Method for preparing lithium carbonate by roasting in multi-layer furnace

By using multi-layer furnace roasting and replacing sodium sulfate with magnesium sulfate, the leaching rate of lepidolite and the purity of lithium carbonate are improved, solving the cumbersome process and solid waste treatment problems in the traditional process, and achieving cost-effective preparation of lithium carbonate.

CN118684248APending Publication Date: 2024-09-24HAICHENG MAGNESIUM FERTILIZER IND CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410889473.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-09-24

AI Technical Summary

Technical Problem

The traditional lepidolite roasting process has problems such as cumbersome process flow, low lithium leaching rate, difficult sodium sulfate solid waste treatment, and high potassium and sodium separation costs.

Method used

Using a multi-layer furnace roasting method, magnesium sulfate is used instead of sodium sulfate, and potassium and magnesium salts are formed by roasting lepidolite, calcium sulfate, and calcium carbonate to improve the leaching rate of lithium, and through multiple impurity removal and sodium carbonate precipitation processes, the lithium carbonate is improved. Purity and Economic Value.

Benefits of technology

It improves the leaching rate of lepidolite concentrate, solves the problem of sodium sulfate solid waste treatment, improves the purity and economic value of lithium carbonate, simplifies the process flow, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a lithium carbonate preparation method, in particular to a method for preparing lithium carbonate by roasting in a multi-layer furnace, the leaching rate of lepidolite concentrate can be improved by using the multi-layer furnace, and meanwhile, magnesium sulfate is used for replacing sodium sulfate in a traditional process, so that the problem of later sodium sulfate solid waste treatment is solved; meanwhile, potassium salt and magnesium salt (potassium sulfate and magnesium sulfate) in the process can be separated out in a crystal form to form potassium and magnesium salt (mixed salt) which can be directly used in a burdening process or chemical fertilizer recycling, so that the economic value during preparation of lithium carbonate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing lithium carbonate, in particular to a method for preparing lithium carbonate by roasting in a multi-layer furnace. Background Art

[0002] In the roasting of lithium mica concentrate, the traditional process is to add sodium sulfate and potassium sulfate to lithium mica concentrate to make agglomerates and then put them into rotary kilns or tunnel kilns for roasting. The disadvantages are that the agglomerates are made and then crushed in the early stage, the process is cumbersome, and the cost is increased; the contact with sulfate is insufficient, and the lithium leaching rate is low. Moreover, when sodium sulfate is used for mixed roasting, it is difficult to deal with the large amount of sodium sulfate solid waste in the later stage, and the separation technology of potassium and sodium is difficult to industrialize and the cost is high.

[0003] The existing patent CN116143149A discloses a method for preparing industrial-grade lithium carbonate using lithium-containing ore recovery materials, including the following process steps: A. sulfate roasting; B. acid leaching; C. lime magnesium removal; D. carbonization impurity removal; E. soda ash lithium precipitation. The existing patent discloses the use of magnesium sulfate instead of sodium sulfate to mix and burn lithium concentrate, but the method of removing a large amount of magnesium in the subsequent lithium extraction stage is not feasible. The magnesium hydroxide colloid filter press is difficult to handle, and removing a large amount of magnesium is a technical difficulty. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing lithium carbonate by roasting in a multi-layer furnace. The present invention uses a multi-layer furnace to improve the leaching rate of lithium mica concentrate, and uses magnesium sulfate to replace sodium sulfate in a traditional process, thereby solving the problem of treating sodium sulfate solid waste in the later stage. At the same time, potassium salt and magnesium salt (potassium sulfate and magnesium sulfate) in the process of the present invention can be precipitated in the form of crystals to form potassium-magnesium salt (mixed salt), which can be directly used in a batching process or recycled for fertilizer utilization, thereby improving the economic value of preparing lithium carbonate.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for calcining lithium carbonate using a multi-layer furnace, comprising:

[0007] S1, feeding lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate into a multi-layer furnace for roasting in a mass ratio of 1:0.3-0.5:0.18-0.185:0.1-0.3, the roasting temperature is 950-1200°C, and the roasting time is 2-3h;

[0008] S2, using the calcined lithium mica clinker as a raw material, and obtaining a lithium sulfate purified liquid through leaching, filtering, impurity removal, and filtering steps;

[0009] S3, pumping the purified lithium sulfate solution into a high-efficiency evaporator for evaporation and concentration, using steam for indirect heating at a temperature of 90-105° C., concentrating the leaching solution to a certain degree, and then pumping it into a lithium precipitation kettle; at this time, potassium salt and magnesium salt (potassium sulfate, magnesium sulfate) in the solution are precipitated in the form of crystals to form potassium magnesium salt (mixed salt), which is reused in the batching process or recycled for fertilizer use, and the evaporated condensed water is collected and reused;

[0010] S4, adding pure water to the lithium precipitation kettle to adjust the concentration, then adding sodium carbonate to the solution to precipitate lithium ions in the form of lithium carbonate, then performing solid-liquid separation to separate the lithium carbonate, and pumping the lithium precipitation mother liquor into the decarbonization process;

[0011] The chemical reaction formula is:

[0012] L i2SO4+Na2CO3→L i2CO3↓+Na2SO4

[0013] S5, the crude lithium carbonate separated by precipitation is washed with pure water to remove the impurities carried as much as possible, and the washing water is pumped into the decarbonization process. After the washing is completed, industrial-grade lithium carbonate is obtained;

[0014] S6, adding industrial grade lithium carbonate into the bicarbonation tower, adding pure water with a mass ratio of 1-1.5 times and stirring to form Li2CO3 slurry, then charging CO2 gas at a certain rate, after a certain period of carbonization reaction, obtaining LiHCO3 solution, filtering to remove impurities that are not carbonized;

[0015] The chemical reaction formula is: Li2CO3+CO2+H2O=2LiHCO3

[0016] S7, heating the filtered and purified LiHCO3 solution to 80-120° C. at a certain stirring rate, and gradually evaporating the solution during the stirring process to slowly precipitate Li2CO3 crystals;

[0017] The reaction equation is: 2LiHCO3=Li2CO3↓+CO2↑+H2O

[0018] S8, the precipitated Li2CO3 crystals are washed with pure water to remove the impurities carried by them as much as possible, and the washing water is pumped into the decarbonization process. After washing, it is dried with boiler steam to reduce its moisture content to below 0.25%. The dried dry Li2CO3 is sent to the air flow mill to be crushed to a particle size of 5um, and the fine powder enters the precision bag dust collector through the pressure difference for gas-solid separation to obtain Li2CO3 micropowder, and the two states of Li2CO3 are classified, packaged and stored.

[0019] Furthermore, in S1, the mass ratio of lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate is 1:0.3:0.185:0.2, the roasting temperature is 1050°C, and the roasting time is 2.5h.

[0020] Further, in S2, the lithium mica clinker is transported to the leaching kettle through a sealed pipeline by the power of a screw feeder, and water is added for leaching at a liquid-to-solid ratio of 1.5-3:1. The leaching time is 50-70 minutes. The leached slurry is sent to a filter press, and after filtering, pressing, washing, and pressing processes, leaching residue, leaching mother liquor, and washing water are obtained.

[0021] It should be noted that in S2, after the lithium mica is roasted, metal elements such as lithium, potassium, rubidium, and cesium exist in the form of sulfates that are easily soluble in water. The lithium mica clinker is sent to the leaching kettle and water is added in a certain proportion for leaching. The leaching process can make metal compounds such as lithium, potassium, rubidium, and cesium fully dissolved in water. After the leached slurry is sent to the filter press for treatment, the leached residue is mainly silicon dioxide, aluminum oxide, calcium fluoride, phosphide, phosphate, etc., which is sent to the tailings yard via a belt conveyor. The leached mother liquor is temporarily stored in the leaching liquid storage tank and then sent to the impurity removal process; the washing water is returned to the leaching process for use.

[0022] Furthermore, S2 also includes an impurity removal process, wherein the leaching mother liquor is sent to a purification and impurity removal tank, and the pH is adjusted to 13-13.5 with NaOH to form hydroxide precipitation and phosphide and phosphate precipitation of aluminum, iron, calcium, magnesium, manganese, etc. 2+ Mg 2+ Na2CO3 is added according to the excess coefficient of 5% to form calcium carbonate and magnesium carbonate precipitation, and finally a purified impurity-removed slurry is obtained. The purified impurity-removed slurry enters a filter press, and after filtering and pressing processes, impurity-removed slag, impurity-removed mother liquor (i.e., lithium sulfate purified liquid), and washing water are obtained;

[0023] Reaction equation for impurity removal and purification:

[0024] M n+ +nOH - = =M(OH) n ; Where n = 2 or 3, M represents the hydrolysis precipitation reaction of aluminum, iron, calcium, magnesium, manganese, etc.;

[0025] M 2+ +CO3 2- ==MCO 3; ; M represents the precipitation reaction of carbonates such as calcium and magnesium.

[0026] It should be noted that in S2, after the impurity removal process, the impurity removal slag mainly includes calcium carbonate, magnesium carbonate, aluminum hydroxide, iron hydroxide, phosphide, phosphate, etc., which are sent to the tailings yard via a belt conveyor; the impurity removal mother liquor is temporarily stored in the impurity removal mother liquor storage tank and then sent to the concentration process; the washing water is sent back to the leaching process for use.

[0027] Further, in S3, the leaching solution is concentrated to 60-80% of the volume of the original solution and then pumped into the lithium precipitation kettle.

[0028] Furthermore, in S4, when pure water is added to the lithium precipitation kettle to adjust the concentration, the amount of water added is 20-40% of the mass of the solution, and then 5-10% of the mass of sodium carbonate is added to the solution to precipitate lithium ions in the form of lithium carbonate.

[0029] Furthermore, in S6, the CO2 gas introduction rate is 8-15 mg / min, and the carbonization reaction time is 40-80 min.

[0030] It should be noted that in S6, the carbonization reaction is a "gas-liquid-solid" three-phase reaction system, which uses CO2 gas to convert Li2CO3 into LiHCO3 with much greater solubility at a certain temperature, while other impurity carbonates are not easily carbonized and can be removed by filtration.

[0031] Further, in S7, the stirring rate is 50-100 r / min, and the temperature is heated to 90-100°C.

[0032] It should be noted that in S7, the LiHCO3 solution is heated and decomposed to obtain Li2CO3 crystals. The decomposition reaction process essentially represents the coupling of the thermal decomposition of LiHCO3 in the solution and the reaction crystallization of Li2CO3. The key to this process is to control the temperature and the heating rate. The higher the temperature, on the one hand, is conducive to increasing the decomposition rate of LiHCO3, and is also conducive to the diffusion of ions in the solution, thereby accelerating the nucleation rate of Li2CO3 crystallization; on the other hand, increasing the temperature will also increase the purity of the Li2CO3 product.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. In the impurity removal process of the present invention, NaOH is first used to adjust the pH to form hydroxide precipitation and phosphide and phosphate precipitation of aluminum, iron, calcium, magnesium, manganese, etc. in the leaching mother liquor, which is equivalent to one impurity removal. Then Na2CO3 is added to form calcium carbonate and magnesium carbonate precipitation to achieve secondary impurity removal. The two impurity removals reduce the impurity content in the solution, thereby improving the purity of the subsequent preparation of lithium carbonate;

[0035] 2. In the present invention, magnesium sulfate replaces sodium sulfate in the traditional process, so that the potassium salt and magnesium salt produced subsequently can be precipitated in the form of crystals to form potassium and magnesium salts, which can be directly used in the batching process or recycled for fertilizer utilization, thereby improving the economic value;

[0036] 3. The multi-layer furnace is used for roasting. The unique structure greatly improves the processing capacity of the equipment compared with the traditional rotary kiln. At the same time, the roasting temperature in the multi-layer furnace is stably controlled, which can improve the lithium leaching rate when roasting lithium mica concentrate. DETAILED DESCRIPTION

[0037] The technical solutions in the present invention will be described clearly and completely in conjunction with the embodiments below. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] A method for calcining lithium carbonate using a multi-layer furnace, comprising:

[0040] S1, lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate are sent into a multi-layer furnace for roasting at a mass ratio of 1:0.3:0.185:0.2, the roasting temperature is 1050°C, and the roasting time is 2.5h:

[0041] S2, the lithium mica clinker is transported to the leaching kettle through the power of a screw feeder through a sealed pipeline, and water is added for leaching at a liquid-to-solid ratio of 2:1, and the leaching time is 60min. The leached slurry is sent to a filter press, and after filtering, squeezing, washing, and squeezing processes, leached residue, leaching mother liquor, and washing water are obtained;

[0042] The leaching mother liquor is sent to the purification and impurity removal tank, and the pH is adjusted to 13 with NaOH to form hydroxide precipitation of aluminum, iron, calcium, magnesium, manganese, etc. and phosphide and phosphate precipitation. 2+ Mg 2+ Na2CO3 is added according to the excess coefficient of 5% to form calcium carbonate and magnesium carbonate precipitation, and finally a purified impurity-removed slurry is obtained. The purified impurity-removed slurry enters a filter press, and after filtering and pressing processes, impurity-removed slag, impurity-removed mother liquor (i.e., lithium sulfate purified liquid), and washing water are obtained;

[0043] S3, pumping the purified lithium sulfate solution into a high-efficiency evaporator for evaporation and concentration, using steam for indirect heating at a temperature of 95° C., concentrating the leaching solution to 70% of the original solution volume, and then pumping it into a lithium precipitation kettle; at this time, potassium salt and magnesium salt (potassium sulfate, magnesium sulfate) in the solution are precipitated in the form of crystals to form potassium and magnesium salts (mixed salts), which are reused in the batching process or recycled for fertilizer use, and the evaporated condensed water is collected and reused;

[0044] S4, adding 30% pure water by weight to the lithium precipitation kettle to adjust the concentration, then adding 5% sodium carbonate to the solution to precipitate lithium ions in the form of lithium carbonate, then performing solid-liquid separation to separate the lithium carbonate, and pumping the lithium precipitation mother liquor into the decarbonization process;

[0045] The chemical reaction formula is:

[0046] L i2SO4+Na2CO3→L i2CO3↓+Na2SO4

[0047] S5, the crude lithium carbonate separated by precipitation is washed with pure water to remove the impurities carried as much as possible, and the washing water is pumped into the decarbonization process. After the washing is completed, industrial-grade lithium carbonate is obtained;

[0048] S6, adding industrial grade lithium carbonate into the bicarbonate tower, adding pure water with a mass ratio of 1 and stirring to form Li2CO3 slurry, then passing CO2 gas at a rate of 10 mg / min, and after carbonization reaction for 60 minutes, obtaining LiHCO3 solution, filtering to remove impurities that are not carbonized;

[0049] The chemical reaction formula is: Li2CO3+CO2+H2O=2LiHCO3

[0050] S7, heating the filtered and purified LiHCO3 solution to about 95°C at a stirring rate of 70 r / min, and the solution gradually evaporates during the stirring process to slowly precipitate Li2CO3 crystals;

[0051] The reaction equation is: 2LiHCO3=Li2CO3↓+CO2↑+H2O

[0052] S8, the precipitated Li2CO3 crystals are washed with pure water to remove the impurities carried by them as much as possible, and the washing water is pumped into the decarbonization process. After washing, it is dried with boiler steam to reduce its moisture content to below 0.25%. The dried dry Li2CO3 is sent to the air flow mill to be crushed to a particle size of 5um, and the fine powder enters the precision bag dust collector through the pressure difference for gas-solid separation to obtain Li2CO3 micropowder, and the two states of Li2CO3 are classified, packaged and stored.

[0053] Example 2

[0054] A method for calcining lithium carbonate using a multi-layer furnace, comprising:

[0055] S1, feeding lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate into a multi-layer furnace for roasting in a mass ratio of 1:0.4:0.18:0.1, at a roasting temperature of 1000°C for 2h;

[0056] S2, the lithium mica clinker is transported to the leaching kettle through the power of a screw feeder through a sealed pipeline, and water is added for leaching at a liquid-to-solid ratio of 1.5:1, and the leaching time is 70min. The leached slurry is sent to a filter press, and after filtering, squeezing, washing, and squeezing processes, leached residues, leached mother liquor, and washing water are obtained;

[0057] The leaching mother liquor is sent to the purification and impurity removal tank, and the pH is adjusted to 13.5 with NaOH to form hydroxide precipitation of aluminum, iron, calcium, magnesium, manganese, etc. and phosphide and phosphate precipitation. 2+ Mg 2+Na2CO3 is added according to the excess coefficient of 5% to form calcium carbonate and magnesium carbonate precipitation, and finally a purified impurity-removed slurry is obtained. The purified impurity-removed slurry enters a filter press, and after filtering and pressing processes, impurity-removed slag, impurity-removed mother liquor (i.e., lithium sulfate purified liquid), and washing water are obtained;

[0058] S3, pumping the purified lithium sulfate solution into a high-efficiency evaporator for evaporation and concentration, using steam for indirect heating at a temperature of 100° C., concentrating the leaching solution to 60-80% of the original solution volume and then pumping it into a lithium precipitation kettle; at this time, potassium salt and magnesium salt (potassium sulfate, magnesium sulfate) in the solution precipitate in the form of crystals to form potassium-magnesium salt (mixed salt);

[0059] S4, adding 25% pure water by weight to the lithium precipitation kettle to adjust the concentration, then adding 7% sodium carbonate by weight to the solution to precipitate lithium ions in the form of lithium carbonate, then performing solid-liquid separation to separate the lithium carbonate, and pumping the lithium precipitation mother liquor into the decarbonization process;

[0060] The chemical reaction formula is:

[0061] L i2SO4+Na2CO3→L i2CO3↓+Na2SO4

[0062] S5, the crude lithium carbonate separated by precipitation is washed with pure water to remove the impurities carried as much as possible, and the washing water is pumped into the decarbonization process. After the washing is completed, industrial-grade lithium carbonate is obtained;

[0063] S6, adding industrial grade lithium carbonate into the bicarbonate tower, adding pure water with a mass ratio of 1 and stirring to form Li2CO3 slurry, then introducing CO2 gas at a rate of 8 mg / min, carbonizing for 80 minutes to obtain LiHCO3 solution, and filtering to remove impurities that are not carbonized;

[0064] The chemical reaction formula is: Li2CO3+CO2+H2O=2LiHCO3

[0065] S7, heating the filtered and purified LiHCO3 solution to 98°C at a stirring rate of 80 r / min, and gradually evaporating the solution during the stirring process to slowly precipitate Li2CO3 crystals;

[0066] The reaction equation is: 2LiHCO3=Li2CO3↓+CO2↑+H2O

[0067] S8, the precipitated Li2CO3 crystals are washed with pure water to remove the impurities carried by them as much as possible, and the washing water is pumped into the decarbonization process. After washing, it is dried with boiler steam to reduce its moisture content to below 0.25%. The dried dry Li2CO3 is sent to the air flow mill to be crushed to a particle size of 5um, and the fine powder enters the precision bag dust collector through the pressure difference for gas-solid separation to obtain Li2CO3 micropowder, and the two states of Li2CO3 are classified, packaged and stored.

[0068] Example 3

[0069] A method for calcining lithium carbonate using a multi-layer furnace, comprising:

[0070] S1, feeding lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate into a multi-layer furnace for roasting in a mass ratio of 1:0.5:0.18:0.2, at a roasting temperature of 1100°C, and roasting for 3 hours;

[0071] S2, the lithium mica clinker is transported to the leaching kettle through the power of a screw feeder through a sealed pipeline, and water is added for leaching at a liquid-to-solid ratio of 2:1, and the leaching time is 60min. The leached slurry is sent to a filter press, and after filtering, squeezing, washing, and squeezing processes, leached residue, leaching mother liquor, and washing water are obtained;

[0072] The leaching mother liquor is sent to the purification and impurity removal tank, and the pH is adjusted to 13.5 with NaOH to form hydroxide precipitation of aluminum, iron, calcium, magnesium, manganese, etc. and phosphide and phosphate precipitation. 2+ Mg 2+ Na2CO3 is added according to the excess coefficient of 5% to form calcium carbonate and magnesium carbonate precipitation, and finally a purified impurity-removed slurry is obtained. The purified impurity-removed slurry enters a filter press, and after filtering and pressing processes, impurity-removed slag, impurity-removed mother liquor (i.e., lithium sulfate purified liquid), and washing water are obtained;

[0073] S3, pumping the purified lithium sulfate solution into a high-efficiency evaporator for evaporation and concentration, using steam for indirect heating at a temperature of 100° C., concentrating the leaching solution to 60% of the original solution volume and then pumping it into a lithium precipitation kettle; at this time, potassium salt and magnesium salt (potassium sulfate, magnesium sulfate) in the solution precipitate in the form of crystals to form potassium-magnesium salt (mixed salt);

[0074] S4, adding 40% pure water by weight to the lithium precipitation kettle to adjust the concentration, then adding 10% sodium carbonate by weight to the solution to precipitate lithium ions in the form of lithium carbonate, then performing solid-liquid separation to separate the lithium carbonate, and pumping the lithium precipitation mother liquor into the decarbonization process;

[0075] The chemical reaction formula is:

[0076] L i2SO4+Na2CO3→L i2CO3↓+Na2SO4

[0077] S5, the crude lithium carbonate separated by precipitation is washed with pure water to remove the impurities carried as much as possible, and the washing water is pumped into the decarbonization process. After the washing is completed, industrial-grade lithium carbonate is obtained;

[0078] S6, adding industrial grade lithium carbonate into the bicarbonate tower, adding pure water with a mass ratio of 1.5 times and stirring to form Li2CO3 slurry, then passing CO2 gas at a rate of 12 mg / min, carbonizing reaction for 50 minutes to obtain LiHCO3 solution, and filtering to remove impurities that are not carbonized;

[0079] The chemical reaction formula is: Li2CO3+CO2+H2O=2LiHCO3

[0080] S7, heating the filtered and purified LiHCO3 solution to 100°C at a stirring rate of 80 r / min, wherein the solution gradually evaporates during the stirring process and Li2CO3 crystals are slowly precipitated;

[0081] The reaction equation is: 2LiHCO3=Li2CO3↓+CO2↑+H2O

[0082] S8, the precipitated Li2CO3 crystals are washed with pure water to remove the impurities carried by them as much as possible, and the washing water is pumped into the decarbonization process. After washing, it is dried with boiler steam to reduce its moisture content to below 0.25%. The dried dry Li2CO3 is sent to the air flow mill to be crushed to a particle size of 5um, and the fine powder enters the precision bag dust collector through the pressure difference for gas-solid separation to obtain Li2CO3 micropowder, and the two states of Li2CO3 are classified, packaged and stored.

[0083] Comparative Example 1

[0084] Comparative Example 1 is the same as Example 1, except that in S1, lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate are fed into a rotary kiln for roasting in a mass ratio of 1:0.3:0.185:0.2, the roasting temperature is 1050° C., and the roasting time is 2.5 hours.

[0085] Comparative Example 2

[0086] Comparative Example 2 is the same as Example 1, except that in S2, the lepidolite clinker is transported to a leaching kettle through a sealed pipeline by the power of a screw feeder, and water is added for leaching at a liquid-to-solid ratio of 2:1, and the leaching time is 60 min. The leached slurry is sent to a filter press, and leached residue, leaching mother liquor, and washing water are obtained through filtering, squeezing, washing, and squeezing processes;

[0087] The leaching mother liquor is sent to the purification and impurity removal tank, and the pH is adjusted to 13 with NaOH to form hydroxide precipitates and phosphide and phosphate precipitates of aluminum, iron, calcium, magnesium, manganese, etc., and finally a purified impurity removal slurry is obtained. The purified impurity removal slurry is sent to the filter press, and after filtering and pressing processes, impurity removal residues, impurity removal mother liquor (i.e., lithium sulfate purification liquid) and washing water are obtained.

[0088] Comparative Example 3

[0089] Comparative Example 2 is the same as Example 1, except that step S3 is not implemented.

[0090] Comparative Example 4

[0091] Comparative Example 2 is the same as Example 1, except that in S7, the filtered and purified LiHCO3 solution is heated to 85°C at a stirring rate of 70 r / min. During the stirring process, the solution gradually evaporates and Li2CO3 crystals are slowly precipitated.

[0092] Comparative Example 5

[0093] Comparative Example 5 is the same as Example 2, except that in S1, lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate are fed into a multi-layer furnace for calcination at a mass ratio of 1:0.4:0.18:0.1, the calcination temperature is 1300° C., and the calcination time is 2 h.

[0094] Comparative Example 6

[0095] Comparative Example 6 is the same as Example 2, except that in S2, the lepidolite clinker is transported to the leaching kettle through a sealed pipeline by the power of a screw feeder, and water is added for leaching at a liquid-to-solid ratio of 1.5:1, and the leaching time is 70 min. The leached slurry is sent to a filter press, and leached residue, leaching mother liquor, and washing water are obtained through filtering, squeezing, washing, and squeezing processes;

[0096] The leaching mother liquor is sent to the purification and impurity removal tank, according to Ca 2+ Mg 2+ Na2CO3 is added according to an excess coefficient of 5% to form calcium carbonate and magnesium carbonate precipitates, and finally a purified and impurity-removed slurry is obtained. The purified and impurity-removed slurry enters a filter press, and after filtering and pressing processes, impurity-removed residues, impurity-removed mother liquor (i.e., lithium sulfate purified liquid) and washing water are obtained.

[0097] Comparative Example 7

[0098] Comparative Example 7 is the same as Example 2, except that step S3 is not implemented.

[0099] Comparative Example 8

[0100] Comparative Example 8 is the same as Example 2, except that in S7, the filtered and purified LiHCO3 solution is heated to 120°C at a stirring rate of 80 r / min, and the solution gradually evaporates during the stirring process to slowly precipitate Li2CO3 crystals.

[0101] Li2CO3 purity test

[0102] The detection method is to weigh 0.5g of the Li2CO3 powder prepared in Examples 1-3 and Comparative Examples 1-8 as Li2CO3 samples, accurately to 0.0001g, and put them into a beaker; add an appropriate amount of distilled water to the beaker, and stir it on a magnetic stirrer to ensure that the sample is completely dissolved; add a few drops of phenolphthalein indicator, and the solution is pink; slowly add a standard hydrochloric acid solution from a burette to the lithium carbonate solution until the color becomes colorless, and record the volume of hydrochloric acid used; slowly titrate the above solution with a standard sodium hydroxide solution until the solution is pink again, and record the volume of sodium hydroxide used. Repeat the titration process at least twice, and take the average value to improve the experimental accuracy.

[0103] Table 1 shows the average purity of Li2CO3 in two tests

[0104]

[0105] It can be seen from the data in Table 1 that the purity of Li2CO3 obtained in Examples 1-3 is all above 99.95%. This is because in the impurity removal process of the present invention, NaOH is first used to adjust the pH value of the leaching mother liquor to form hydroxide precipitates and phosphide and phosphate precipitates of aluminum, iron, calcium, magnesium, manganese, etc., which is equivalent to primary impurity removal. Na2CO3 is then added to form calcium carbonate and magnesium carbonate precipitates. The two impurity removals reduce the impurity content in the solution.

[0106] In addition, after the industrial-grade lithium carbonate is formed, the present invention adds pure water and injects CO2 gas to carbonize it to form a LiHCO3 solution. By converting Li2CO3 into LiHCO3 with much greater solubility, other impurity carbonates are not easily carbonized and can be removed by filtration, which further removes impurities in the solution. The LiHCO3 solution is heated and decomposed to obtain Li2CO3 crystals. In the present invention, impurities in the solution are more thoroughly removed in a multi-stage manner, so that the finally formed Li2CO3 has high purity.

[0107] Compared with the data of Example 1, Comparative Example 1 uses a traditional rotary kiln for roasting, and the leaching rate of lithium is low, so that the purity of the lithium carbonate produced subsequently is low; from the data of Comparative Examples 2-3 and Comparative Examples 6-7, it can be seen that Comparative Examples 2, 3, 6 and 7 do not fully adopt a multi-stage impurity removal method, which makes the amount of impurities removed in the solution relatively small, thereby affecting the purity of Li2CO3. From the data of Comparative Examples 4 and 8, it can be seen that when the LiHCO3 solution is heated and decomposed, when the temperature is low, it is not conducive to the nucleation of Li2CO3 crystallization, and when the temperature is high, the crystallization rate of Li2CO3 does not increase, and is even suppressed, which shows that the appropriate temperature can make the coupling efficiency of LiHCO3 thermal decomposition and Li2CO3 reaction crystallization the highest.

[0108] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for calcining lithium carbonate using a multi-layer furnace, characterized in that: include: S1, feeding lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate into a multi-layer furnace for roasting in a mass ratio of 1:0.3-0.5:0.18-0.185:0.1-0.3, the roasting temperature is 950-1200°C, and the roasting time is 2-3h; S2, using the calcined lithium mica clinker as a raw material, and obtaining a lithium sulfate purified liquid through leaching, filtering, impurity removal, and filtering steps; S3, pumping the purified lithium sulfate liquid into a high-efficiency evaporator for evaporation and concentration, using steam for indirect heating at a temperature of 90-105°C, concentrating the leaching solution to a certain degree, and then pumping it into a lithium precipitation kettle; at this time, potassium salt and magnesium salt in the solution precipitate in the form of crystals to form potassium and magnesium salts, wherein the potassium salt is potassium sulfate and the magnesium salt is magnesium sulfate, which are reused in the batching process or recycled for fertilizer use, and the evaporated condensed water is collected and reused; S4, adding pure water to the lithium precipitation kettle to adjust the concentration, then adding sodium carbonate to the solution to precipitate lithium ions in the form of lithium carbonate, then performing solid-liquid separation to separate the lithium carbonate, and pumping the lithium precipitation mother liquor into the decarbonization process; The chemical reaction formula is: Li2SO4+Na2CO3→Li2CO3↓+Na2SO4 S5, the crude lithium carbonate separated by precipitation is washed with pure water to remove the impurities carried as much as possible, and the washing water is pumped into the decarbonization process. After the washing is completed, industrial-grade lithium carbonate is obtained; S6, adding industrial-grade lithium carbonate into a hydrogenation tower, adding 1-1.5 times of pure water by mass ratio and stirring to form a Li2CO3 slurry, then charging CO2 gas at a certain rate, after a certain period of carbonization reaction, obtaining a LiHCO3 solution, filtering to remove impurities that are not carbonized; The chemical reaction formula is: Li2CO3+CO2+H2O=2LiHCO3 S7, heating the filtered and purified LiHCO3 solution to 80-120° C. at a certain stirring rate, and gradually evaporating the solution during the stirring process to slowly precipitate Li2CO3 crystals; The reaction equation is: 2LiHCO3=Li2CO3↓+CO2↑+H2O S8, the precipitated Li2CO3 crystals are washed with pure water to remove the impurities carried by them as much as possible, and the washing water is pumped into the decarbonization process. After washing, it is dried with boiler steam to reduce its moisture content to below 0.25%. The dried dry Li2CO3 is sent to the air flow mill to be crushed to a particle size of 5um, and the fine powder enters the precision bag dust collector through the pressure difference for gas-solid separation to obtain Li2CO3 micropowder, and the two states of Li2CO3 are classified, packaged and stored.

2. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: In S1, the mass ratio of lepidolite, calcium sulfate, magnesium sulfate and calcium carbonate is 1:0.3:0.185:0.2, the roasting temperature is 1050°C, and the roasting time is 2.5h.

3. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: In S2, the lithium mica clinker is transported to the leaching kettle through a sealed pipeline by the power of a screw feeder, and water is added for leaching at a liquid-to-solid ratio of 1.5-3:

1. The leaching time is 50-70 minutes. The leached slurry is sent to a filter press, and after filtering, pressing, washing, and pressing processes, leaching residue, leaching mother liquor, and washing water are obtained.

4. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: S2 also includes a decontamination process, in which the leaching mother liquor is sent to a purification and decontamination tank, and the pH is adjusted to 13-13.5 with NaOH to form hydroxide precipitation of aluminum, iron, calcium, magnesium, manganese, etc. and phosphide and phosphate precipitation. 2+ Mg 2+ Na2CO3 is added according to the excess coefficient of 5% to form calcium carbonate and magnesium carbonate precipitation, and finally a purified impurity-removed slurry is obtained. The purified impurity-removed slurry enters a filter press, and after filtering and pressing processes, impurity-removed slag, impurity-removed mother liquor (i.e., lithium sulfate purified liquid), and washing water are obtained; Reaction equation for impurity removal and purification: M n+ +nOH - = =M(OH) n ; Where n = 2 or 3, M represents the hydrolysis precipitation reaction of aluminum, iron, calcium, magnesium, and manganese; M 2+ +CO3 2- ==MCO3; M represents calcium and magnesium carbonate precipitation reaction.

5. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: In S3, the leaching solution is concentrated to 60-80% of the original solution volume and then pumped into the lithium precipitation kettle.

6. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: In S4, when pure water is added to the lithium precipitation kettle to adjust the concentration, the amount of water added is 20-40% of the mass of the solution, and then 5-10% of the mass of sodium carbonate is added to the solution to precipitate lithium ions in the form of lithium carbonate.

7. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: In S6, the CO2 gas introduction rate is 8-15 mg / min, and the carbonization reaction time is 40-80 min.

8. A method for calcining lithium carbonate using a multi-layer furnace according to claim 1, characterized in that: In S7, the stirring rate is 50-100 r / min and the temperature is heated to 90-100°C.

Citation Information

Cited By

  • Industrial furnace fan and method for extracting lithium by sintering lepidolite under assistance of spodumene desulfurization plate frame slag

    CN121205962A

  • Industrial furnace fan and lithium mica lithium extraction method by spodumene desulfurization plate frame slag assisted burning

    CN121205962B