc oxide, 2-4 parts of stearic acid, 1.5-3.5 parts of sulfur, 0.1-0.5 parts of an accelerator, and 0.5-1 parts of an antioxidant;
[0007] The modified EPDM rubber is prepared by grafting carboxylated nano-titanium dioxide into the EPDM rubber structure through a chemical reaction; the modified silica is prepared by grafting DOPO derivatives into the silica structure through a chemical reaction.
[0008] Preferably, the accelerator is a mixture of one or more of accelerator DM, accelerator M, accelerator TMTD, accelerator D, accelerator DTDM, and accelerator BZ; the antioxidant is a combination of one or more of N-phenyl-α-naphthylamine, N-phenyl-β-naphthylamine, and NN-diphenyl-p-phenylenediamine.
[0009] Preferably, the preparation method of the modified EPDM rubber comprises the following steps:
[0010] A. Dissolve EPDM rubber in n-hexane, add formic acid and Tween 80 at 40-60°C, stir and mix, then add hydrogen peroxide to react for 8-12 hours, add anhydrous sodium carbonate aqueous solution for washing after the reaction is completed, pour into a separatory funnel and let stand to remove the water phase, then wash with deionized water until neutral, precipitate and dry to prepare epoxidized EPDM rubber;
[0011] B. Take nano titanium dioxide and dissolve it in deionized water, stir and mix it at room temperature and disperse it ultrasonically, add sodium chloroacetate and drop sodium hydroxide solution to adjust the pH of the system to 11-13, then place it in an oil bath at 100-120°C and heat it for 3-6 hours. After the reaction is completed, wash it with deionized water until it is neutral, then centrifuge and dry it to prepare carboxylated nano titanium dioxide;
[0012] C. Take carboxylated nano-titanium dioxide in anhydrous butyl acetate and disperse it by ultrasonic, add epoxidized ethylene propylene rubber fully dissolved in xylene solvent, and add triphenylphosphine, place it at 90-120°C and stir to react for 8-12h. After the reaction is completed, rotary evaporate and dry to prepare modified ethylene propylene rubber.
[0013] Preferably, in step A, the mass ratio of EPDM rubber, formic acid and hydrogen peroxide is 25-30:0.5-1.2:4-7.
[0014] Preferably, in step C, the mass ratio of carboxylated nano-titanium dioxide to epoxidized EPDM rubber is 1:1.2-2.
[0015] Preferably, the preparation method of the modified silica comprises the following steps:
[0016] (1) Ultrasonic dispersion of white carbon black in anhydrous ethanol, adding 5-isocyanate isophthaloyl chloride and dibutyltin dilaurate, stirring and reacting at 45-70° C. for 6-12 hours, centrifugation and vacuum drying after the reaction is completed, to prepare chlorinated white carbon black;
[0017] (2) 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is placed in a reactor, diethanolamine and deionized water are added, the mixture is stirred at 80-95°C, and then paraformaldehyde is added, and the mixture is refluxed in a nitrogen atmosphere for 1-3 hours. After the reaction is completed, the mixture is subjected to rotary evaporation, washing, and drying to obtain a DOPO derivative;
[0018] (3) Take acyl chloride silica and DOPO derivatives in N, N-dimethylacetamide, ultrasonically disperse them at room temperature, then add pyridine, and reflux at 120-135°C for 36-48 hours. After the reaction is completed, filter, wash, and dry to prepare modified silica.
[0019] Preferably, in step (1), the mass ratio of white carbon black to 5-isocyanate isophthaloyl chloride is 1:0.5-1.2.
[0020] Preferably, in step (2), the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diethanolamine and paraformaldehyde is 5-5.5:2-3:0.5-1.
[0021] Preferably, in step (3), the mass ratio of chlorinated silica to DOPO derivative is 3-7:5-9.
[0022] Preferably, the preparation method of the rubber composition is specifically as follows: weigh each raw material by weight, add natural rubber, modified EPDM rubber and butadiene rubber into a rubber mixing mill for plasticizing, add modified silica, nano zinc oxide, stearic acid and antioxidant for mixing for 3 to 5 minutes after plasticizing evenly, finally add sulfur and accelerator for mixing evenly, and vulcanize at 120 to 160° C. for 8 to 10 minutes to prepare the rubber composition.
[0023] Beneficial effects of the present invention:
[0024] The invention utilizes formic acid and hydrogen peroxide to convert double bonds in the molecular chain of EPDM rubber into epoxy groups, and then reacts with carboxylated nano titanium dioxide, so that the epoxy groups in the EPDM rubber structure and the carboxyl groups on the surface of the nano titanium dioxide undergo grafting reaction. The nano titanium dioxide, as an important inorganic ultraviolet shielding agent, has good weather resistance and heat resistance, can reduce ultraviolet light aging, and has spectrum antibacterial, deodorizing, mildew-proof and other functions. The nano titanium dioxide and the EPDM rubber are firmly combined through chemical bonds to increase the polarity of the EPDM rubber, which is beneficial to the dispersion of the nano titanium dioxide, enhances the compatibility and interface bonding performance of the nano titanium dioxide and the rubber matrix, avoids the agglomeration of the nano titanium dioxide to increase its particle size, and affects the ultraviolet shielding efficiency. The EPDM rubber has a good reinforcing and toughening effect on tire rubber, and can effectively enhance the rebound rate, tensile strength and other comprehensive properties of the rubber composition.
[0025] The invention uses a catalyst dibutyltin dilaurate to catalyze the reaction of hydroxyl groups on the surface of white carbon black with isocyanate groups on the surface of 5-isocyanate isophthaloyl chloride to generate chlorinated white carbon black. At the same time, the invention uses 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diethanolamine and polyformaldehyde to prepare a DOPO derivative flame retardant, which is then grafted with chlorinated white carbon black. The surface of the DOPO derivative contains dihydroxyl groups, which are covalently grafted to the surface of chlorinated white carbon black, thereby modifying the DOPO derivative flame retardant on the surface of the white carbon black. The two are firmly combined through chemical bonds, which can not only play a good flame retardant effect, but also avoid the migration and seepage of the flame retardant, thereby ensuring that the tire rubber achieves a long-term flame retardant effect. In addition, the self-aggregation of white carbon black is reduced, so that the modified white carbon black is dispersed and stably in the matrix, the compatibility of white carbon black and the rubber matrix is enhanced, and the mechanical properties thereof are avoided to be affected. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1 A method for preparing a modified EPDM rubber comprises the following steps:
[0028] A. Take 15g of EPDM rubber and dissolve it in 250mL of n-hexane, add 0.6g of formic acid and 0.7g of Tween 80 at 40°C and stir to mix, then add 3.1g of hydrogen peroxide to react for 12h, add 0.25wt.% anhydrous sodium carbonate aqueous solution for washing after the reaction is completed, pour it into a separatory funnel and let it stand to remove the water phase, then wash it with deionized water until neutral, then add it into 500mL of anhydrous ethanol for flocculation and precipitation, and finally dry it in a vacuum oven to prepare epoxidized EPDM rubber;
[0029] B. Take 2g of nano titanium dioxide and dissolve it in 300mL of deionized water, stir and mix it at room temperature and disperse it ultrasonically, add 2.5g of sodium chloroacetate and drop a 0.1mol / L sodium hydroxide solution to adjust the pH of the system to 12, then place it in an oil bath at 115°C and heat it for 4h. After the reaction is completed, wash it with deionized water until it is neutral, then centrifuge and dry it to prepare carboxylated nano titanium dioxide;
[0030] C. Take 3g of carboxylated nano-titanium dioxide and dissolve it in 60mL of anhydrous butyl acetate and disperse it ultrasonically. Take 5g of epoxidized EPDM rubber and dissolve it in 120mL of xylene solvent and then add it. Then add 0.008g of triphenylphosphine. Place it at 115°C and stir to react for 12h. After the reaction is completed, evaporate it and dry it to prepare modified EPDM rubber.
[0031] Example 2 A method for preparing modified white carbon black comprises the following steps:
[0032] (1) 5 g of white carbon black was ultrasonically dispersed in 100 mL of anhydrous ethanol, 4.7 g of 5-isocyanate isophthaloyl chloride and 0.002 g of dibutyltin dilaurate were added, and the mixture was stirred at 60° C. for 12 h. After the reaction was completed, the mixture was centrifuged and vacuum dried to prepare chlorinated white carbon black;
[0033] (2) 10 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was placed in a reactor, 4.6 g of diethanolamine and 100 mL of deionized water were added, the mixture was stirred at 85 °C, and then 1.7 g of paraformaldehyde was added, and the mixture was refluxed in a nitrogen atmosphere for 2 h. After the reaction was completed, the mixture was subjected to rotary evaporation, washing, and drying to obtain a DOPO derivative;
[0034] (3) Take 4.2 g of acyl chloride silica and 6.3 g of DOPO derivative in 250 mL of N,N-dimethylacetamide, add 2 mL of pyridine after ultrasonic dispersion at room temperature, and reflux at 125 °C for 38 h. After the reaction is completed, filter, wash and dry to prepare modified silica.
[0035] Example 3 A highly wear-resistant rubber composition for automobile tire tread comprises the following raw materials in parts by weight: 57 parts of natural rubber, 5 parts of modified EPDM rubber, 21 parts of butadiene rubber, 12 parts of modified silica, 5 parts of nano zinc oxide, 2 parts of stearic acid, 1.5 parts of sulfur, 0.2 parts of accelerator DM, and 0.5 parts of antioxidant N-phenyl-α-naphthylamine.
[0036] The preparation method of the rubber composition is specifically as follows:
[0037] The raw materials were weighed according to their weight, and natural rubber, modified EPDM rubber and butadiene rubber were added to a rubber mixing mill for plasticizing. After plasticizing evenly, modified silica, nano zinc oxide, stearic acid and antioxidant were added and mixed for 5 minutes. Finally, sulfur and accelerator were added and mixed evenly, and then vulcanized at 140°C for 8 minutes to prepare a rubber composition.
[0038] Example 4 A highly wear-resistant rubber composition for automobile tire tread comprises the following raw materials in parts by weight: 68 parts of natural rubber, 10 parts of modified EPDM rubber, 25 parts of butadiene rubber, 17 parts of modified silica, 6 parts of nano zinc oxide, 3 parts of stearic acid, 2 parts of sulfur, 0.4 parts of accelerator M, and 1 part of antioxidant N-phenyl-β-naphthylamine.
[0039] The preparation method of the rubber composition is the same as that of Example 3.
[0040] Example 5 A highly wear-resistant rubber composition for automobile tire tread comprises the following raw materials in parts by weight: 77 parts of natural rubber, 15 parts of modified EPDM rubber, 38 parts of butadiene rubber, 25 parts of modified silica, 8 parts of nano zinc oxide, 4 parts of stearic acid, 3.5 parts of sulfur, 0.5 parts of accelerator TMTD, and 1 part of antioxidant NN-diphenyl-p-phenylenediamine.
[0041] The preparation method of the rubber composition is the same as that of Example 3.
[0042] Comparative Example 1 A highly wear-resistant rubber composition for automobile tire treads comprises the following raw materials in parts by weight: 77 parts of natural rubber, 8 parts of EPDM rubber, 7 parts of nano-titanium dioxide, 38 parts of butadiene rubber, 25 parts of modified silica, 8 parts of nano-zinc oxide, 4 parts of stearic acid, 3.5 parts of sulfur, 0.5 parts of accelerator TMTD, and 1 part of antioxidant NN-diphenyl-p-phenylenediamine.
[0043] The preparation method of the rubber composition is the same as that of Example 3.
[0044] Comparative Example 2 A rubber composition for highly wear-resistant automobile tire tread comprises the following raw materials in parts by weight: 77 parts of natural rubber, 15 parts of EPDM rubber, 38 parts of butadiene rubber, 25 parts of modified silica, 8 parts of nano zinc oxide, 4 parts of stearic acid, 3.5 parts of sulfur, 0.5 parts of accelerator TMTD, and 1 part of antioxidant NN-diphenyl-p-phenylenediamine.
[0045] The preparation method of the rubber composition is the same as that of Example 3.
[0046] Comparative Example 3 A highly wear-resistant rubber composition for automobile tire tread comprises the following raw materials in parts by weight: 77 parts of natural rubber, 15 parts of modified EPDM rubber, 38 parts of butadiene rubber, 25 parts of white carbon black, 8 parts of nano zinc oxide, 4 parts of stearic acid, 3.5 parts of sulfur, 0.5 parts of accelerator TMTD, and 1 part of antioxidant NN-diphenyl-p-phenylenediamine.
[0047] The preparation method of the rubber composition is the same as that of Example 3.
[0048] Performance Testing
[0049] (1) Mechanical property test: The rubber compositions prepared in Examples 3-5 and Comparative Examples 1-3 were subjected to mechanical property tests. A 2 mm thick sample was cut into a dumbbell-shaped strip with a width of 6 mm. The speed of the clamp during stretching was 500 mm / min. The tensile strength and elongation at break were tested according to GB / T 528-2009. A 2 mm thick sample was cut into a right angle shape. The speed of the clamp during stretching was 500 mm / min. The tear strength was tested according to GB / T 529-2008. The resilience was tested according to GB / T 1681-2009. The data results are shown in Table 1.
[0050] The wear resistance test was carried out according to GB / T 1689-2014. The sample was made into a long strip with a thickness of 3.2 mm and a width of 12.7 mm. After grinding on both sides, it was glued to the rubber wheel. The glued sample rubber wheel was fixed on the rubber wheel shaft. The angle between the rubber wheel shaft and the grinding wheel shaft was 15°. The sample was subjected to a load of 26.7 N. The motor was started to rotate the sample in a clockwise direction. After pre-grinding for 20 minutes, it was removed, the rubber scraps were brushed off, and the pre-grinding mass was weighed. The pre-grinded sample was used for the test. The sample was removed after traveling 1.61 km, the rubber scraps were brushed off, and the test mass was weighed. The wear amount was calculated as the pre-grinding mass-test mass. The data results are shown in Table 1.
[0051] Table 1 Test results of mechanical properties of samples
[0052]
[0053] It can be seen from the data in Table 1 that the rubber compositions prepared in Examples 3-5 of the present invention all have the characteristics of high tensile strength, good wear resistance, and not easy to break. In Comparative Example 1, EPDM rubber and nano-titanium dioxide were not grafted, and the two were blended, and the mechanical properties of the two decreased. In Comparative Example 2, EPDM rubber was not modified, and the mechanical properties measured decreased significantly. In Comparative Example 3, white carbon black was not modified, and aggregates may have formed in the substrate, resulting in slightly worse mechanical properties than Examples 3-5.
[0054] (2) UV aging performance test: The light source is a 20W UV lamp, emitting short-wave UV light with a characteristic wavelength of 253.7nm. The UV irradiation intensity at 20cm from the vertical center of the lamp tube is 1400μw / cm 2 , the sample was placed in a fixed position parallel to the light source and subjected to UV aging test, and the data results were shown in Table 2.
[0055] Table 2 UV aging performance test results of samples
[0056]
[0057] It can be seen from the data in Table 2 that the rubber compositions prepared in Examples 3-5 of the present invention still have high tensile strength and elongation at break after aging for 200h, 400h and 800h, indicating that the rubber compositions have excellent resistance to ultraviolet aging. In Comparative Example 1, EPDM rubber and nano-titanium dioxide are not grafted, and in Comparative Example 2, EPDM rubber is not modified. It is measured that the tensile strength and elongation at break of the rubber compositions of Comparative Examples 1-2 after aging decrease significantly compared with those of Examples 3-5.
[0058] (3) Flame retardant performance test: The limiting oxygen index test is used, and the sample size is 130×6.5×3.2mm 3 The data results are shown in Table 3.
[0059] Table 3 Test results of flame retardant properties of samples
[0060]
[0061] It can be seen from the data in Table 3 that the rubber compositions prepared in Examples 3-5 of the present invention and Comparative Examples 1-2 all have good flame retardant properties. In Comparative Example 3, white carbon black is not modified, and the flame retardant properties of the rubber measured are significantly reduced.
[0062] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0063] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A highly wear-resistant rubber composition for automobile tire tread, characterized in that: The invention comprises the following raw materials in parts by weight: 55-80 parts of natural rubber, 5-15 parts of modified EPDM rubber, 20-40 parts of butadiene rubber, 10-25 parts of modified white carbon black, 5-8 parts of nano zinc oxide, 2-4 parts of stearic acid, 1.5-3.5 parts of sulfur, 0.1-0.5 parts of accelerator and 0.5-1 parts of antioxidant; The modified EPDM rubber is made by grafting carboxylated nano-titanium dioxide into the EPDM rubber structure through a chemical reaction; the modified silica is made by grafting DOPO derivatives into the silica structure through a chemical reaction; The preparation method of the modified EPDM rubber comprises the following steps: A. Dissolve EPDM rubber in n-hexane, add formic acid and Tween 80 at 40-60°C, stir and mix, then add hydrogen peroxide to react for 8-12 hours, add anhydrous sodium carbonate aqueous solution for washing after the reaction is completed, pour into a separatory funnel and let stand to remove the water phase, then wash with deionized water until neutral, precipitate and dry to prepare epoxidized EPDM rubber; B. Take nano titanium dioxide and dissolve it in deionized water, stir and mix it at room temperature and disperse it ultrasonically, add sodium chloroacetate and drop sodium hydroxide solution to adjust the pH of the system to 11-13, then place it in an oil bath at 100-120°C and heat it for 3-6 hours. After the reaction is completed, wash it with deionized water until it is neutral, then centrifuge and dry it to prepare carboxylated nano titanium dioxide; C. Take carboxylated nano-titanium dioxide in anhydrous butyl acetate and disperse it by ultrasonic, add epoxidized ethylene propylene rubber fully dissolved in xylene solvent, and add triphenylphosphine, place it at 90-120° C. and stir to react for 8-12 hours. After the reaction is completed, rotary evaporate and dry to prepare modified ethylene propylene rubber; The preparation method of the modified white carbon black comprises the following steps: (1) Ultrasonic dispersion of white carbon black in anhydrous ethanol, adding 5-isocyanate isophthaloyl chloride and dibutyltin dilaurate, stirring and reacting at 45-70° C. for 6-12 hours, centrifugation and vacuum drying after the reaction is completed, to prepare chlorinated white carbon black; (2) 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is placed in a reactor, diethanolamine and deionized water are added, the mixture is stirred at 80-95°C, and then paraformaldehyde is added, and the mixture is refluxed in a nitrogen atmosphere for 1-3 hours. After the reaction is completed, the mixture is subjected to rotary evaporation, washing, and drying to obtain a DOPO derivative; (3) Take acyl chloride silica and DOPO derivatives in N, N-dimethylacetamide, ultrasonically disperse them at room temperature, then add pyridine, and reflux at 120-135°C for 36-48 hours. After the reaction is completed, filter, wash, and dry to prepare modified silica.
2. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: The accelerator is a mixture of one or more of accelerator DM, accelerator M, accelerator TMTD, accelerator D, accelerator DTDM, and accelerator BZ; the antioxidant is a combination of one or more of N-phenyl-α-naphthylamine, N-phenyl-β-naphthylamine, and NN-diphenyl-p-phenylenediamine.
3. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: In the step A, the mass ratio of EPDM rubber, formic acid and hydrogen peroxide is 25-30:0.5-1.2:4-7.
4. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: In the step C, the mass ratio of carboxylated nano-titanium dioxide to epoxidized ethylene propylene diene monomer rubber is 1:1.2-2.
5. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: In the step (1), the mass ratio of white carbon black to 5-isocyanate isophthaloyl chloride is 1:0.5-1.
2.
6. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: In the step (2), the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diethanolamine and paraformaldehyde is 5-5.5:2-3:0.5-1.
7. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: In the step (3), the mass ratio of chlorinated white carbon black to DOPO derivative is 3-7:5-9.
8. The highly wear-resistant rubber composition for automobile tire tread according to claim 1, characterized in that: The preparation method of the rubber composition is specifically as follows: weighing each raw material by weight, adding natural rubber, modified EPDM rubber and butadiene rubber into a rubber mixing mill for plasticizing, adding modified white carbon black, nano zinc oxide, stearic acid and antioxidant for mixing for 3 to 5 minutes after the plasticizing is uniform, and finally adding sulfur and accelerator for mixing uniformly and vulcanizing at 120 to 160° C. for 8 to 10 minutes to prepare the rubber composition.