Fused heterocyclic ring polymer containing biisoquinoline structure as well as preparation method and application of fused heterocyclic ring polymer
Through a one-pot reaction of raw materials such as internal acetylenic monomers and benzil monomers under rhodium catalysis, an efficient fused heterocyclic polymer containing bisisoquinoline structure was successfully prepared, which solved the difficulty of preparing bisisoquinoline with the existing technology. By solving the problem of pholine repeating units, it has achieved efficient fluorescence performance and chiral induced circular dichroism signal, and expanded the application of chiral fluorescent functional polymers.
Patent Information
- Application Number
- CN202410927594.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing polyisoquinoline preparation methods are difficult to prepare functional polymer materials containing diisoquinoline repeating units, and the monomer structure is kept from racemization during the synthesis process, resulting in limitations in chiral recognition and asymmetric catalytic applications. limit.
Internal alkyne monomers, benzil monomers, ammonium salts, rhodium catalysts, acids and oxidants are used to perform metal rhodium-catalyzed C-H activation/cyclization one-pot reactions in solvents to obtain fused heterocycles containing bisisoquinoline structures. Polymers can be prepared efficiently by controlling reaction conditions and raw material molar ratios.
Achieve efficient and simple preparation of high molecular weight fused heterocyclic polymers containing biisoquinoline structure, which have excellent fluorescence properties and chiral induced circular dichroism signals, and have unique application value in the field of chiral fluorescent functional polymers .
Smart Images

Figure CN118725264A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of fused heterocyclic polymers, and in particular to a fused heterocyclic polymer containing a biisoquinoline structure and a preparation method and application thereof. Background Art
[0002] Condensed heterocyclic polymers containing quinoline or isoquinoline structures are an important class of functional polymers. Due to their excellent chemical stability, good mechanical properties, special metal coordination and chelating abilities, and excellent optoelectronic properties, they have attracted widespread attention in many fields, and have shown good application prospects in the fields of stimulus-responsive polymer materials, high-temperature resistant conductive polymer materials, electroluminescent or electrochromic devices, and bio / chemical fluorescence sensors. Among them, the preparation method of polyquinoline materials has been relatively fully developed, and can be obtained by oxidative polymerization or electro-oxidative polymerization of quinoline monomers. Polyquinolines with substituents are mostly prepared by acid-catalyzed Friedlander synthesis using benzyl cyanide derivatives as raw materials. In recent years, two-component and multi-component cyclopolymerization based on amine monomers has also been applied to the preparation of substituted polyquinolines. In contrast, the preparation method of polyisoquinoline materials is still developing very slowly. The existing preparation method of polyisoquinoline is difficult to prepare functional polymer materials containing diisoquinoline (a bicyclic structure formed by two isoquinoline units connected by a biphenyl bridge) repeating units.
[0003] In addition, in current research, the diisoquinoline structure mainly appears in the form of small molecules. This type of structural material plays a key role in many fields such as drug manufacturing, biomedicine and optical applications due to its special axial chirality and potential optical activity. Compared with small molecule materials, the physical and chemical properties of polymers can be finely controlled by adjusting multiple parameters such as degree of polymerization, molecular weight distribution, topological structure and morphology. At the same time, they perform better in mechanical strength, thermal stability and processing performance. However, limited by the existing synthesis methods of polyisoquinoline polymers, the preparation, properties and application research of polymer materials containing diisoquinoline structures are still under exploration. In addition, it is also an important technical challenge to keep the monomer structure from being racemized during the synthesis process, and then obtain chiral fused heterocyclic polymer materials with certain application potential in fields such as chiral recognition and asymmetric catalysis.
[0004] Therefore, developing a simple and efficient method to prepare fused heterocyclic functional polymers containing biisoquinoline structures is of great value in both academic research and industrial applications. It will help promote the development of chiral fluorescent functional polymer materials with high chiral purity and superior fluorescent properties, and promote progress in related technical fields. Summary of the invention
[0005] Based on the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a fused heterocyclic polymer containing a biisoquinoline structure and a preparation method and application thereof, aiming to provide a simple and efficient method for preparing a fused heterocyclic functional polymer containing a biisoquinoline structure, so as to solve the problem that the existing polyisoquinoline preparation method is difficult to prepare a functional polymer material containing a biisoquinoline repeating unit.
[0006] The technical solution of the present invention is as follows:
[0007] The first aspect of the present invention provides a method for preparing a fused heterocyclic polymer containing a biisoquinoline structure, which comprises the following steps:
[0008] Adding an internal alkyne monomer, a benzil monomer, an ammonium salt, a rhodium catalyst, an acid and an oxidant into a solvent, and reacting to obtain the fused heterocyclic polymer containing a biisoquinoline structure;
[0009] Wherein, the structural formula of the internal alkyne monomer is as shown in formula (I):
[0010]
[0011] The general structural formula of the benzil monomer is shown in formula (II):
[0012]
[0013] The general structural formula of the fused heterocyclic polymer containing a biisoquinoline structure is shown in formula (III):
[0014]
[0015] In formula (I) and formula (III), R1 and R2 are each independently an aryl group (such as phenyl, substituted phenyl, naphthyl, substituted naphthyl, etc., but not limited thereto), an aryl derivative (such as heteroaryl, etc., specifically a pyridine group, a thiophene group, a furan group, an indole group, etc.), an unsubstituted alkyl group (such as methyl, ethyl, propyl, butyl, etc., of course not limited thereto) or a substituted alkyl group (for example, an alkoxy group, etc., but not limited thereto);
[0016] In formula (II) and formula (III), R3 and R4 are located at any possible position on their respective benzene rings; R3 and R4 are independently an aryl group, an aryl derivative, an aliphatic group (the aliphatic group may be an aliphatic group containing an ester group, or may be an aliphatic group not containing an ester group, for example, the aliphatic group may be an unsubstituted alkyl group; or a substituted alkyl group, such as an alkylamine group, an alkoxy group, an allyl group, an alkyl ester group, etc., but not limited thereto; the aliphatic group may also be an aliphatic alcohol group), a hydrogen atom, a halogen atom (such as F, Cl, Br or I, etc.), a nitro group, a cyano group or a biologically active fragment, wherein the biologically active fragment includes one of terpenes, steroids and vitamins;
[0017] In formula (III), x, y, and z are each independently an integer between 1 and 200 (specifically, 1, 2, 5, 10, 15, 20, 50, 70, 80, 100, 120, 130, 150, 180 or 200, etc.).
[0018] The preparation method provided by the present invention is simple and efficient, and only requires one-step reaction, i.e., a one-pot reaction of CH activation / cyclization catalyzed by metal rhodium, to obtain the target product, and the polymerization reaction yield is high, the raw materials used are cheap and easily available, and the prepared fused heterocyclic polymer containing a biisoquinoline structure has a high molecular weight (weight average molecular weight of 10,000 to 30,000, and polymer dispersity index of 1.2 to 1.8), has excellent solution state or aggregate state fluorescence performance, and can show good circular dichroism spectral signals through chiral induction, and has unique potential application value in the field of chiral fluorescent functional polymers. The present invention effectively solves the problem that the existing polyisoquinoline preparation method is difficult to prepare a functional polymer material containing a biisoquinoline repeating unit.
[0019] In the present invention, the aryl and aryl derivative groups can provide a good conjugation effect, improve the stability of the polymer molecules, and regulate the luminescence properties of the polymer. The aliphatic group can regulate the solubility of the polymer molecules, increase the rotation hindrance of the polymer molecules, and change the polarity of the molecules.
[0020] In the present invention, the role of the ammonium salt is to provide amino groups as a nitrogen source, the role of the acid is to provide an acidic environment to promote the activation cyclization of the reaction, and the role of the oxidant is to promote the catalytic cycle.
[0021] Optionally, the ammonium salt includes at least one of ammonium acetate, ammonium chloride, ammonium carbonate and hydroxylamine hydrochloride, but is not limited thereto;
[0022] The rhodium catalyst comprises one of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer, {(dichloro)(16bR)-1,2,3-trimethyl-2H-cyclopentyl[b]-[6,7]cyclooctane[2,1-a:3,4-a']binaphthyl rhodium(III) dimer} and {(diiodo)(13bS)-7,13-dimethoxy-1,2,3,4,10,12-hexahydro-8H-cyclopentane[5,6]cyclononane[1,2,3-cd:1,9,8-c'd']spirocyclic rhodium(III) dimer}, or the rhodium catalyst comprises (13bR)H-cyclopentadienyl[6,7]cyclooctane[2,1-A:3,4-A']binaphthyl, 4,7-dihydro-2,8-dimethoxy and RhCl3;
[0023] The acid includes at least one of glacial acetic acid, p-toluenesulfonic acid, benzoic acid and pivalic acid, but is not limited thereto;
[0024] The oxidant includes at least one of copper acetate monohydrate, copper sulfate pentahydrate and copper chloride, but is not limited thereto;
[0025] The solvent includes at least one of methanol, 2,2,2-trifluoroethanol, hexafluoroisopropanol, ethanol and isopropanol, but is not limited thereto.
[0026] Optionally, the reaction conditions are:
[0027] Under an inert gas atmosphere or an air atmosphere, the reaction temperature is 80-120°C (for example, 80°C, 90°C, 100°C, 110°C or 120°C, etc.), and the reaction time is 1-24h (for example, 1h, 2h, 5h, 10h, 15h, 20h or 24h, etc.).
[0028] In the present invention, the reaction can be carried out in an inert gas atmosphere or an air atmosphere.
[0029] Optionally, the molar ratio of the internal alkyne monomer, benzil monomer, ammonium salt, rhodium catalyst, acid and oxidant is 1:(0.75-2):(7-14):(0.05-0.2):(6-10):(2-6); for example, the molar ratio of the internal alkyne monomer, benzil monomer, ammonium salt, rhodium catalyst, acid and oxidant may be 1:0.75:7:0.05:6:2, 1:1:10:0.1:8:4, 1:2:14:0.2:10:6, 1:1:12:0.2:10:4 or 1:1.5:11:0.15:9:5, etc.
[0030] The reaction concentration of the internal acetylenic monomer is 0.05-0.3 mol / L, for example, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L or 0.3 mol / L.
[0031] Optionally, after the reaction, before obtaining the fused heterocyclic polymer containing a biisoquinoline structure, the following steps are further included:
[0032] The reaction solution obtained after the reaction is cooled to room temperature, and filtered to obtain a filtrate;
[0033] The filtrate is added to a precipitant for precipitation, and then filtered and dried.
[0034] The polymer product obtained in the present invention is easy to separate, and only needs to be precipitated once in a precipitant to obtain a condensed heterocyclic polymer containing a biisoquinoline structure with high purity.
[0035] In the present invention, specifically, the reaction solution obtained after the reaction is cooled to room temperature, diluted with dichloromethane, and simply filtered through neutral alumina to obtain a filtrate, and then the filtrate is added to a precipitant for precipitation, and the precipitate is collected after filtration and dried to constant weight to obtain a fused heterocyclic polymer containing a biisoquinoline structure.
[0036] Optionally, the precipitant includes at least one of diethyl ether, acetone and n-hexane, but is not limited thereto.
[0037] Optionally, R1 is selected from one of the following structural formulas 1 to 26, R2 is selected from one of the following structural formulas 27 to 41, and R3 and R4 are each independently selected from one of the following structural formulas 27 to 42:
[0038]
[0039]
[0040] represents a connection; m, p, q, r, s, t, and f are each independently an integer between 1 and 20 (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.); u and v are each independently an integer between 0 and 20 (for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.);
[0041] X is an oxygen atom, a sulfur atom or a selenium atom;
[0042] R, R' and R" are each independently a hydrogen atom, a halogen atom (such as F, Cl, Br or I, etc.), an unsubstituted alkyl group, a substituted alkyl group (such as an alkoxy group, an alkylamine group, an allyl group, an alkyl ester group, etc., but not limited thereto), a nitro group, a cyano group, an aryl group (such as a phenyl group, a naphthyl group, an anthracene group, etc.), an aryl derivative (such as a heteroaryl group, such as a pyridine group, a thiophene group, a furan group, an indole group, etc.) or a biologically active fragment, wherein the biologically active fragment includes one of a terpenoid, a steroid, a fatty alcohol and a vitamin.
[0043] The second aspect of the present invention provides a fused heterocyclic polymer containing a biisoquinoline structure, wherein the general structural formula of the fused heterocyclic polymer containing a biisoquinoline structure is:
[0044]
[0045] Wherein, R1 and R2 are each independently an aryl group, an aryl derivative, an unsubstituted alkyl group or a substituted alkyl group (such as an alkoxy group, but not limited thereto);
[0046] R3 and R4 are located at any possible position on the respective benzene rings; R3 and R4 are independently an aryl group, an aryl derivative, an aliphatic group (the aliphatic group may be an aliphatic group containing an ester group, or may be an aliphatic group without an ester group, for example, the aliphatic group may be an unsubstituted alkyl group; it may also be an unsubstituted alkyl group, such as an alkylamine group, an alkoxy group, an allyl group, an alkyl ester group, etc., but not limited thereto; the aliphatic group may also be an aliphatic alcohol group), a hydrogen atom, a halogen atom, a nitro group, a cyano group or a biologically active fragment, wherein the biologically active fragment includes one of terpenes, steroids and vitamins;
[0047] Each group of x, y, and z is independently an integer between 1 and 200 (specifically, it can be 1, 2, 5, 10, 15, 20, 50, 70, 80, 100, 120, 130, 150, 180 or 200, etc.).
[0048] Optionally, R1 is selected from one of the following structural formulas 1 to 26, R2 is selected from one of the following structural formulas 27 to 41, and R3 and R4 are each independently selected from one of the following structural formulas 27 to 42:
[0049]
[0050]
[0051] in, represents a connection; m, p, q, r, s, t, and f are each independently an integer between 1 and 20 (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.); u and v are each independently an integer between 0 and 20 (for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.); X is an oxygen atom, a sulfur atom or a selenium atom; R, R' and R" are each independently a hydrogen atom, a halogen atom (such as F, Cl, Br or I, etc.), an unsubstituted alkyl group, a substituted alkyl group (such as an alkoxy group, an alkylamine group, an allyl group, an alkyl ester group, etc., but not limited thereto), a nitro group, a cyano group, an aryl group, an aryl derivative (such as a heteroaryl group, such as a pyridine group, a thiophene group, a furan group, an indole group, etc.) or a biologically active fragment, and the biologically active fragment includes one of a terpenoid, a steroid, a fatty alcohol and a vitamin.
[0052] The third aspect of the present invention provides a fused heterocyclic polymer containing a biisoquinoline structure prepared by the preparation method of the present invention as described above and / or the use of the fused heterocyclic polymer containing a biisoquinoline structure as described above as an aggregation-induced emission material or a chiral fluorescent material.
[0053] Beneficial effects: The preparation method provided by the present invention is simple and efficient. Only one-step reaction, i.e., a one-pot reaction of CH activation / cyclization catalyzed by metal rhodium, is required to obtain the target product. The polymerization reaction yield is high, and the raw materials used are cheap and readily available. The prepared fused heterocyclic polymer containing a biisoquinoline structure has a high molecular weight (weight average molecular weight of 10,000-30,000, and polymer dispersity index of 1.2-1.8), excellent solution state or aggregate state fluorescence performance, and can show good circular dichroism spectral signals through chiral induction, and has unique potential application value in the field of chiral fluorescent functional polymers. The present invention effectively solves the problem that the existing polyisoquinoline preparation method is difficult to prepare functional polymer materials containing biisoquinoline repeating units. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is the H NMR spectrum of the fused heterocyclic polymer P1 prepared in Example 1 in deuterated dichloromethane.
[0055] Figure 2 This is the H NMR spectrum of the fused heterocyclic polymer P2 prepared in Example 2 in deuterated dichloromethane.
[0056] Figure 3 This is the H NMR spectrum of the fused heterocyclic polymer P3 prepared in Example 3 in deuterated dichloromethane.
[0057] Figure 4This is the H NMR spectrum of the fused heterocyclic polymer P4 prepared in Example 4 in deuterated dichloromethane.
[0058] Figure 5 This is the H NMR spectrum of the fused heterocyclic polymer P5 prepared in Example 5 in deuterated dichloromethane.
[0059] Figure 6 This is the H NMR spectrum of the fused heterocyclic polymer P6 prepared in Example 6 in deuterated dichloromethane.
[0060] Figure 7 (A) is a photoluminescence curve of the condensed heterocyclic polymer P6 in Example 6 in N,N-dimethylformamide solutions with different water contents, (B) is a photoluminescence curve of the condensed heterocyclic polymer P5 in Example 5 in N,N-dimethylformamide solutions with different water contents, (C) is a photoluminescence curve of the condensed heterocyclic polymer P2 in Example 2 and the condensed heterocyclic polymer P4 in Example 4 in solution state and aggregated state, (D) is a graph showing the change trend of the fluorescence emission intensity of the condensed heterocyclic polymer P5 in Example 5 and the condensed heterocyclic polymer P6 in Example 6 in N,N-dimethylformamide solutions with different water contents.
[0061] Figure 8 The absorption spectrum and circular dichroism spectrum of the chiral fused heterocyclic polymer containing a biisoquinoline structure prepared in Example 7 in N,N-dimethylformamide solution. DETAILED DESCRIPTION
[0062] The present invention provides a fused heterocyclic polymer containing a biisoquinoline structure and a preparation method and application thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0063] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0064] The present invention will be further described below by means of specific examples.
[0065] Unless otherwise specified, the raw materials used in the following examples are all commercially available products.
[0066] In the following examples, 4,4′-(1,4-hexenedioxy)bis(tolane) was prepared according to the method disclosed in the literature (Gao, M.; Lam, JWY; Liu, Y.; Li, J.; Tang, BZ Polymer Chemistry 2013, 4(9), 2841-2849).
[0067] 1,1′-[1,2-bis[4-(2-phenylethynyl)phenyl]-1,2-vinyl]bibenzene was prepared according to the method disclosed in the literature (Gao, M.; Lam, JWY; Liu, Y.; Li, J.; Tang, BZ Polymer Chemistry 2013, 4(9), 2841-2849).
[0068] Example 1
[0069] This embodiment provides a fused heterocyclic polymer containing a biisoquinoline structure (ie, fused heterocyclic polymer P1), the structural formula of which is:
[0070]
[0071] This embodiment also provides a method for preparing the above-mentioned fused heterocyclic polymer containing a biisoquinoline structure, wherein the synthesis route of the fused heterocyclic polymer containing a biisoquinoline structure is as follows:
[0072]
[0073] The preparation method of the fused heterocyclic polymer containing a biisoquinoline structure comprises the following steps:
[0074] According to the above synthesis route, under air conditions, 94.1 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 42.1 mg of dibenzoyl, 185.0 mg of ammonium acetate (NH4OAc), 24.7 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer ([Cp*RhCl2]2) and 160 mg of copper(II) acetate hydrate (Cu(OAc)2·H2O), 0.114 mL of glacial acetic acid (AcOH) were added to 2 mL of dry hexafluoroisopropanol (HFIP) to dissolve, and the reaction was stirred at 120°C for 24 h. After the reaction is complete, the reaction mother liquor is diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and then directly precipitated in 100 mL of ether solution. The precipitate is collected and dried under vacuum at 65° C. to constant weight to obtain a fused heterocyclic polymer containing a biisoquinoline structure (i.e., a fused heterocyclic polymer P1) with a yield of 93.9%, an absolute weight average molecular weight of 22800 g / mol, and a polymer dispersibility index (PDI) of 1.70.
[0075] The H NMR spectrum of the fused heterocyclic polymer P1 prepared in Example 1 in deuterated dichloromethane is as follows: Figure 1 As shown. Figure 1 It can be seen that the solvent peak and water peak of deuterated dichloromethane are located at 5.32ppm and 1.52ppm respectively. In addition, all other signals are hydrogen atom signals of fused heterocyclic polymer P1, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 4.0ppm is the characteristic peak of hydrogen atoms on the methylene connected to oxygen on the alkyl chain.
[0076] Example 2
[0077] This embodiment provides a fused heterocyclic polymer containing a biisoquinoline structure (ie, fused heterocyclic polymer P2), the structural formula of which is:
[0078]
[0079] This embodiment also provides a method for preparing the above-mentioned fused heterocyclic polymer containing a biisoquinoline structure, wherein the synthesis route of the fused heterocyclic polymer containing a biisoquinoline structure is as follows:
[0080]
[0081] The preparation method of the fused heterocyclic polymer containing a biisoquinoline structure comprises the following steps:
[0082] According to the above synthesis route, under air conditions, 94.1 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 65.4 mg of dimethyl 4,4'-oxalyldibenzoate, 185.0 mg of ammonium acetate, 24.7 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer and 160 mg of copper(II) acetate hydrate, and 0.114 mL of glacial acetic acid were added to 2 mL of dry hexafluoroisopropanol for dissolution, and the reaction was stirred at 120°C for 24 h. After the reaction is complete, the reaction mother liquor is diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and then directly precipitated in 100 mL of ether solution. The precipitate is collected and dried under vacuum at 65° C. to constant weight to obtain a fused heterocyclic polymer containing a diisoquinoline structure (fused heterocyclic polymer P2) with a yield of 98.0%, an absolute weight average molecular weight of 32700 g / mol, and a PDI of 1.52.
[0083] The H NMR spectrum of the fused heterocyclic polymer P2 prepared in Example 2 in deuterated dichloromethane is as follows: Figure 2 As shown. Figure 2It can be seen that the solvent peak and water peak of deuterated dichloromethane are located at 5.32ppm and 1.52ppm respectively. In addition, all other signals are hydrogen atom signals of fused heterocyclic polymer P2, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 3.8ppm is the characteristic peak of hydrogen atoms of methoxy in fused heterocyclic polymer P2, and 4.0ppm is the characteristic peak of hydrogen atoms on methylene connected to oxygen on the alkyl chain.
[0084] Example 3
[0085] This embodiment provides a fused heterocyclic polymer containing a biisoquinoline structure (ie, a fused heterocyclic polymer P3), the structural formula of which is:
[0086]
[0087] This embodiment also provides a method for preparing the above-mentioned fused heterocyclic polymer containing a biisoquinoline structure, wherein the synthesis route of the fused heterocyclic polymer containing a biisoquinoline structure is as follows:
[0088]
[0089] The preparation method of the fused heterocyclic polymer containing a biisoquinoline structure comprises the following steps:
[0090] According to the above synthetic route, under air conditions, 94.1 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 64.5 mg of 4,4-di-tert-butylbenzil, 185.0 mg of ammonium acetate, 24.7 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer, 160 mg of copper(II) acetate hydrate, and 0.114 mL of glacial acetic acid were added to 2 mL of dry hexafluoroisopropanol for dissolution, and stirred at 120°C for 24 hours. After the reaction was complete, the reaction mother liquor was diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and directly precipitated in 100 mL of ether solution, the precipitate was collected, and vacuum dried at 65°C to constant weight to obtain a fused heterocyclic polymer containing a diisoquinoline structure (i.e., fused heterocyclic polymer P3), with a yield of 48.8%, an absolute weight average molecular weight of 41700 g / mol, and a PDI of 2.22.
[0091] The nuclear magnetic hydrogen spectrum of the fused heterocyclic polymer P3 prepared in Example 3 in deuterated dichloromethane is as follows Figure 3 As shown. Figure 3It can be seen that the solvent peak and water peak of deuterated dichloromethane are located at 5.32ppm and 1.52ppm respectively. In addition, all other signals are hydrogen atom signals of fused heterocyclic polymer P3, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 1.2ppm is the characteristic peak of hydrogen atoms of methyl in fused heterocyclic polymer P3, and 4.0ppm is the characteristic peak of hydrogen atoms on methylene connected to oxygen on the alkyl chain.
[0092] Example 4
[0093] This embodiment provides a fused heterocyclic polymer containing a biisoquinoline structure (ie, fused heterocyclic polymer P4), the structural formula of which is:
[0094]
[0095] This embodiment also provides a method for preparing the above-mentioned fused heterocyclic polymer containing a biisoquinoline structure, wherein the synthesis route of the fused heterocyclic polymer containing a biisoquinoline structure is as follows:
[0096]
[0097] The preparation method of the fused heterocyclic polymer containing a biisoquinoline structure comprises the following steps:
[0098] According to the above synthetic route, under air conditions, 94.1 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 54.1 mg of 3,3'-dimethoxybenzil, 185.0 mg of ammonium acetate, 24.7 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer, 160 mg of copper(II) acetate hydrate, and 0.114 mL of glacial acetic acid were added to 2 mL of dry hexafluoroisopropanol for dissolution, and stirred at 120°C for 24 hours. After the reaction was complete, the reaction mother liquor was diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and directly precipitated in 100 mL of ether solution, the precipitate was collected, and vacuum dried at 65°C to constant weight to obtain a fused heterocyclic polymer containing a diisoquinoline structure (i.e., fused heterocyclic polymer P4), with a yield of 16.6%, an absolute weight average molecular weight of 23100 g / mol, and a PDI of 1.48.
[0099] The H NMR spectrum of the fused heterocyclic polymer P4 prepared in Example 4 in deuterated dichloromethane is as follows: Figure 4 As shown. Figure 4It can be seen that the solvent peak and water peak of deuterated dichloromethane are located at 5.32ppm and 1.52ppm respectively. In addition, all other signals are hydrogen atom signals of fused heterocyclic polymer P4, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 3.3-4.2ppm includes the characteristic peaks of hydrogen atoms of methoxy in fused heterocyclic polymer P4, and the characteristic peaks of hydrogen atoms on methylene connected to oxygen on the alkyl chain.
[0100] Example 5
[0101] This embodiment provides a fused heterocyclic polymer containing a biisoquinoline structure (ie, fused heterocyclic polymer P5), the structural formula of which is:
[0102]
[0103] This embodiment also provides a method for preparing the above-mentioned fused heterocyclic polymer containing a biisoquinoline structure, wherein the synthesis route of the fused heterocyclic polymer containing a biisoquinoline structure is as follows:
[0104]
[0105] The preparation method of the fused heterocyclic polymer containing a biisoquinoline structure comprises the following steps:
[0106] According to the above synthetic route, under air conditions, 94.1 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 54.1 mg of 2,2-dimethoxybenzil, 185.0 mg of ammonium acetate, 24.7 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer, 160 mg of copper(II) acetate hydrate and 0.114 mL of glacial acetic acid were added to 2 mL of dry hexafluoroisopropanol for dissolution, and stirred at 120°C for 24 hours. After the reaction was complete, the reaction mother liquor was diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and then directly precipitated in 100 mL of ether solution, the precipitate was collected, and vacuum dried at 65°C to constant weight to obtain a fused heterocyclic polymer containing a diisoquinoline structure (i.e., fused heterocyclic polymer P5), with a yield of 89.5%, an absolute weight average molecular weight of 21800 g / mol, and a PDI of 1.28.
[0107] The H NMR spectrum of the fused heterocyclic polymer P5 prepared in this example in deuterated dichloromethane is as follows: Figure 5 As shown. Figure 5It can be seen that the solvent peak and water peak of deuterated dichloromethane are located at 5.32ppm and 1.52ppm respectively. In addition, all other signals are hydrogen atom signals of fused heterocyclic polymer P5, and several characteristic hydrogen atom signals can also be assigned accordingly. Among them, 3.3-4.1ppm includes the characteristic peak of hydrogen atoms of methoxy in fused heterocyclic polymer P5, and the characteristic peak of hydrogen atoms on methylene connected to oxygen on the alkyl chain. The characteristic peak of hydrogen atoms of methoxy in fused heterocyclic polymer P5.
[0108] Example 6
[0109] This embodiment provides a fused heterocyclic polymer containing a biisoquinoline structure (ie, fused heterocyclic polymer P6), the structural formula of which is:
[0110]
[0111] This embodiment also provides a method for preparing the above-mentioned fused heterocyclic polymer containing a biisoquinoline structure, wherein the synthesis route of the fused heterocyclic polymer containing a biisoquinoline structure is as follows:
[0112]
[0113] The preparation method of the fused heterocyclic polymer containing a biisoquinoline structure comprises the following steps:
[0114] Under air conditions, 106.5 mg of 1,1'-[1,2-bis[4-(2-phenylethynyl)phenyl]-1,2-vinyl]bisbenzene, 42.1 mg of dibenzoyl, 185.0 mg of ammonium acetate, 24.7 mg of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer, 160 mg of copper(II) acetate hydrate and 0.114 mL of glacial acetic acid were added to 2 mL of dry hexafluoroisopropanol solution for dissolution, and stirred for reaction at 120° C. for 24 h. After the reaction was complete, the reaction mother liquor was diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and then directly precipitated in 100 mL of ether solution. The precipitate was collected and dried under vacuum at 65° C. to constant weight to obtain a fused heterocyclic polymer containing a diisoquinoline structure (i.e., a fused heterocyclic polymer P6), with a yield of 61.2%, an absolute weight average molecular weight of 18900 g / mol, and a PDI of 1.19.
[0115] The H NMR spectrum of the fused heterocyclic polymer P6 prepared in this example in deuterated dichloromethane is as follows: Figure 6 As shown. Figure 6 It can be seen that the solvent peak and water peak of deuterated dichloromethane are located at 5.32ppm and 1.52ppm respectively. In addition, all other signals are hydrogen atom signals of P6.
[0116] The photoluminescence curves and fluorescence emission intensity variation trends of the condensed heterocyclic polymer P2 in Example 2, the condensed heterocyclic polymer P4 in Example 4, the condensed heterocyclic polymer P5 in Example 5, and the condensed heterocyclic polymer P6 in Example 6 in N,N-dimethylformamide solutions with different water contents (i.e., mixed solutions of N,N-dimethylformamide and water with different water contents, wherein the volume content of water is 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% and 90%, respectively) were tested. The results are as follows Figure 7 The luminescence curves and fluorescence emission intensity variation trends of the condensed heterocyclic polymer P6 prepared in Example 6 in N,N-dimethylformamide solutions with different water contents are shown in FIG. Figure 7 As shown in (A) and (D), I is the luminescence intensity in N,N-dimethylformamide solutions with different water contents, and I0 is the luminescence intensity in pure N,N-dimethylformamide solutions. It can be seen that with the increase of water content, the fluorescence emission intensity of the condensed heterocyclic polymer P6 gradually increases, and is still stronger than 0% water content at 90% water content, proving that the condensed heterocyclic polymer P6 exhibits aggregation-induced emission and has excellent aggregated state fluorescence properties. Specifically, due to the restricted intramolecular motion (RIM) mechanism, in the tetraphenylethylene group, the benzene ring can rotate freely and consume energy through non-radiative pathways, but when the tetraphenylethylene groups aggregate in the polymer, these rotations return to restrictions, thereby suppressing the non-radiative relaxation channel and enhancing the radiative luminescence of the excited state.
[0117] As can be seen from (C) in 7, the condensed heterocyclic polymers P2 and P4 emit light well in N,N-dimethylformamide solution with 0% water content (solution state), but the fluorescence intensity of the condensed heterocyclic polymers P2 and P4 in N,N-dimethylformamide solution with 90% water content (aggregate state) is weaker than that in N,N-dimethylformamide solution with 0% water content (solution state), that is, the condensed heterocyclic polymers P2 and P4 exhibit aggregation-induced quenching effect.
[0118] From (B) and (D) in 7, it can be seen that in N,N-dimethylformamide, with the increase of water content, the fluorescence emission intensity of the condensed heterocyclic polymer P5 gradually weakens, showing the phenomenon of aggregation-induced quenching. The above results indicate that the condensed heterocyclic polymers P2, P4, and P5 have aggregation-induced quenching properties.
[0119] Example 7
[0120] This embodiment provides a method for preparing a chiral fused heterocyclic polymer containing a biisoquinoline structure (chiral fused heterocyclic polymer P5, denoted as P5-chiral), comprising the following steps:
[0121] Under air conditions, 47.05 mg of 4,4'-(1,4-hexenedioxy)bis(diphenylacetylene), 27.05 mg of 2,2-dimethoxybenzil, 92.5 mg of ammonium acetate, 24.76 mg of chiral catalyst {(dichloro)(16bR)-1,2,3-trimethyl-2H-cyclopentyl[b]-[6,7]cyclooctane[2,1-a:3,4-a']binaphthyl rhodium (III) dimer}, 80 mg of copper (II) acetate hydrate and 0.057 mL of glacial vinegar were added. The acid was added to 1 mL of dry hexafluoroisopropanol solution to dissolve, and the reaction was stirred at 120° C. for 24 h. After the reaction was complete, the reaction mother liquor was diluted with 2 mL of dichloromethane, filtered through a 2 cm high neutral alumina column, and then directly precipitated in 100 mL of ether solution. The precipitate was collected and dried under vacuum at 65° C. to constant weight to obtain a chiral fused heterocyclic polymer containing a diisoquinoline structure, namely P5-chirality, with a yield of 91.8%, an absolute weight average molecular weight of 26500 g / mol, and a PDI of 1.38.
[0122] In this embodiment, the use of a chiral catalyst can induce the generation of an optically active chiral condensed heterocyclic polymer P5. At the same time, this embodiment also uses the same method to induce the generation of a chiral condensed heterocyclic polymer P3 (denoted as P3-chirality) and a chiral condensed heterocyclic polymer P4 (denoted as P4-chirality) using a chiral catalyst. The absorption spectra of P3-chirality, P4-chirality, and P5-chirality in N,N-dimethylformamide solution ( Figure 8 ) and Circular Dichroism (CD) spectra ( Figure 8 As shown in the figure below Figure 8 As shown. Figure 8 It can be seen that the generated polymer has a positive CD signal at 270-340nm, which corresponds to the absorption of the polymer, indicating that the above method has prepared a fused heterocyclic polymer with a specific axial chiral stereostructure.
[0123] In summary, the present invention provides a fused heterocyclic polymer containing a biisoquinoline structure and a preparation method and application thereof. The preparation method provided by the present invention is simple, and only requires a one-step reaction, i.e., a one-pot reaction of CH activation / cyclization catalyzed by metal rhodium, to obtain the target product, and the polymerization reaction yield is good. The raw materials used are cheap and readily available. The prepared fused heterocyclic polymer containing a biisoquinoline structure has a high molecular weight (weight average molecular weight of 10,000 to 30,000, and PDI of 1.2 to 1.8), has excellent solution state or aggregate state fluorescence performance, and can show good circular dichroism spectral signals through chiral induction, and has unique potential application value in the field of chiral fluorescent functional polymers.
[0124] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a fused heterocyclic polymer containing a biisoquinoline structure, characterized in that: The steps include: Adding an internal alkyne monomer, a benzil monomer, an ammonium salt, a rhodium catalyst, an acid and an oxidant into a solvent, and reacting to obtain the fused heterocyclic polymer containing a biisoquinoline structure; Wherein, the structural formula of the internal alkyne monomer is as shown in formula (I): The general structural formula of the benzil monomer is shown in formula (II): The general structural formula of the fused heterocyclic polymer containing a biisoquinoline structure is shown in formula (III): In formula (I) and formula (III), R1 and R2 are each independently an aryl group, an aryl derivative, an unsubstituted alkyl group or a substituted alkyl group; In formula (II) and formula (III), R3 and R4 are located at any possible position on the respective benzene rings; R3 and R4 are independently an aryl group, an aryl derivative, an aliphatic group, a hydrogen atom, a halogen atom, a nitro group, a cyano group or a biologically active fragment, wherein the biologically active fragment comprises one of a terpenoid, a steroid and a vitamin; In formula (III), x, y and z are each independently an integer between 1 and 200.
2. The preparation method according to claim 1, characterized in that: The ammonium salt includes at least one of ammonium acetate, ammonium chloride, ammonium carbonate and hydroxylamine hydrochloride; The rhodium catalyst comprises one of dichloro(pentamethylcyclopentadienyl)rhodium(III) dimer, {(dichloro)(16bR)-1,2,3-trimethyl-2H-cyclopentyl[b]-[6,7]cyclooctane[2,1-a:3,4-a']binaphthyl rhodium(III) dimer} and {(diiodo)(13bS)-7,13-dimethoxy-1,2,3,4,10,12-hexahydro-8H-cyclopentane[5,6]cyclononane[1,2,3-cd:1,9,8-c'd']spirocyclic rhodium(III) dimer}, or the rhodium catalyst comprises (13bR)H-cyclopentadienyl[6,7]cyclooctane[2,1-A:3,4-A']binaphthyl, 4,7-dihydro-2,8-dimethoxy and RhCl3; The acid comprises at least one of glacial acetic acid, p-toluenesulfonic acid, benzoic acid and pivalic acid; The oxidant comprises at least one of copper acetate monohydrate, copper sulfate pentahydrate and copper chloride; The solvent includes at least one of methanol, 2,2,2-trifluoroethanol, hexafluoroisopropanol, ethanol and isopropanol.
3. The preparation method according to claim 1, characterized in that: The reaction conditions are: In an inert gas atmosphere or an air atmosphere, the reaction temperature is 80 to 120° C. and the reaction time is 1 to 24 hours.
4. The preparation method according to claim 1, characterized in that: The molar ratio of the internal acetylene monomer, benzil monomer, ammonium salt, rhodium catalyst, acid and oxidant is 1:(0.75-2):(7-14):(0.05-0.2):(6-10):(2-6); The reaction concentration of the internal acetylene monomer is 0.05-0.3 mol / L.
5. The preparation method according to claim 3, characterized in that: After the reaction, the following steps are further included before obtaining the fused heterocyclic polymer containing a biisoquinoline structure: The reaction solution obtained after the reaction is cooled to room temperature, and filtered to obtain a filtrate; The filtrate is added to a precipitant for precipitation, and then filtered and dried.
6. The preparation method according to claim 5, characterized in that: The precipitant includes at least one of ether, acetone and n-hexane.
7. The preparation method according to any one of claims 1 to 6, characterized in that: R1 is selected from one of the following structural formulas 1 to 26, R2 is selected from one of the following structural formulas 27 to 41, and R3 and R4 are each independently selected from one of the following structural formulas 27 to 42: Indicates a connection; m, p, q, r, s, t, f are each independently an integer between 1 and 20; u and v are each independently an integer between 0 and 20; X is an oxygen atom, a sulfur atom or a selenium atom; R, R' and R" are each independently a hydrogen atom, a halogen atom, an unsubstituted alkyl group, a substituted alkyl group, a nitro group, a cyano group, an aryl group, an aryl derivative or a biologically active fragment, wherein the biologically active fragment includes one of a terpenoid, a steroid, a fatty alcohol and a vitamin.
8. A fused heterocyclic polymer containing a biisoquinoline structure, characterized in that: The general structural formula of the fused heterocyclic polymer containing a biisoquinoline structure is: Wherein, R1 and R2 are each independently an aryl group, an aryl derivative, an unsubstituted alkyl group or a substituted alkyl group; R3 and R4 are located at any possible position on the respective benzene rings; R3 and R4 are each independently an aryl group, an aryl derivative, an aliphatic group, a hydrogen atom, a halogen atom, a nitro group, a cyano group or a biologically active fragment, wherein the biologically active fragment comprises one of terpenes, steroids and vitamins; Each of x, y and z is independently an integer between 1 and 200.
9. The fused heterocyclic polymer containing a biisoquinoline structure according to claim 8, characterized in that: R1 is selected from one of the following structural formulas 1 to 26, R2 is selected from one of the following structural formulas 27 to 41, and R3 and R4 are each independently selected from one of the following structural formulas 27 to 42: in, represents a connection point; m, p, q, r, s, t, f are each independently an integer between 1 and 20; u and v are each independently an integer between 0 and 20; X is an oxygen atom, a sulfur atom or a selenium atom; R, R' and R" are each independently a hydrogen atom, a halogen atom, an unsubstituted alkyl group, a substituted alkyl group, a nitro group, a cyano group, an aryl group, an aryl derivative or a biologically active fragment, wherein the biologically active fragment includes one of a terpenoid, a steroid, a fatty alcohol and a vitamin.
10. Use of a fused heterocyclic polymer containing a biisoquinoline structure prepared by the preparation method according to any one of claims 1 to 7 and / or a fused heterocyclic polymer containing a biisoquinoline structure according to any one of claims 8 to 9 as an aggregation-induced emission material or a chiral fluorescent material.
Citation Information
Patent Citations
Polyquinolinazine compound, and preparation method and application thereof
CN113388105A
Polyquinoline diketone compound as well as preparation method and application thereof
CN113683776A
Synthesis method of aminoisoquinoline polycondensed ring compound
CN114456111A
Polysubstituted polyquinoline as well as preparation method and application thereof
CN115651193A
Polysubstituted nitrogen and sulfur-containing fused heterocycle polymer as well as preparation method and application thereof
CN116462843A
Cited By
Fused heterocyclic polymer, and preparation method therefor and use thereof
WO2026156950A1