A flame retardant, ageing-resistant composite rubber material and its preparation method and application

Through the melt blending and vulcanization molding of modified graphene and ethylene propylene ternary rubber, the problems of flammability and inefficiency of rubber materials are solved, and efficient flame retardant and aging resistance are improved, and smoke release is avoided. Green and environmentally friendly characteristics.

CN118703001BActive Publication Date: 2024-12-03赵灵芝
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411183139.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Rubber materials are flammable and not resistant to aging. The existing flame-retardant composite materials release toxic smoke during combustion and have poor UV aging resistance.

Method used

By placing carboxylated graphene with N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphophenophen-10-yl)methyl]-1,3,5-triazine -2,4,6-triamine and 4-dimethylaminopyridine react to form modified graphene, and melt blended with ethylene propylene ternary rubber, styrene butadiene rubber and anti-aging agent are added, and the formation is formed by vulcanization. Composite rubber material with flame retardant and aging resistance.

Benefits of technology

It improves the flame retardant and aging resistance of composite rubber materials, avoids smoke release, has green and environmentally friendly characteristics, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of rubber materials, and discloses an anti-aging composite rubber material with flame retardant effect, a preparation method and application thereof. Modified EPDM rubber and styrene-butadiene rubber are used as raw materials, and the composite rubber material is obtained through mixing, refining and vulcanization molding under the joint action of an antioxidant, a lubricant, a vulcanizing agent, an activator zinc oxide and stearic acid. The organic flame retardant and graphene introduced into the composite rubber material work synergistically, and when heated and burned, a denser and impermeable carbon layer is generated on the surface of the matrix to prevent heat conduction. The flame retardant component used does not contain halogen and has the characteristics of being green and environmentally friendly. An ultraviolet absorber is introduced and works together with graphene and styrene-butadiene rubber, so that the composite rubber material has excellent ultraviolet aging resistance and heat-oxidation aging resistance, good processing performance, high production efficiency, can be applied to the fields of automotive parts, electronic appliances, etc., and has excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber materials, in particular to an ageing-resistant composite rubber material with flame retardancy and a preparation method and application thereof. Background Art

[0002] Rubber is a polymer elastic material. Due to its excellent elasticity, sealing and wear resistance, it is widely used in electronics, automobiles, construction, aerospace and other fields. However, rubber materials are easy to burn when encountering fire or high temperature environment, and may spread rapidly, posing a certain threat to people's property safety and personal safety, which limits its application scope. During use, rubber materials are often affected by factors such as heat, oxygen, light, and ozone, which causes aging, resulting in performance degradation, discoloration, hardening, brittleness and other problems, which seriously affects the service life of rubber materials. Therefore, the development of composite rubber materials with flame retardant and aging resistance has become a hot topic in current research.

[0003] Chinese patent application CN107868348A discloses a highly flame-retardant conductive EPDM rubber and its preparation method, which is composed of the following components: EPDM rubber, zinc oxide, stearic acid, aluminum hydroxide, conductive carbon black, paraffin oil, decabromodiphenylethane, antimony trioxide, accelerator, sulfur, and the flame retardant system is made of aluminum hydroxide, decabromodiphenylethane, and antimony trioxide. The flame retardant performance of the obtained EPDM rubber is greatly improved, and the comprehensive performance is good. Adding flame retardants is an effective method to improve the flame retardancy of rubber, but halogen-containing compounds are easy to release a large amount of smoke and toxic gases when burning, which is easy to cause environmental pollution and endanger human health. At the same time, the aging resistance of the EPDM rubber is average. Chinese patent application CN105585780A discloses a flame retardant and heat aging resistant EPDM composite material, the raw materials of which include: EPDM, chlorinated butyl rubber, natural rubber, chlorinated polyethylene, maleic anhydride grafted ethylene-vinyl acetate copolymer, carbon black, carbon nanotubes, calcined kaolin, montmorillonite, zinc oxide, stearic acid, sulfur, dilauroyl peroxide, antioxidant, accelerator TMTD, accelerator BZ, accelerator CZ, anti-scorch agent, samarium trioxide, phenyltrimethoxysilane. The composite material has good flame retardancy and heat aging resistance, but poor ultraviolet aging resistance, and directly adding various inorganic materials has poor dispersibility and greatly reduced comprehensive performance. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In order to solve the above technical problems, the present invention provides an aging-resistant composite rubber material with flame retardant effect and a preparation method and application thereof, which solves the problems of flammability and poor aging resistance of rubber materials.

[0006] (II) Technical solution

[0007] In order to achieve the above object, the present invention discloses a method for preparing an aging-resistant composite rubber material with flame retardant effect, comprising the following steps:

[0008] Step 1, adding carboxylated graphene to an organic solvent, ultrasonically dispersing it uniformly, then adding N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, dicyclohexylcarbodiimide and 4-dimethylaminopyridine, mixing them uniformly, reacting, after the reaction is completed, filtering, washing with anhydrous ethanol, and vacuum drying at 60° C. for 12 hours to obtain modified graphene;

[0009] Step 2: Evenly mix ethylene propylene diene monomer rubber, glycidyl methacrylate, styrene, 4-acryloxy-2-hydroxybenzophenone and an initiator, transfer the mixture to a twin-screw extruder for a melt reaction, extrude the mixture after the reaction is completed, and cool the mixture to obtain epoxidized ethylene propylene diene monomer rubber;

[0010] Step 3, uniformly mixing the EPDM rubber, the epoxidized EPDM rubber and the modified graphene, transferring the mixture to a torque rheometer for melt blending, and cooling the mixture after the reaction to obtain the modified EPDM rubber;

[0011] Step 4: Add modified EPDM rubber, styrene-butadiene rubber, antioxidant and lubricant to an internal mixer in sequence, mix at 105-115°C for 8-12 minutes, then add vulcanizer, zinc oxide and stearic acid, mix for 12-15 minutes to obtain a mixed product, and refining the mixed product in an open mixer. After the refining is completed, blow dry and cool, place for 24 hours to obtain a mixed rubber, and then transfer it to a flat vulcanizer for vulcanization molding, discharging, and obtaining an aging-resistant composite rubber material with flame retardant effect.

[0012] Preferably, in the step 1, the mass ratio of carboxylated graphene, organic solvent, N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine is 100:3800-4500:155-210:28-40:9-15, the reaction temperature is 25-35°C, and the reaction time is 6-9h.

[0013] Preferably, the carboxylated graphene in step 1 can be prepared by the following method: 40 mL of graphene oxide dispersion and 60 mL of deionized water are mixed evenly, and then 5.0 g of sodium hydroxide and 7.5 g of sodium chloroacetate are added, mixed for 8 hours, centrifuged at a rate of 8000 r / min, centrifuged for 5 minutes, washed, neutralized, dialyzed, and dried at 60° C. for 12 hours to obtain carboxylated graphene.

[0014] Furthermore, the graphene oxide dispersion was purchased from Beijing Carbon Century Technology Co., Ltd., model number CCTGO-204.

[0015] Preferably, the organic solvent in step 1 comprises any one or more of N,N-dimethylformamide, toluene and tetrahydrofuran.

[0016] Preferably, in the step 2, the mass ratio of EPDM rubber, glycidyl methacrylate, styrene, 4-acryloxy-2-hydroxybenzophenone and initiator is 100:3-4:0.5-0.8:4-6:3-5.

[0017] Preferably, the initiator in step 2 is dicumyl peroxide.

[0018] Preferably, during the melting reaction in step 2, the rotor speed is 100 r / min, the melting reaction temperature is 220-240° C., and the melting reaction time is 5 min.

[0019] Preferably, in step three, the mass ratio of EPDM rubber, epoxidized EPDM rubber and modified graphene is 100:12-18:5-8.

[0020] Preferably, during the melt blending process in step 3, the rotor speed is 50 r / min, the melt blending temperature is 225-235° C., and the melt blending time is 5 min.

[0021] Preferably, in step 4, the mass ratio of the modified EPDM rubber, styrene-butadiene rubber, antioxidant, lubricant, vulcanizing agent, zinc oxide and stearic acid is 100:5-8:0.3-0.5:1-2:2-3:1-2:0.5-1.5.

[0022] Preferably, the antioxidant in step 4 is N,N'-di(β-naphthyl)-p-phenylenediamine.

[0023] Preferably, the lubricant in step 4 is pentaerythritol stearate.

[0024] Preferably, the vulcanizing agent in step 4 is di-tert-butyl peroxide isopropylbenzene.

[0025] Preferably, in the step 4, the temperature of the rolling in the open mill is 110-130° C., and the rolling time is 9-12 min.

[0026] Preferably, in the step 4, the temperature of the vulcanization molding in the flat vulcanizing agent is 160-180° C., and the vulcanization molding time is 12-18 minutes.

[0027] A flame retardant and aging resistant composite rubber material prepared by the method for preparing the flame retardant and aging resistant composite rubber material.

[0028] The invention discloses an application of the ageing-resistant composite rubber material with flame retardancy in automobile parts and electronic appliances.

[0029] 3. Beneficial technical effects

[0030] (1) In the present invention, carboxylated graphene is first modified, and the carboxyl groups on the surface of the carboxylated graphene and the amino groups on N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine undergo amidation reaction under the action of dicyclohexylcarbodiimide and 4-dimethylaminopyridine, and an organic flame retardant is introduced on the surface of the graphene to obtain modified graphene. EPDM rubber, glycidyl methacrylate, styrene, and 4-acryloyloxy-2-hydroxybenzophenone undergo in-situ polymerization under the action of an initiator, and epoxy groups and hydroxybenzophenone are introduced on the EPDM rubber to obtain epoxidized EPDM rubber. The unreacted amino groups on the surface of modified graphene react with the epoxy groups on the epoxidized EPDM rubber to undergo a ring-opening reaction, and are mixed with the EPDM rubber to obtain modified EPDM rubber, which effectively improves the compatibility between the raw materials, improves the dispersibility, and improves the comprehensive performance of the composite rubber material. Using modified EPDM rubber and styrene-butadiene rubber as raw materials, under the joint action of antioxidants, lubricants, vulcanizers, activators zinc oxide and stearic acid, through mixing, refining, and vulcanization molding, a flame-retardant and aging-resistant composite rubber material is obtained.

[0031] (2) The graphene used in the present invention has excellent mechanical properties and can effectively improve the mechanical properties of the matrix. At the same time, graphene also has excellent flame retardant properties and resistance to thermal oxygen aging. Due to its small size, it can effectively reflect ultraviolet rays and has anti-ultraviolet ability. An organic flame retardant is introduced on the surface of graphene, which contains phosphorus heterocycles and amino groups. During the combustion process of the matrix, the phosphorus heterocycles will generate acidic substances such as phosphoric acid and phosphorous acid, which promote the carbonization of the matrix and prevent the combustion reaction from proceeding. The PO· free radicals generated during the combustion process can capture ·OH and H· free radicals in the flame, interrupt the combustion chain reaction, and reduce the heat released by the combustion. At the same time, a large amount of nitrogen-containing non-combustible gas will be generated, which effectively dilutes the concentration of oxygen in the combustion system and further improves the flame retardant effect. During the combustion process, graphene can char and form a dense carbon layer, which can effectively block the surface from contacting oxygen or flammable gases, thereby inhibiting the spread of flames. At the same time, graphene has good thermal conductivity and can quickly disperse local heat to other parts, further reducing the risk of fire. Organic flame retardants and graphene work synergistically to generate a denser, impermeable carbon layer on the surface of the substrate when heated and burned, preventing heat conduction. At the same time, no smoke is generated during the combustion process. The flame retardant ingredients used do not contain halogens and are green and environmentally friendly.

[0032] (3) The main chain of the EPDM rubber in the present invention is composed of chemically stable saturated hydrocarbons and has good aging resistance. The epoxidized EPDM rubber is prepared by in-situ polymerization, into which hydroxybenzophenone is introduced, which is an excellent ultraviolet absorber that can absorb high-energy ultraviolet light. The carbonyl group in the molecule and the hydrogen bond in the molecule form an internal hydrogen bond to form a chelate ring. After absorbing the ultraviolet light energy, the molecule undergoes thermal vibration, the internal hydrogen bond is destroyed, the chelate ring opens, and the corresponding energy conversion is performed, converting the energy of the ultraviolet light into harmless low-radiation heat energy to release the energy, thereby improving the ultraviolet aging resistance of the matrix. Through the chemical grafting method, the durability of the ultraviolet absorber is improved, and the aging resistance of the matrix is ​​further improved. The aging resistance time is longer, the service life is increased, the replacement frequency is reduced, and the use cost is reduced. Graphene has ultraviolet absorption and reflection capabilities, and works together with the organic ultraviolet absorber to obtain a composite rubber material with excellent aging resistance.

[0033] (4) After the graphene is modified in the present invention, the agglomeration of graphene is effectively avoided, and the graphene can be evenly dispersed in the matrix, further improving the mechanical properties, flame retardancy and aging resistance of the composite rubber material. Styrene-butadiene rubber has excellent heat resistance, and the interaction with modified graphene can improve the thermal stability of the material, slow down the breakage of molecular segments and the generation of polar functional groups during the aging process, and has excellent aging resistance. The material can maintain excellent mechanical properties. Furthermore, styrene-butadiene rubber has good processing properties, which can effectively improve the processing properties of the composite rubber material and improve production efficiency. The composite rubber material can be well applied to the fields of automotive parts, electronic appliances, etc., and has excellent comprehensive performance. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] Example 1, (1) 10 g of carboxylated graphene was added to 380 g of N,N-dimethylformamide, and ultrasonically dispersed uniformly, and then 15.5 g of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, 2.8 g of dicyclohexylcarbodiimide and 0.9 g of 4-dimethylaminopyridine were added, mixed uniformly, and reacted at 25° C. for 9 h. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain modified graphene;

[0036] (2) 20 g of ethylene propylene diene monomer rubber, 0.6 g of glycidyl methacrylate, 0.1 g of styrene, 0.8 g of 4-acryloxy-2-hydroxybenzophenone, and 0.6 g of initiator diisopropyl peroxide were mixed evenly, and transferred to a twin-screw extruder for melt reaction. During the melt reaction, the rotor speed was 100 r / min, the melt reaction temperature was 220°C, and the melt reaction time was 5 min. After the reaction was completed, the mixture was extruded and cooled to obtain epoxidized ethylene propylene diene monomer rubber;

[0037] (3) 100 g of EPDM rubber, 12 g of epoxidized EPDM rubber, and 5 g of modified graphene were mixed evenly, and transferred to a torque rheometer for melt blending. During the melt blending process, the rotor speed was 50 r / min, the melt blending temperature was 225°C, and the melt blending time was 5 min. After the reaction was completed, the mixture was cooled to obtain modified EPDM rubber;

[0038] (4) 100 g of modified EPDM rubber, 5 g of styrene-butadiene rubber, 0.3 g of antioxidant N,N'-di(β-naphthyl)-p-phenylenediamine and 1 g of lubricant pentaerythritol stearate were added to an internal mixer in sequence. After mixing at 105°C for 12 min, 2 g of vulcanizing agent di-tert-butyl peroxyisopropylbenzene, 1 g of zinc oxide and 0.5 g of stearic acid were added and mixed for 12 min to obtain a mixed product. The mixed product was re-mixed in an open mixer at a temperature of 110°C for 12 min. After the re-mixing was completed, it was blown dry and cooled, and placed for 24 h to obtain a mixed rubber. The mixed rubber was then transferred to a flat vulcanizer for vulcanization molding at a temperature of 160°C for 18 min. The material was discharged to obtain a flame retardant and aging-resistant composite rubber material.

[0039] Example 2, (1) 10 g of carboxylated graphene was added to 405 g of N,N-dimethylformamide, and ultrasonically dispersed uniformly, and then 18 g of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, 3.2 g of dicyclohexylcarbodiimide and 1.2 g of 4-dimethylaminopyridine were added, mixed uniformly, and reacted at 30° C. for 8 h. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain modified graphene;

[0040] (2) 20 g of ethylene propylene diene monomer rubber, 0.65 g of glycidyl methacrylate, 0.12 g of styrene, 0.9 g of 4-acryloxy-2-hydroxybenzophenone, and 0.8 g of initiator dicumyl peroxide were mixed evenly, and transferred to a twin-screw extruder for melt reaction. During the melt reaction, the rotor speed was 100 r / min, the melt reaction temperature was 230°C, and the melt reaction time was 5 min. After the reaction was completed, the mixture was extruded and cooled to obtain epoxidized ethylene propylene diene monomer rubber;

[0041] (3) 100 g of EPDM rubber, 14 g of epoxidized EPDM rubber, and 6 g of modified graphene were mixed evenly, and transferred to a torque rheometer for melt blending. During the melt blending process, the rotor speed was 50 r / min, the melt blending temperature was 230° C., and the melt blending time was 5 min. After the reaction was completed, the mixture was cooled to obtain modified EPDM rubber.

[0042] (4) 100 g of modified EPDM rubber, 7 g of styrene-butadiene rubber, 0.4 g of antioxidant N,N'-di(β-naphthyl)-p-phenylenediamine and 1.5 g of lubricant pentaerythritol stearate were added to an internal mixer in sequence, mixed at 110°C for 10 min, and then 2.4 g of vulcanizing agent di-tert-butyl peroxyisopropylbenzene, 1.5 g of zinc oxide and 1.2 g of stearic acid were added and mixed for 14 min to obtain a mixed product. The mixed product was re-mixed in an open mixer at a temperature of 120°C for 10 min. After the re-mixing was completed, it was blown dry and cooled, and allowed to stand for 24 h to obtain a mixed rubber. The mixed rubber was then transferred to a flat vulcanizer for vulcanization molding at a temperature of 170°C for 15 min. The material was discharged to obtain a flame retardant and aging-resistant composite rubber material.

[0043] Example 3, (1) 10 g of carboxylated graphene was added to 440 g of N,N-dimethylformamide, and ultrasonically dispersed uniformly, and then 20 g of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, 3.8 g of dicyclohexylcarbodiimide and 1.4 g of 4-dimethylaminopyridine were added, mixed uniformly, and reacted at 30° C. for 8 h. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain modified graphene;

[0044] (2) 20 g of ethylene propylene diene monomer rubber, 0.75 g of glycidyl methacrylate, 0.15 g of styrene, 1.1 g of 4-acryloxy-2-hydroxybenzophenone, and 0.9 g of initiator diisopropyl peroxide were mixed evenly, and transferred to a twin-screw extruder for melt reaction. During the melt reaction, the rotor speed was 100 r / min, the melt reaction temperature was 230°C, and the melt reaction time was 5 min. After the reaction was completed, the mixture was extruded and cooled to obtain epoxidized ethylene propylene diene monomer rubber;

[0045] (3) 100 g of EPDM rubber, 14 g of epoxidized EPDM rubber, and 6 g of modified graphene were mixed evenly, and transferred to a torque rheometer for melt blending. During the melt blending process, the rotor speed was 50 r / min, the melt blending temperature was 230° C., and the melt blending time was 5 min. After the reaction was completed, the mixture was cooled to obtain modified EPDM rubber.

[0046] (4) 100 g of modified EPDM rubber, 7 g of styrene-butadiene rubber, 0.4 g of antioxidant N,N'-di(β-naphthyl)-p-phenylenediamine and 1.5 g of lubricant pentaerythritol stearate were added to an internal mixer in sequence, mixed at 110°C for 10 min, and then 2.4 g of vulcanizing agent di-tert-butyl peroxyisopropylbenzene, 1.5 g of zinc oxide and 1.2 g of stearic acid were added and mixed for 14 min to obtain a mixed product. The mixed product was re-mixed in an open mixer at a temperature of 120°C for 10 min. After the re-mixing was completed, it was blown dry and cooled, and allowed to stand for 24 h to obtain a mixed rubber. The mixed rubber was then transferred to a flat vulcanizer for vulcanization molding at a temperature of 170°C for 15 min. The material was discharged to obtain a flame retardant and aging-resistant composite rubber material.

[0047] Example 4: The difference between this example and Example 3 is that 17 g of epoxidized ethylene propylene diene rubber and 7.5 g of modified graphene are added in step (3), and other conditions remain unchanged.

[0048] Example 5, (1) 10 g of carboxylated graphene was added to 450 g of N,N-dimethylformamide, and ultrasonically dispersed uniformly, and then 21 g of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, 4 g of dicyclohexylcarbodiimide and 1.5 g of 4-dimethylaminopyridine were added, mixed uniformly, and reacted at 35° C. for 6 h. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain modified graphene;

[0049] (2) 20 g of ethylene propylene diene monomer rubber, 0.8 g of glycidyl methacrylate, 0.16 g of styrene, 1.2 g of 4-acryloxy-2-hydroxybenzophenone, and 1 g of initiator diisopropyl peroxide were mixed evenly, and transferred to a twin-screw extruder for melt reaction. During the melt reaction, the rotor speed was 100 r / min, the melt reaction temperature was 240°C, and the melt reaction time was 5 min. After the reaction was completed, the mixture was extruded and cooled to obtain epoxidized ethylene propylene diene monomer rubber;

[0050] (3) 100 g of EPDM rubber, 18 g of epoxidized EPDM rubber, and 8 g of modified graphene were mixed evenly, and transferred to a torque rheometer for melt blending. During the melt blending process, the rotor speed was 50 r / min, the melt blending temperature was 235° C., and the melt blending time was 5 min. After the reaction was completed, the mixture was cooled to obtain modified EPDM rubber;

[0051] (4) 100 g of modified EPDM rubber, 8 g of styrene-butadiene rubber, 0.5 g of antioxidant N,N'-di(β-naphthyl)-p-phenylenediamine and 2 g of lubricant pentaerythritol stearate were added to an internal mixer in sequence. After mixing at 115°C for 8 min, 3 g of vulcanizing agent di-tert-butyl peroxyisopropylbenzene, 2 g of zinc oxide and 1.5 g of stearic acid were added and mixed for 15 min to obtain a mixed product. The mixed product was re-mixed in an open mixer at a temperature of 130°C for 9 min. After the re-mixing was completed, it was blown dry and cooled, and allowed to stand for 24 h to obtain a mixed rubber. The mixed rubber was then transferred to a flat vulcanizer for vulcanization molding at a temperature of 180°C for 12 min. The material was discharged to obtain a flame retardant and aging-resistant composite rubber material.

[0052] Comparative Example 1, (1) 20 g of ethylene propylene diene monomer rubber, 0.75 g of glycidyl methacrylate, 0.15 g of styrene, 1.1 g of 4-acryloxy-2-hydroxybenzophenone, and 0.9 g of initiator diisopropyl peroxide were mixed uniformly, and transferred to a twin-screw extruder for melt reaction. During the melt reaction, the rotor speed was 100 r / min, the melt reaction temperature was 230° C., and the melt reaction time was 5 min. After the reaction was completed, the mixture was extruded and cooled to obtain epoxidized ethylene propylene diene monomer rubber;

[0053] (2) 100 g of EPDM rubber, 17 g of epoxidized EPDM rubber, 2.5 g of carboxylated graphene, and 5 g of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine were mixed evenly, and transferred to a torque rheometer for melt blending. During the melt blending process, the rotor speed was 50 r / min, the melt blending temperature was 230° C., and the melt blending time was 5 min. After the reaction was completed, the mixture was cooled to obtain a modified EPDM rubber;

[0054] (3) 100 g of modified EPDM rubber, 7 g of styrene-butadiene rubber, 0.4 g of antioxidant N,N'-di(β-naphthyl)-p-phenylenediamine and 1.5 g of lubricant pentaerythritol stearate were added to an internal mixer in sequence, mixed at 110°C for 10 min, and then 2.4 g of vulcanizing agent di-tert-butyl peroxyisopropylbenzene, 1.5 g of zinc oxide and 1.2 g of stearic acid were added and mixed for 14 min to obtain a mixed product. The mixed product was re-mixed in an open mixer at a temperature of 120°C for 10 min. After the re-mixing was completed, it was blown dry and cooled, and placed for 24 h to obtain a mixed rubber. The mixed rubber was then transferred to a flat vulcanizer for vulcanization molding at a temperature of 170°C for 15 min. The material was discharged to obtain a flame retardant and aging-resistant composite rubber material.

[0055] Comparative Example 2, (1) 10 g of carboxylated graphene was added to 440 g of N,N-dimethylformamide, and ultrasonically dispersed uniformly, and then 20 g of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, 3.8 g of dicyclohexylcarbodiimide and 1.4 g of 4-dimethylaminopyridine were added, mixed uniformly, and reacted at 30° C. for 8 h. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain modified graphene;

[0056] (2) 116 g of ethylene propylene diene monomer rubber, 1 g of 4-acryloxy-2-hydroxybenzophenone, and 7.5 g of modified graphene were mixed evenly, and transferred to a torque rheometer for melt blending. During the melt blending process, the rotor speed was 50 r / min, the melt blending temperature was 230° C., and the melt blending time was 5 min. After the reaction was completed, the mixture was cooled to obtain modified ethylene propylene diene monomer rubber;

[0057] (3) 100 g of modified EPDM rubber, 7 g of styrene-butadiene rubber, 0.4 g of antioxidant N,N'-di(β-naphthyl)-p-phenylenediamine and 1.5 g of lubricant pentaerythritol stearate were added to an internal mixer in sequence, mixed at 110°C for 10 min, and then 2.4 g of vulcanizing agent di-tert-butyl peroxyisopropylbenzene, 1.5 g of zinc oxide and 1.2 g of stearic acid were added and mixed for 14 min to obtain a mixed product. The mixed product was re-mixed in an open mixer at a temperature of 120°C for 10 min. After the re-mixing was completed, it was blown dry and cooled, and placed for 24 h to obtain a mixed rubber. The mixed rubber was then transferred to a flat vulcanizer for vulcanization molding at a temperature of 170°C for 15 min. The material was discharged to obtain a flame retardant and aging-resistant composite rubber material.

[0058] The carboxylated graphene in the embodiments and comparative examples of the present invention is prepared by the following method: 40 mL of graphene oxide dispersion and 60 mL of deionized water are mixed evenly, and then 5.0 g of sodium hydroxide and 7.5 g of sodium chloroacetate are added, mixed for 8 h, centrifuged at a rate of 8000 r / min, centrifuged for 5 min, washed, neutralized, dialyzed, and dried at 60 ° C for 12 h to obtain carboxylated graphene.

[0059] The EPDM rubber in the embodiments and comparative examples of the present invention was purchased from PetroChina Jilin Chemical Engineering Co., Ltd., model 2070; the styrene-butadiene rubber was purchased from PetroChina Co., Ltd., model 1502; the CAS number of N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine was 66499-31-8, and the molecular formula was C 16 H 15 N6O2P; the CAS number of 4-acryloyloxy-2-hydroxybenzophenone is 15419-94-0; other undisclosed reagents are commercially available.

[0060] Corresponding tests were performed on the composite rubber materials prepared in Examples 1-5 and Comparative Examples 1-2. The test methods and test results are as follows:

[0061] (1) Flame retardant performance test: The composite rubber materials prepared in Examples 1-5 and Comparative Examples 1-2 were cut into square strips and subjected to a flame retardant performance test on a PX-01-005 oxygen index analyzer. The samples were placed vertically, ignited, and their oxygen concentrations were measured. Each group was tested three times and the average value was taken. The test results are shown in Table 1:

[0062] Table 1

[0063]

[0064] According to the test results in Table 1, it can be seen that the limiting oxygen index of the samples corresponding to Examples 1-5 all reach the flame retardant level. The organic flame retardant and graphene work synergistically. When heated and burned, a denser and impermeable carbon layer will be generated on the surface of the substrate, giving the composite rubber material good flame retardant properties. Among them, the limiting oxygen index of the composite rubber material corresponding to Example 4 can reach 35.3%. In Comparative Example 1, carboxylated graphene oxide and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine are directly added to the substrate, the dispersibility becomes worse, the compatibility is reduced, and the synergistic flame retardant performance is reduced. In Comparative Example 2, there is no reaction with epoxidized ethylene propylene rubber, which has a certain effect on the flame retardant properties.

[0065] (2) Aging resistance test: The composite rubber materials prepared in Examples 1-5 and Comparative Examples 1-2 were used as samples, and the tensile properties of the samples were tested using an Instron 5567 universal testing machine in accordance with the test standard GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", wherein the temperature was 25°C, the load was 1000N, the tensile rate was 500mm / min, and the sample was dumbbell-shaped; the samples were placed in a UV aging test chamber for 72 hours of aging treatment, and the UV aging was performed using a xenon lamp with a power of 35W. After the treatment, the samples were taken out and subjected to the same tensile test; the samples were placed in a heat aging test chamber in accordance with the national standard GB / T 3512-2001, with an aging temperature of 120°C and a thermal oxygen aging time of 72 hours, and subjected to the same tensile test; the above test results are shown in Table 2:

[0066] Table 2

[0067]

[0068] According to the test results in Table 2, it can be seen that the samples corresponding to Examples 1-5 have excellent resistance to ultraviolet aging and thermal oxygen aging. The introduction of graphene and organic ultraviolet absorbers improves the resistance to ultraviolet aging of the composite rubber material. The synergistic effect of graphene and styrene-butadiene rubber improves its resistance to thermal oxygen aging. After ultraviolet aging and thermal oxygen aging treatment, the tensile strength and elongation at break of Examples 1-5 decrease slowly.

[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an aging-resistant composite rubber material with flame retardant effect, Features: The steps include: Step 1, adding carboxylated graphene to an organic solvent, uniformly dispersing by ultrasonication, then adding N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, dicyclohexylcarbodiimide and 4-dimethylaminopyridine, mixing evenly, reacting, after the reaction is completed, filtering, washing, and vacuum drying at 60° C. for 12 h to obtain modified graphene; Step 2: Evenly mix ethylene propylene diene monomer rubber, glycidyl methacrylate, styrene, 4-acryloxy-2-hydroxybenzophenone and an initiator, transfer the mixture to a twin-screw extruder for a melt reaction, extrude the mixture after the reaction is completed, and cool the mixture to obtain epoxidized ethylene propylene diene monomer rubber; Step 3, uniformly mixing the EPDM rubber, the epoxidized EPDM rubber and the modified graphene, transferring the mixture to a torque rheometer for melt blending, and cooling the mixture after the reaction to obtain the modified EPDM rubber; Step 4: Add modified EPDM rubber, styrene-butadiene rubber, antioxidant and lubricant into an internal mixer, mix at 105-115° C. for 8-12 minutes, add vulcanizing agent, zinc oxide and stearic acid, mix for 12-15 minutes to obtain a mixed product, and refining the mixed product in an open mill. After the refining is completed, blow dry and cool, place for 24 hours to obtain a mixed rubber, and then transfer it to a flat vulcanizer for vulcanization molding, discharge the material, and obtain an aging-resistant composite rubber material with flame retardant effect; In the step 1, the mass ratio of carboxylated graphene, organic solvent, N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine is 100:3800-4500:155-210:28-40:9-15, the reaction temperature is 25-35° C., and the reaction time is 6-9 h; In the step 2, the mass ratio of EPDM rubber, glycidyl methacrylate, styrene, 4-acryloxy-2-hydroxybenzophenone, and initiator is 100:3-4:0.5-0.8:4-6:3-5, and the initiator is dicumyl peroxide; In the step 3, the mass ratio of EPDM rubber, epoxidized EPDM rubber and modified graphene is 100:12-18:5-8. During the melt blending process, the rotor speed is 50 r / min, the melt blending temperature is 225-235° C., and the melt blending time is 5 min. In the step 4, the mass ratio of the modified EPDM rubber, styrene-butadiene rubber, antioxidant, lubricant, vulcanizing agent, zinc oxide and stearic acid is 100:5-8:0.3-0.5:1-2:2-3:1-2:0.5-1.

5.

2. The method for preparing a flame retardant and aging resistant composite rubber material according to claim 1, Features: The organic solvent in step 1 includes any one or more of N,N-dimethylformamide, toluene, and tetrahydrofuran.

3. The method for preparing the flame retardant and aging resistant composite rubber material according to claim 1, Features: During the melting reaction in step 2, the rotor speed is 100 r / min, the melting reaction temperature is 220-240° C., and the melting reaction time is 5 min.

4. The method for preparing a flame retardant and aging resistant composite rubber material according to claim 1, Features: In the step 4, the temperature of refining in the open mill is 110-130° C., the refining time is 9-12 min, the temperature of vulcanization molding in the flat vulcanizing agent is 160-180° C., and the vulcanization molding time is 12-18 min.

5. An aging-resistant composite rubber material with flame retardant effect prepared by the method for preparing an aging-resistant composite rubber material with flame retardant effect as claimed in any one of claims 1 to 4.

6. Use of the flame retardant and aging resistant composite rubber material according to claim 5 in automobile parts and electronic appliances.

Citation Information

Patent Citations

  • Flame-retardant thermal-aging-resistant EPDM composite material

    CN105585780A

  • Conductive EPDM (ethylene propylene diene monomer) with high flame retardant property and preparation method thereof

    CN107868348A

  • Efficient halogen-free flame retardant rubber system as well as preparation method thereof

    CN104558716A

  • Graphene containing DOPO group and preparation method thereof

    CN105001451A

  • Graphene oxide-based phosphorus-nitrogen flame retardant and flame-retardant ABS (Acrylonitrile Butadiene Styrene) plastic