Preparation method of dermis filling agent of composite polymer microspheres and dermis filling agent based on dermis filling agent
Through a cross-linking reaction, degradable polymer microspheres are mixed with a solution containing protein to form a dense semi-interpenetrating network structure of the dermal filler, which solves the problems in the preparation process of composite microsphere collagen fillers in the existing technology. Uniform problem, achieving longer-lasting filling effect and better cosmetic effect.
Patent Information
- Application Number
- CN202410812241.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-19
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
The step-by-step cross-linking of existing composite microsphere collagen fillers during the preparation process results in inhomogeneity, resulting in varying degrees of microsphere stimulation after implantation into the skin. The filling and wrinkle removal effect is locally significant and affects the cosmetic effect.
Using a primary cross-linking reaction, degradable polymer microspheres are mixed with a solution containing protein, and polyethylene glycol and its derivatives with a molecular weight of 200 to 4000 Da are used as cross-linking agents to form a dense semi-interpenetrating network structure of the dermis. Fillers.
It achieves a denser and more uniform filling system, with better support and longer-lasting three-dimensional maintenance effect, avoiding the problem of uneven local irritation reactions, significantly promoting fibroblast proliferation, promoting collagen fiber production, and forming a longer-lasting filling effect. .
Smart Images

Figure CN118718097A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and particularly relates to a preparation method of a dermal filler of composite polymer microspheres and a dermal filler based thereon. Background Art
[0002] Human skin aging is affected by many factors such as genes, age, and environment, but generally speaking, the characteristics of aging include loss of subcutaneous tissue, decreased skin elasticity and moisture, and increased skin folds and wrinkles. These changes are related to thinning of the epidermis, atrophy of the dermis, loss of elastic tissue in the dermis, and loss of dermal collagen. In order to improve these problems, the development of drugs and implantable biomaterials has received a good response. Among them, injectable fillers have become more and more popular due to their advantages such as simple operation, less damage, and quick effect.
[0003] The physical fillers currently on the market (filling materials are mainly collagen and hyaluronic acid) have the following problems: First, they will be quickly catalyzed and degraded by enzymes in the body, and the filling effect is difficult to maintain; second, the injection site is shallow, and most of them can only improve dull skin and fine lines, but cannot permanently solve problems such as deep skin wrinkles and skin depressions, and new fillers need to be continuously added to maintain the effect; third, the clinical repair effect is too single and cannot meet the diverse needs of beauty seekers.
[0004] In order to be able to be used for filling the middle or deep layers of the dermis, physical filling materials are usually selected to be mixed with degradable polymer microspheres that can accelerate the induction of collagen regeneration. The current method for preparing collagen fillers with composite degradable polymer microspheres is usually: first prepare degradable polymer microspheres and collagen solution and cross-link them separately, and then mix the collagen cross-linked product with the degradable polymer microsphere cross-linked product. Since the particle size of the collagen gel itself is different, it will not form a uniform phase during the mixing process. Therefore, this preparation method will cause the collagen filler to have unevenness problems, resulting in different degrees of microsphere stimulation after implantation in the skin. The results vary greatly, which then causes the filling and wrinkle removal effect to be locally significant, making the local medical beauty marks too heavy, affecting the beauty effect. Summary of the invention
[0005] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a dermal filler of composite polymer microspheres and a dermal filler based thereon, so as to solve the problem of heterogeneity caused by step-by-step cross-linking in the preparation process of existing composite microsphere collagen fillers.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention discloses a method for preparing a dermal filler of composite polymer microspheres, wherein degradable polymer microspheres are mixed with a solution containing protein and then cross-linked once to obtain a dermal filler;
[0008] The components of the protein-containing solution include recombinant functional proteins and glycerol, and the recombinant functional proteins include recombinant collagen and recombinant elastin; the cross-linking agent used for cross-linking is one of polyethylene glycol and its derivatives with a molecular weight of 200 to 4000 Da.
[0009] Preferably, the degradable polymer microspheres are any one of polycaprolactone block copolymers, polyethylene glycol block copolymers, poly-L-lactic acid block copolymers, poly-D-lactic acid block copolymers, polylactic acid-glycolic acid block copolymers and polyracemic lactic acid block copolymers, or are obtained by melting, granulating and screening two or three of polycaprolactone, polyethylene glycol, poly-L-lactic acid, poly-D-lactic acid and polylactic acid-glycolic acid.
[0010] Preferably, the recombinant collagen is one or both of type I recombinant collagen and type III recombinant collagen.
[0011] Preferably, the molecular weight of the recombinant collagen is 40-100 kDa.
[0012] Preferably, the molecular weight of the recombinant elastin is 10-30 kDa.
[0013] Preferably, the recombinant functional protein can also be added with one or more of recombinant mussel mucin, recombinant fibronectin and recombinant silk protein; the components of the protein-containing solution can also be added with polysaccharides, which are one or more of hyaluronic acid, hyaluronate and sodium alginate.
[0014] More preferably, the mass ratio of the recombinant functional protein, glycerol and polysaccharide is 1:(0.1-10):(0-10).
[0015] Preferably, the total concentration of the recombinant functional protein is 10-60 mg / mL.
[0016] Preferably, the mass ratio of the degradable polymer microspheres to the solution containing the protein is (0.2-20):1.
[0017] Preferably, the degradable polymer microspheres are mixed with a solution containing protein to obtain a composite microsphere collagen solution, and the composite microsphere collagen solution is mixed with a cross-linking agent at a mass ratio of 1:(0.1-1) to obtain a dermal filler.
[0018] Preferably, the degradable polymer microspheres are mixed with a solution containing protein and then cross-linked once, and then an anesthetic and a protein protective agent are added and mixed to obtain a dermal filler.
[0019] More preferably, the mass ratio of the protein protective agent to the recombinant functional protein is (0.5-3):1.
[0020] The second aspect of the present invention discloses a dermal filler prepared by the above preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a method for preparing a dermal filler of composite polymer microspheres, which obtains a more dense and uniform filling system through a single crosslinking reaction. Compared with the method of crosslinking collagen and blended microspheres separately and then mixing the crosslinked products of the two in the traditional method, the method first mixes the protein-containing solution with the degradable polymer microspheres before crosslinking. During this reaction process, the hydroxyl groups on some microspheres combine with the amino acid residues on some proteins to form amide bonds. After that, polyethylene glycol or its derivatives are added for one-step crosslinking. During this reaction process, a ring cleavage reaction occurs in the polyethylene glycol or its derivatives in the solution. A part of the hydroxyl groups generated after the epoxy ring is opened combines with the amino groups on the protein to form amide bonds, and a part of them combines with the hydroxyl groups on the microspheres to form ester bonds. Finally, a crosslinked product with a dense semi-interpenetrating network structure, i.e., a dermal filler, is obtained. The dermal filler has better support and a more durable three-dimensional retention effect. At the same time, it also avoids the problem of different local irritation reactions caused by uneven blending of protein fillers containing microspheres in the prior art.
[0023] The protein-containing solution in this solution has recombinant collagen, recombinant elastin and glycerol as main components. Recombinant elastin is the main component of elastic fibers in tissues, which mainly gives elasticity and tensile resistance to tissues or organs, and can maintain the skin's tone, structure and elasticity. Recombinant collagen and recombinant elastin can replenish the missing collagen in the implantation site in time after filling, improve the elasticity of loose skin, and achieve the effect of filling wrinkles and depressions and providing skin elasticity. In this solution, glycerol is added at the initial stage of protein dissolution, which can absorb moisture in the surrounding environment and form a moisturizing layer on the protein surface to prevent the protein from denaturing due to loss of moisture. At the same time, glycerol can also form hydrogen bonds and van der Waals forces with the protein surface, increasing the stability of the protein.
[0024] This solution uses a combination of different proteins to avoid the problem of single effect of single protein fillers in the prior art. This solution uses a composite protein form that can significantly promote the proliferation of fibroblasts, and proteins with different molecular weights promote the proliferation of fibroblasts (fibroblasts are the main production cells of recombinant elastin and recombinant collagen) in the body for different periods of time, which can play a role in continuously and stably proliferating fibroblasts and promoting the production of elastic fibers and collagen fibers. As the protein degrades, the degradable polymer microspheres continuously stimulate the production of collagen fibers, forming a longer-term filling effect, technically achieving the effects of short-term support and long-term stimulation of regeneration.
[0025] This scheme selects one of polyethylene glycol and its derivatives as a crosslinking agent. PEG and its derivatives are linear or branched polyethers composed of repeated oxyethylene groups, which are easily hydrolyzed and undergo ring cleavage reactions in aqueous solutions to generate hydroxyl groups. The generated hydroxyl groups can be connected with the amino groups at the N-terminal of the amino acid side chain and the hydroxyl groups on the microspheres to obtain a more compact crosslinked product. In addition, the preparation method of this scheme is simple. After mixing the protein-containing solution with the degradable polymer microspheres, they are directly crosslinked in one step without the need for complex processes such as freeze-drying.
[0026] Furthermore, degradable polymer microspheres are prepared with block copolymers. Different block copolymer microspheres have different degradation times in the human body. The degradable block copolymer microspheres can act as scaffolds to stimulate the formation of collagen fibers during the collagen degradation process. Moreover, the degradation products of block copolymers, such as amino acids and polysaccharides, can continuously provide substrates for collagen regeneration, further promoting collagen regeneration and forming a longer-lasting filling effect.
[0027] Furthermore, one or more of recombinant mussel mucin, recombinant fibronectin, recombinant silk protein, hyaluronic acid, hyaluronate and sodium alginate are added to the protein-containing solution, among which recombinant mussel mucin has multiple capabilities of whitening, anti-oxidation, promoting cell repair and promoting wound repair; recombinant fibronectin plays an important role in cell adhesion, growth, migration and differentiation, and promoting wound healing; and the addition of recombinant silk protein will significantly change the mechanical properties of the product; hyaluronic acid or hyaluronate is one of the main components of the human extracellular matrix and intercellular matrix, and is a filler between cells. The hydroxyl, amino and other functional groups in its molecular structure react with the amino acid residues on the protein to form a covalent bond, which can provide a spatial framework for the distribution of collagen fibers and elastin. The three together form a skin scaffold to maintain the stability of skin tissue, maintain skin elasticity, and slow down skin aging and the formation of wrinkles.
[0028] Furthermore, during the preparation process, the protein-containing solution and the cross-linking agent are mixed at a mass ratio of 1:(0.1-1), which can ensure that the prepared dermal filler does not become sandy, and the pushing force is maintained in the range of 10-25N. It can be directly injected into the deep layer of the dermis, achieving rapid replenishment of collagen while also continuously stimulating collagen regeneration.
[0029] Furthermore, the continued addition of anesthetics and protein protectants after cross-linking can protect the activity of the protein, further maintain the stability of the protein in a solution state, and reduce the pain caused during the injection process.
[0030] The present invention provides a dermal filler, wherein the preparation method of the microspheres is simple in composition compared with the traditional emulsification-solvent method, and no new chemical substances are introduced except the target copolymer, and the prepared microspheres are of high purity and good biosafety. The protein-containing solution is mixed with the degradable polymer microspheres and then directly cross-linked, and the dermal filler is obtained by one-time cross-linking. Compared with the collagen filler of the traditional composite microspheres, the dermal filler has a denser and more uniform structure and a more lasting effect. Therefore, the dermal filler has a good application prospect and can be applied to the fields of implanted medical devices, skin beauty care, etc., especially for filling and correcting wrinkles such as facial wrinkles, hand wrinkles, eye wrinkles, neck wrinkles, stretch marks, butterfly sleeves, buttocks and thigh muscle relaxation. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The figure is a graph showing the pushing force test results of each group of dermal fillers of the present invention;
[0032] Figure 2 Graph showing the rotational rheological test results of each group of dermal fillers of the present invention; wherein G' is the viscous modulus, and G" is the elastic modulus;
[0033] Figure 3 The microscopic photographs of the dermal fillers of each group of the present invention are shown;
[0034] Figure 4 The morphological diagrams of the mouse fibroblasts in each group of the present invention are shown;
[0035] Figure 5 These are the HE staining results of each group of the present invention. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0037] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0038] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0039] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0040] Herein, unless otherwise specified, “recombinant collagen” refers to collagen with a highly humanized sequence, and “recombinant elastin” refers to elastin with a highly humanized sequence.
[0041] Herein, the protein in the "protein-containing solution" includes, but is not limited to, recombinant collagen, recombinant elastin, recombinant mussel mucin, recombinant fibronectin and recombinant silk fibroin.
[0042] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0043] The present invention provides a method for preparing a dermal filler of composite polymer microspheres and a dermal filler based thereon, comprising the following steps:
[0044] (1) Obtaining biodegradable polymer microspheres with a molecular weight of 200 to 2,000,000 kDa;
[0045] The biodegradable polymer microspheres are any one of polycaprolactone (PCL), polyethylene glycol (PEG), poly-L-lactic acid (PLLA), poly-D-lactic acid (PDLA), poly-lactic acid-glycolic acid copolymer (PLGA) and poly-racemic lactic acid (PDLLA); or any two or three of polycaprolactone (PCL), polyethylene glycol (PEG), poly-L-lactic acid (PLLA), poly-D-lactic acid (PDLA), poly-lactic acid-glycolic acid copolymer (PLGA) and poly-racemic lactic acid (PDLLA), which are melted at 180-260° C., granulated and screened to obtain microsphere particles with a particle size range of 10-100 μm, specifically PCL-PEG-PLLA, PCL-PEG-PDLA, PCL-PEG-PLGA, PCL-PEG-PDLLA, PCL-PLLA-PDLA, PCL-PLLA-PLGA, PCL-PLLA-PDLLA, PCL-PDLA-PLGA, PCL-PDLA-PDLLA A. PCL-PLGA-PDLLA, PEG-PLLA-PDLA, PEG-PLLA-PLGA, PEG-PLLA-PDLLA, PEG-PDLA-PLGA, PEG-PDLA-PDLLA, PEG-PLGA-PDLLA, PLLA-PDLA-PLGA, PLLA-PDLA-PDLLA, PLLA-PLGA-PDLLA, PDLA-PLGA-PD LLA, PCL-PEG, PCL-PLLA, PCL-PDLA, PCL-PLGA, PCL-PDLLA, PEG-PLLA, PEG-PDLA, PEG-PLGA, PEG-PDLLA, PLLA-PDLA, PLLA-PLGA, PLLA–PDLLA, PDLA-PLGA, PDLA-PDLLA, PLGA-PDLLA, PCL-PEG-PC L. PCL-PLLA-PCL, PCL-PDLA-PCL, PCL-PLGA-PCL, PCL-PDLLA-PCL, PEG-PLLA-PEG, PEG-PDLA-PEG, PEG-PLGA-PEG, PEG-PDLLA-PEG, PL Any of LA-PDLA-PLLA, PLLA-PLGA-PLLA, PLLA–PDLLA-PLLA, PDLA-PLGA-PDLA, PDLA-PDLLA-PDLA and PLGA-PDLLA-PLGA.
[0046] (2) dissolving the recombinant functional protein, glycerol and polysaccharide in water at a mass ratio of 1:(0.1-10):(0-10), adjusting the pH value of the solution to 7-8 with NaOH, and preparing a solution containing the protein;
[0047] Among them, the total concentration of the recombinant functional protein is 10-60 mg / mL; the recombinant functional protein includes but is not limited to recombinant collagen and recombinant elastin in a mass ratio of 1: (0.2-20), the recombinant collagen is one or both of recombinant type I collagen and recombinant type III collagen, and the molecular weight is 40-100 kDa; the molecular weight of the recombinant elastin is 10-30 kDa; one or more of recombinant mussel mucin, recombinant fibronectin and recombinant silk protein can also be added; polysaccharides can also be added, and the polysaccharides are one or more of hyaluronic acid, hyaluronate and sodium alginate.
[0048] (3) The degradable polymer microspheres of step (1) and the protein-containing solution obtained in step (2) are mixed at a mass ratio of (0.2-20):1 to obtain a composite microsphere collagen solution; the composite microsphere collagen solution is mixed with a cross-linking agent at a mass ratio of 1:(0.1-1), cross-linked at 20-50° C. for 2-24 hours, and the cross-linked gel is swollen, washed, and homogenized to prepare a dermal filler with a particle size of 200-1000 μm.
[0049] The cross-linking agent is one of polyethylene glycol and its derivatives, specifically one of PEG, PEGDE, PEG-dichlorotriazine derivatives, PEG-tetrazine derivatives, PEG-succinimidyl carbonate, PEG-propionaldehyde and PEG-butyraldehyde.
[0050] In addition, as an optimization scheme, an anesthetic and a protein protective agent may be further added to the homogenized product in the above step (3), mixed, homogenized, filled, and sterilized to obtain a dermal filler;
[0051] Wherein, the anesthetic includes but is not limited to lidocaine hydrochloride, and the protein protective agent includes but is not limited to one or more of mannitol, urea, disodium ethylenediaminetetraacetic acid, glycine, arginine, histidine and lysine; the mass ratio of the protein protective agent to the protein in the solution containing the protein is (0.5-3):1.
[0052] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0053] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" represents mass percentage and ratio represents mass ratio.
[0054] 1. Preparation of dermal fillers
[0055] Embodiment 1:
[0056] (1) Preparation of degradable polymer microspheres:
[0057] PLLA, PEG and PDLA were melt-blended at 190°C in a mass fraction of 50:10:40, and the blended sample was dried in a vacuum oven at 80°C for 12 hours. Then, granulated using an extruder to obtain PLLA-PEG-PDLA degradable polymer microspheres, and the size of the degradable polymer microspheres was sieved to collect microsphere particles of 20 to 40 μm for later use.
[0058] (2) Preparation of dermal fillers:
[0059] Recombinant type III collagen, recombinant elastin collagen and glycerol were weighed in a mass ratio of 1:1:2 and placed in a beaker. After dissolving with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 30 mg / mL.
[0060] Weigh twice the mass of the degradable polymer microspheres as that of the solution containing the protein, and add them into the solution containing the protein under stirring to obtain a composite microsphere collagen solution.
[0061] Then, 0.3 times the mass of the composite microsphere collagen solution and a cross-linking agent PEGDE with a molecular weight of 800 were added during continuous stirring. After cross-linking at 30° C. for 20 hours, the mixture was broken into gel blocks, swelled in PBS buffer, and then washed with PBS buffer at room temperature. The washed gel was homogenized and dispersed, and then 0.3% lidocaine and 1.5% mannitol were added. After stirring and mixing evenly, the mixture was homogenized, filled, and sterilized by wet heat to obtain a dermal filler.
[0062] Embodiment 2:
[0063] (1) Preparation of degradable polymer microspheres:
[0064] PCL, PEG and PDLA were melt-blended at 190°C in a mass fraction of 50:10:40, and the blended sample was dried in a vacuum oven at 80°C for 12 h. Then, it was granulated by an extruder to obtain PCL-PEG-PDLA degradable polymer microspheres. The size of the degradable polymer microspheres was sieved, and microsphere particles of 20 to 40 μm were collected for later use.
[0065] (2) Preparation of dermal fillers:
[0066] Recombinant type III collagen, recombinant elastin collagen, hyaluronic acid, recombinant mussel mucin and glycerol were weighed in a mass ratio of 1:1:20:1:2 and placed in a beaker. After dissolving with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 60 mg / mL.
[0067] Weigh 20 times the mass of the degradable polymer microspheres of the solution containing the protein, and add them into the solution containing the protein under stirring to obtain a composite microsphere collagen solution.
[0068] Then, 1.0 times the mass of the composite microsphere collagen solution and a cross-linking agent PEGDE with a molecular weight of 4000 were added during continuous stirring. After cross-linking at 50° C. for 2 hours, the mixture was broken into gel blocks, swelled in PBS buffer, and then washed with PBS buffer. The washed gel was homogenized and dispersed, and then 0.3% lidocaine and 1.5% mannitol were added. After stirring and mixing evenly, the mixture was homogenized, filled, and sterilized by wet heat to obtain a dermal filler.
[0069] Embodiment 3:
[0070] (1) Preparation of degradable polymer microspheres:
[0071] The polyethylene glycol block copolymer was dried in a vacuum oven at 80° C. for 12 hours, and then granulated by an extruder to obtain degradable polymer microspheres. The size of the degradable polymer microspheres was sieved, and microsphere particles of 20 to 40 μm were collected for later use.
[0072] (2) Preparation of dermal fillers:
[0073] Recombinant type III collagen, recombinant elastin collagen and glycerol were weighed in a mass ratio of 1:1:2 and placed in a beaker. After dissolving with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 10 mg / mL.
[0074] Weigh 0.2 times the mass of the degradable polymer microspheres of the solution containing the protein, and add them into the solution containing the protein under stirring to obtain a composite microsphere collagen solution.
[0075] Then, 0.1 times the mass of the composite microsphere collagen solution and a cross-linking agent PEGDE with a molecular weight of 200 were added during continuous stirring. After cross-linking at 20° C. for 24 hours, the solution was broken into gel blocks, swelled in PBS buffer, and then washed with PBS buffer. The washed gel was homogenized and dispersed, and then 0.3% lidocaine and 1.5% mannitol were added. After stirring and mixing evenly, the mixture was homogenized, filled, and sterilized by wet heat to obtain a dermal filler.
[0076] Embodiment 4:
[0077] (1) Preparation of degradable polymer microspheres:
[0078] PLLA-PEG was melt-blended in sequence at a mass fraction of 70:30 at 200°C, the blended sample was dried in a vacuum oven at 85°C for 12 hours, and then granulated with an extruder to obtain degradable polymer microspheres. The size of the degradable polymer microspheres was sieved, and microsphere particles of 20 to 40 μm were collected for later use.
[0079] (2) Preparation of dermal fillers:
[0080] Recombinant type III collagen, recombinant type I collagen, recombinant elastin collagen, recombinant fibronectin and glycerol were weighed in a mass ratio of 0.8:0.2:1:0.5:2 and placed in a beaker. After dissolving with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 40 mg / mL.
[0081] Weigh 1 times the mass of the protein-containing solution with degradable polymer microspheres, and add them into the protein-containing solution under stirring to obtain a composite microsphere collagen solution.
[0082] Then, 0.2 times the mass of the composite microsphere collagen solution and a cross-linking agent PEGDE with a molecular weight of 400 were added during continuous stirring. After cross-linking at 40° C. for 6 hours, the mixture was broken into gel blocks, swelled in PBS buffer, and then washed with PBS buffer. The washed gel was homogenized and dispersed, and then 0.3% lidocaine and 1.5% mannitol were added. After stirring and mixing evenly, the mixture was homogenized, filled, and sterilized by wet heat to obtain a dermal filler.
[0083] Embodiment 5:
[0084] The difference from Example 1 is that the composition of the solution containing protein and the ratio of the added protein are different, and the other steps are consistent with Example 1.
[0085] Recombinant type III collagen, recombinant type I collagen, recombinant elastin collagen, recombinant fibronectin, recombinant mussel mucin, recombinant silk fibroin, sodium alginate and glycerol were weighed in a beaker according to the mass ratio of 0.8:0.2:1:0.5:0.5:0.5:10:2.
[0086] Embodiment 6:
[0087] The difference from Example 1 is that the composition of the solution containing protein and the ratio of the added protein are different, and the other steps are consistent with Example 1.
[0088] Recombinant type III collagen, recombinant type I collagen, recombinant elastin collagen, recombinant fibronectin, recombinant mussel mucin, recombinant silk fibroin, sodium hyaluronate and glycerol were weighed in a beaker according to the mass ratio of 0.8:0.2:1:0.5:0.5:0.5:10:2.
[0089] Comparative Example 1:
[0090] The difference from Example 1 is that no degradable polymer microspheres were added in this experiment.
[0091] Preparation of control dermal filler 1: Weigh type III recombinant collagen, recombinant elastin collagen and glycerol in a mass ratio of 1:1:2 and place them in a beaker. Dissolve them in 100 mL of purified water and adjust the pH value of the solution to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 30 mg / mL. Add 0.3 times the mass of the protein-containing solution to the crosslinking agent PEGDE while continuously stirring the protein-containing solution. Crosslink at 30°C for 20 hours and break into gel blocks. Swell in PBS buffer and then wash with PBS buffer. Homogenize and disperse the washed gel. Add 0.3% lidocaine and 1.5% mannitol. Stir and mix evenly and then homogenize, fill and sterilize with wet heat to obtain control dermal filler 1.
[0092] Comparative Example 2:
[0093] The difference from Example 1 is that no cross-linking was performed in this experiment.
[0094] (1) Preparation of degradable polymer microspheres:
[0095] The preparation method is the same as Example 1.
[0096] (2) Preparation of control dermal filler 2:
[0097] Type III recombinant collagen, recombinant elastin collagen and glycerol were weighed in a mass ratio of 1:1:2 and placed in a beaker. After dissolving with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 30 mg / mL.
[0098] Weigh twice the mass of the degradable polymer microspheres as that of the solution containing the protein, and add them into the solution containing the protein under stirring to obtain a composite microsphere collagen solution.
[0099] 0.3% lidocaine and 1.5% mannitol were added to the composite microsphere collagen solution, and the mixture was stirred and evenly mixed, and then homogenized, filled, and sterilized by wet heat to obtain a control dermal filler 2.
[0100] Comparative Example 3:
[0101] The difference from Example 1 is that this experiment was prepared by a traditional method of secondary cross-linking followed by mixing.
[0102] (1) Preparation of degradable polymer microspheres:
[0103] PLLA-PEG-PDLA microspheres were prepared by emulsification-solvent evaporation method. The particle size of microspheres was controlled within 20 μm by adjusting parameters such as oil phase concentration, aqueous phase emulsifier concentration, oil-water phase ratio, stirring rate, etc. to obtain degradable polymer microspheres.
[0104] (2) Preparation of control dermal filler 3:
[0105] Type III recombinant collagen, recombinant elastin collagen and glycerol were weighed in a mass ratio of 1:1:2 and placed in a beaker. After being dissolved with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 30 mg / mL. Under continuous stirring, 0.3 times the mass of the protein-containing solution was added with a cross-linking agent PEGDE. After cross-linking at 30°C for 20 hours, the solution was broken into gel blocks, swelled in PBS buffer, and then washed with PBS buffer. The washed gel was homogenously dispersed to obtain a composite gel.
[0106] (3) Mixing:
[0107] Degradable polymer microspheres twice the mass of the composite gel, lidocaine at a mass concentration of 0.3% and mannitol at a mass concentration of 1.5% were added to the prepared composite gel, and then homogenized, filled and sterilized by wet heat to obtain a control dermal filler 3.
[0108] Comparative Example 4:
[0109] The difference from Example 1 is that the mass of the cross-linking agent added in this experiment is twice the mass of the composite microsphere collagen solution.
[0110] (1) Preparation of degradable polymer microspheres:
[0111] The preparation method is the same as Example 1.
[0112] (2) Preparation of control dermal filler 4:
[0113] Type III recombinant collagen, recombinant elastin collagen and glycerol were weighed in a mass ratio of 1:1:2 and placed in a beaker. After dissolving with 100 mL of purified water, the pH value of the solution was adjusted to 7.0-8.0 with NaOH to prepare a protein-containing solution with a final concentration of 30 mg / mL.
[0114] Weigh twice the mass of the protein-containing solution of degradable polymer microspheres, and add them into the collagen solution under stirring to obtain a composite microsphere collagen solution.
[0115] Then, under continuous stirring, a cross-linking agent PEGDE with a molecular weight of 800 in an amount twice the mass of the composite microsphere collagen solution was added. After cross-linking at 30°C for 20 hours, the mixture was broken into gel blocks, swelled in PBS buffer, and then washed with PBS buffer at room temperature. The washed gel was homogenized and dispersed, and then 0.3% lidocaine and 1.5% mannitol were added. After stirring and mixing evenly, the mixture was homogenized, filled, and sterilized by wet heat to obtain control dermal filler 4.
[0116] 2. Performance Testing of Dermal Fillers
[0117] 1. Push force test
[0118] Data from similar products and clinical literature show that the ideal pushing force range for filler products that are easy for doctors to inject is 10 to 25N.
[0119] A 1.0 mL syringe from Weigao and a 27G TW1 / 2 needle from Terumo were used to test the pushing force of each group of dermal fillers in the body sliding mode of the intelligent electronic tensile testing machine (XLW-PC) at a test speed of 30 mm / min.
[0120] The push force test results are as follows Figure 1As shown, with the increase of the cross-linking agent content (Example 3, Example 1, Example 2 and Comparative Example 4), the pushing force also shows an increasing trend, and the dermal filler of Comparative Example 4 is sandy, indicating that with the increase of the cross-linking agent content, the cross-linking degree of the gel increases, the hardness increases accordingly, and the pushing force increases accordingly, but the excessive cross-linking agent content will cause sandy phenomenon, which is not conducive to subsequent use. With the increase of the content of degradable polymer microspheres (Comparative Example 1, Example 3, Example 1 and Example 2), the pushing force gradually increases, indicating that with the increase of the concentration of degradable polymer microspheres, the structure of the composite gel becomes more compact, the hardness increases, and the pushing force increases accordingly.
[0121] 2. Rotational rheology test
[0122] The rotational rheology of each group of dermal fillers was tested using a rotational rheometer (NETZSCH Kinexus Lab+), with the frequency range set to 0-10 Hz.
[0123] like Figure 2 As shown in the rotational rheological results of 0.1 Hz, with the increase of the crosslinking agent content (Example 1, Example 2, Comparative Example 4), the rotational rheological data of the gel shows a decreasing trend, indicating that too high a crosslinking agent dosage will cause the gel to be too hard and brittle, and the elastic modulus G' will decrease instead; compared with the gel of Comparative Example 1 without adding the degradable polymer microspheres, the addition of the degradable polymer microspheres in Example 1 can also improve the mechanical properties of the gel, resulting in an increase in viscoelasticity and an increase in the pushing force; compared with the rotational rheological data of the dermal filler prepared by the traditional secondary crosslinking method in Example 1 and Comparative Example 3, it can be seen that the elastic modulus G' of Example 1 is larger than that of Comparative Example 3. This is because the dermal filler prepared by the present invention is not just a physical mixture of microspheres and collagen, but through the action of the crosslinking agent, a multiple crosslinking combination form is formed between the recombinant functional protein, the microspheres and the crosslinking agent, and a denser network structure is constructed. Therefore, the mechanical properties of the dermal filler prepared by the present invention are less likely to be deformed, and it is more suitable for deep and large-area filling.
[0124] 3. Morphological Characterization
[0125] The samples prepared in Example 1, Example 3 and Comparative Example 3 were respectively dispersed and placed on a glass slide, covered with a cover glass, and observed and photographed under an Olympus (Olmpus CX 33) microscope.
[0126] The morphology is as follows Figure 3 As shown, under a microscope, the overall distribution of the dermal filler in Example 1 is more uniform than that in Comparative Example 3.
[0127] 4. In vitro cytotoxicity assay
[0128] Mouse fibroblasts (NCTC Clone 929, L cell, L-929, derivative of Strain L) were cultured in MEM medium containing antibiotics and 10% serum in an incubator at 37°C and 5% CO2. When the cell density reached 80%, they were digested with trypsin and collected for counting. The cell concentration was adjusted to 1×10 5 Add the cell suspension to a 96-well plate, 100 μL per well, for a total of 1×10 4 Cells / well, 37°C, 5% CO2 culture for 24h. Prepare each group of samples to be tested according to 0.2g / mL serum-containing culture medium, extract in a shaker for 24h, the temperature is 37°C, and the speed is 100r / min. After the culture is completed, the culture medium in the culture plate is discarded, and the extract of Example 1 is added to the experimental group; the remaining groups discard the original culture solution, set up a negative control group to add 0.2g / mL serum-containing culture medium, the positive control group to add 10% dimethyl sulfoxide, and the blank control group does not add other substances. Each group has 5 wells and is placed in a 37°C, 5% CO2 incubator for 24h. Subsequently, take out the cell culture plate, discard the culture medium, add 50μL (1mg / mL) of MTT stain to each well, and place it in a 37°C, 5% CO2 saturated humidity incubator for 2h. Finally, discard the liquid in the culture plate, add 100μL of isopropanol to each well, shake and mix, put it into an ELISA reader, and read at 570nm (reference wavelength 620nm). The relative cell survival rate of each concentration group and the positive control group was calculated by the OD value of the blank control group. Relative cell survival rate (%) = (average OD value of the test group / average OD value of the blank control group), with the blank control group being recorded as 100%.
[0129] The results of relative survival rates showed that the relative survival rates of cells in Example 1, the negative control group, and the positive control group were 99%, 98%, and 20%, respectively, indicating that the dermal filler prepared by this method is safe.
[0130] The cell morphology of each group was observed under an inverted microscope (XL Core).
[0131] Cell morphology Figure 4 The negative control has a similar cell morphology to that of Example 1, with no cell lysis and no decrease in cell proliferation. Based on the cell proliferation rate and cell morphology, it can be determined that the dermal filler prepared by the present invention has no cytotoxicity, indicating that it has high biological safety.
[0132] 5. In vivo biocompatibility and degradation testing
[0133] Experimental Animals:
[0134] Adult rats, 8 weeks old, 200-300g, half male and half female
[0135] Experimental process:
[0136] The back skin of the rats was shaved, and 0.1 mL of each sample to be tested (Comparative Example 1, Example 1, Example 3, Comparative Example 3) was taken from the 5×6 cm (tattooed) area on both sides of the spine. Under sterile conditions, a syringe with a 27G thin-walled needle was slowly implanted subcutaneously on the dorsal side of each group of rats, with both sides about 1 cm away from the spine line, and the same side was parallel to the spine line, and the implantation distance (1-2 cm) and implantation shape (elliptical) were ensured to be consistent. Observation points: before surgery, immediately after surgery, 3d, 1w, 2w, 4w, 8w, 12w. The diet, body weight and mental state of the animals were observed, and the injection sites were photographed and recorded. At 12w, the groups were clearly marked, and the samples were taken after taking general photos, embedded for HE staining, and the biocompatibility and degradation of the gel were analyzed.
[0137] HE results are as follows Figure 5 As shown in the figure, the samples prepared by the present invention have no obvious inflammatory reaction, indicating that they have good biocompatibility. It can also be seen from the figure that the degradation of comparative example 1 is the fastest, followed by example 3. When implanted for 3m, the material of comparative example 1 has been completely degraded. This is because the pure collagen filler is easily degraded into amino acid fragments in the body. After compounding with degradable polymer microspheres, as the content of degradable polymer microspheres increases (example 3 and example 1), the degradation of the gel in the body gradually slows down. This is mainly due to the scaffolding effect of the degradable polymer microspheres in the body. In addition, as the content of the degradable polymer microspheres increases, the collagen fibers around the material increase accordingly, indicating that the degradable polymer microspheres can stimulate the regeneration of collagen in the body. The degradation rate of Example 1 is lower than that of Example 1. This is because in the traditional secondary cross-linking preparation method, the cross-linked composite microspheres are physically mixed with the composite protein cross-linked products, while the composite microspheres in the process of the present invention are cross-linked by the covalent bond between collagen and microspheres. Multiple cross-linking networks are formed between the composite microspheres and the protein-containing solution under the action of the cross-linking agent. The overall cross-linking result is tighter, so the prepared dermal filler is injected into the rat body and degrades slowly. In addition, it can be seen from the HE section results that the distribution of the degradable polymer microspheres in Example 3 is not uniform, and the stimulation of collagen regeneration is also uneven.
[0138] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a dermal filler of composite polymer microspheres, characterized in that: The degradable polymer microspheres are mixed with a solution containing protein and then cross-linked once to obtain a dermal filler; The components of the protein-containing solution include recombinant functional proteins and glycerol, and the recombinant functional proteins include recombinant collagen and recombinant elastin; the cross-linking agent used for cross-linking is one of polyethylene glycol and its derivatives with a molecular weight of 200 to 4000 Da.
2. The method for preparing a composite polymer microsphere dermal filler according to claim 1, characterized in that: The degradable polymer microspheres are any one of polycaprolactone block copolymers, polyethylene glycol block copolymers, poly-L-lactic acid block copolymers, poly-D-lactic acid block copolymers, polylactic acid-glycolic acid block copolymers and polyracemic lactic acid block copolymers, or are obtained by melting, granulating and screening two or three of polycaprolactone, polyethylene glycol, poly-L-lactic acid, poly-D-lactic acid and polylactic acid-glycolic acid.
3. The method for preparing a composite polymer microsphere dermal filler according to claim 1, characterized in that: The recombinant functional protein can also be added with one or more of recombinant mussel mucin, recombinant fibronectin and recombinant silk protein; the components of the solution containing protein can also be added with polysaccharides, which are one or more of hyaluronic acid, hyaluronate and sodium alginate.
4. The method for preparing a composite polymer microsphere dermal filler according to claim 3, characterized in that: The mass ratio of the recombinant functional protein, glycerol and polysaccharide is 1:(0.1-10):(0-10).
5. The method for preparing a composite polymer microsphere dermal filler according to claim 1, characterized in that: The total concentration of the recombinant functional protein is 10-60 mg / mL.
6. The method for preparing a composite polymer microsphere dermal filler according to claim 1, characterized in that: The mass ratio of the degradable polymer microspheres to the solution containing the protein is (0.2-20):
1.
7. The method for preparing a composite polymer microsphere dermal filler according to claim 1, characterized in that: The degradable polymer microspheres are mixed with a solution containing protein to obtain a composite microsphere collagen solution, and the composite microsphere collagen solution is mixed with a cross-linking agent at a mass ratio of 1:(0.1-1) to obtain a dermal filler.
8. The method for preparing a composite polymer microsphere dermal filler according to any one of claims 1 to 7, characterized in that: The degradable polymer microspheres are mixed with a solution containing protein and then cross-linked once, and then an anesthetic and a protein protective agent are added and mixed to obtain a dermal filler.
9. The method for preparing a composite polymer microsphere dermal filler according to claim 8, characterized in that: The mass ratio of protein protective agent to recombinant functional protein is (0.5-3):
1.
10. The dermal filler prepared by the method for preparing a dermal filler of composite polymer microspheres according to any one of claims 1 to 9.
Citation Information
Cited By
Medical wound surface composite freeze-dried dressing and preparation method thereof
CN119455076A
Injection type facial filler composition gel for medical beauty as well as preparation method and application of injection type facial filler composition gel
CN121371311A
COMPOSITION FOR COSMETIC TREATMENT OF THE DERMAL
IT202400028338A1
Composition for cosmetic treatment of the dermis
WO2026126162A1