Active energy ray curable adhesive composition, cured product and adhesive sheet
By optimizing the ratio of polyurethane and polyisocyanate and combining it with specific mono(meth)acrylate, a high-performance active energy ray-curable adhesive composition is formed, which solves the problems of light resistance, adhesion and adhesive strength in the existing technology. The problem of height difference and conformability achieves excellent performance and durability under high temperature, high humidity and sunlight conditions.
Patent Information
- Application Number
- CN202410356402.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
Smart Images

Figure BDA0004761489120000041 
Figure BDA0004761489120000251 
Figure BDA0004761489120000261
Abstract
Description
Technical Field The present disclosure relates to an active energy ray-curable adhesive composition, a cured product, and an adhesive sheet. Background Art
[0001] In recent years, display devices such as touch panels have been used in digital information devices such as mobile phones, portable game consoles, and car navigation systems. In addition, optical components such as liquid crystal elements, light-emitting diode elements, and organic electroluminescent elements are often used in the above-mentioned display devices.
[0002] For the purpose of bonding the display device to the above-mentioned optical member and the optical member to each other, a transparent double-sided adhesive sheet is used when manufacturing the display device. The above-mentioned double-sided adhesive sheet requires properties such as adhesion and transparency. As such an adhesive sheet, an active energy line-curable adhesive composition containing polyurethane and various monomers is proposed, and the polyurethane is a polyurethane formed by reacting a hydroxyl-containing (meth) acrylate and a hydroxyl-containing photopolymerization initiator with respect to a prepolymer of a polyol and a polyisocyanate (see Patent Document 1). Prior art literature Patent Literature
[0003] Patent Document 1: Japanese Patent Application Laid-Open No. 2020-037689 Summary of the invention Technical problem to be solved by the invention
[0004] The active energy ray-curable adhesive composition of Patent Document 1 has room for improvement in terms of the property of not changing color when exposed to sunlight, light from optical components, etc. (also referred to as "light resistance" in this disclosure), but this improvement also has problems in terms of excellent adhesion, conformability to height differences, moisture and heat resistance, etc.
[0005] The technical problem of the present disclosure is to provide an active energy ray-curable adhesive composition, a cured product, and an adhesive sheet that are excellent in adhesive strength, conformability to uneven heights, moisture and heat resistance, and light resistance. Technical means to solve technical problems
[0006] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by using a predetermined active energy ray-curable adhesive composition, a cured product thereof, and an adhesive sheet having the cured product thereof, thereby completing the present invention.
[0007] That is, the present invention relates to the following items 1 to 3. (Item 1) 1. An active energy ray-curable adhesive composition, wherein the composition contains: (A) polyurethane, which is a reaction product of (a1) a polyether polyol containing a linear aliphatic hydrocarbon group, (a2) a polyisocyanate, and (a3) a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate, (B) a mono(meth)acrylate containing a primary hydroxyl group, and (C) a mono(meth)acrylate having no hydroxyl group; The component (C) contains (c1) and / or (c2), wherein (c1) is a (meth)acrylate having a glass transition temperature of less than -5°C when forming a homopolymer, and (c2) is a (meth)acrylate having a glass transition temperature of -5°C or higher when forming a homopolymer; With respect to the total amount of component (a1), component (a2) and component (a3), which is 100 mol%, component (a1) is 35 mol% to 70 mol%, component (a2) is 25 mol% to 60 mol%, and component (a3) is 1 mol% to 20 mol%; Relative to 100% by mass (solid content conversion) of the total amount of component (A), component (B) and component (C), component (A) is 10% to 40% by mass, component (B) is 20% to 35% by mass, component (c1) is 20% to 40% by mass, and component (c2) is 10% to 25% by mass. (Item 2) A cured product, which is a cured product of the active energy ray-curable adhesive composition according to item 1. (Item 3) An adhesive sheet having the cured product according to item 2 on at least one surface of a substrate. Beneficial Effects
[0008] The adhesive layer (also referred to as “cured product” in the present disclosure) of the active energy ray-curable adhesive composition of the present disclosure is excellent in adhesive strength, conformability to uneven surfaces, moisture and heat resistance, and light resistance. DETAILED DESCRIPTION
[0009] In the whole of the present disclosure, the numerical range of each physical property value, content, etc. can be appropriately set (for example, selected from the upper and lower limits described in the following items). Specifically, with respect to the numerical value α, when A1, A2, A3, etc. are exemplified as the lower limit of the numerical value α and B1, B2, B3, etc. are exemplified as the upper limit of the numerical value α, the range of the numerical value α is exemplified as above A1, above A2, above A3, below B1, below B2, below B3, A1-B1, A1-B2, A1-B3, A2-B1, A2-B2, A2-B3, A3-B1, A3-B2, A3-B3, etc. In addition, in the present disclosure, "-" is used to indicate the meaning of including the numerical values before and after it as the lower limit and upper limit. Below, each component, cured product, adhesive sheet, etc. of the active energy ray-curable adhesive composition provided by the present disclosure are described in detail.
[0010] <(A)Component> (A) is a polyurethane which is a reaction product of (a1) a linear aliphatic hydrocarbon group-containing polyether polyol, (a2) a polyisocyanate, and (a3) a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate.
[0011] <(a1)Component> Component (a1) is a polyether polyol containing a straight-chain aliphatic hydrocarbon group. If a polyether polyol containing a branched aliphatic hydrocarbon group (polypropylene glycol, dipropylene glycol, etc.) is used as a substitute for component (a1), the light resistance is deteriorated, which is not preferred. In addition, "polyether polyol containing a straight-chain aliphatic hydrocarbon group" means a polyether polyol having only a straight chain in the aliphatic hydrocarbon portion, and is a polyether polyol having no branched chain, aliphatic ring, or aromatic ring in the portion.
[0012] As the component (a1), one or more selected from polyethylene glycol and polytetramethylene ether glycol can be exemplified.
[0013] The component (a1) may be a commercially available product. Examples of such products include: polyethylene glycol, product name: "Polyethylene Glycol #1,540" (manufactured by Nacalai Tesque Co., Ltd.); polytetramethylene ether glycol, product names: "PTMG650", "PTMG1000", "PTMG2000", "PTMG3000" (manufactured by Mitsubishi Chemical Co., Ltd.), etc.
[0014] The component (a1) is preferably polytetramethylene ether glycol because the adhesive layer is likely to become flexible and the durability after a light resistance test is likely to be excellent.
[0015] As the upper limit of the number average molecular weight of (a1) component, 10000, 9000, 8000, 7000, 6000, 5000, 4000, 3000, 2000, 1000 etc. can be exemplified, and as the lower limit, 9000, 8000, 7000, 6000, 5000, 4000, 3000, 2000, 1000, 700 etc. can be exemplified. In one embodiment, the number average molecular weight of (a1) component is preferably more than 700 and less than 10000. The lower the number average molecular weight of (a1) component, the more there is a tendency for the adhesive layer to harden, and the higher the number average molecular weight of (a1) component, the more there is a tendency for the adhesive layer to soften, therefore, if within the above-mentioned preferred range, it is easy to take into account both adhesion and height difference conformability. In the present disclosure, the number average molecular weight can be obtained by the method described in JIS K7252-1:2016. In addition, the "height difference conformability" of the present disclosure has the same meaning as that described in Japanese Patent Application Laid-Open No. 2020-037689.
[0016] The component (a1) may also contain a repeating unit containing a hydrocarbon group having an ether bond, such as polytetramethylene ether glycol represented by the general formula (1). The upper limit of the number of carbon atoms of the hydrocarbon group in the repeating unit of the component (a1) may be 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, etc., and the lower limit may be 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, etc. As one embodiment, in order to easily increase the compatibility with other components and to easily achieve the effects of the present disclosure, the number of carbon atoms of the hydrocarbon group in the repeating unit of the component (a1) is preferably 1 to 30, more preferably 3 to 6, and particularly preferably 4 to 6.
[0017] General formula (1): [Chemistry 1]
[0018] (In the formula, n is an integer from 1 to 30.)
[0019] Examples of the upper limit of n in the general formula (1) include 30, 25, 20, 15, 10, 5, 4, 3, 2, etc., and examples of the lower limit include 25, 20, 15, 10, 5, 4, 3, 2, 1, etc. In one embodiment, n in the general formula (1) is preferably about 1 to 30.
[0020] As the upper limit of the hydroxyl number of (a1) component, 3.0, 2.8, 2.5, 2.3, 2.0, 1.8, etc. can be exemplified, and as the lower limit, 2.8, 2.5, 2.3, 2.0, 1.8, 1.5, etc. can be exemplified. In one embodiment, the hydroxyl number of (a1) component is preferably more than 1.5 and less than 3.0, more preferably more than 1.8 and less than 2.5. Because the hydroxyl number of (a1) component is within the above range, the height difference conformability and cutting property of the adhesive layer are more excellent, so it is preferred. In the present disclosure, the hydroxyl number can be obtained by the method described in JIS K1557-1:2007. Specifically, the hydroxyl number can be obtained by acetylation.
[0021] In the total amount of 100 mass % of the components (a1), (a2) and (a3) of the present disclosure, as the upper limit of the content (solid content conversion) occupied by the component (a1), 99 mass %, 95 mass %, 90 mass %, 85 mass %, 80 mass %, 75 mass %, 70 mass %, 65 mass %, 60 mass %, 55 mass %, etc., can be exemplified, and as the lower limit, 95 mass %, 90 mass %, 85 mass %, 80 mass %, 75 mass %, 70 mass %, 65 mass %, 60 mass %, 55 mass %, 50 mass %, etc. can be exemplified. In one embodiment, in order to well show the effect of the present disclosure, in the total amount of 100 mass % of the components (a1), (a2) and (a3) of the present disclosure, the content (solid content conversion) occupied by the component (a1) is preferably 50 mass % to 99 mass %.
[0022] The upper limit of the content (in terms of solid content) of the component (a1) in the total amount of 100 mol% of the component (a1), the component (a2), and the component (a3) of the present disclosure may be 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, etc., and the lower limit may be 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, etc. In one embodiment, in order to well demonstrate the effect of the present disclosure, the content (in terms of solid content) of the component (a1) in the total amount of 100 mol% of the component (a1), the component (a2), and the component (a3) of the present disclosure is 35 mol% to 70 mol%.
[0023] <(a2) Component> (a2) component is a polyisocyanate. As the (a2) component, one or more selected from aliphatic polyisocyanates and aromatic polyisocyanates can be exemplified. As the aliphatic, one or more selected from linear aliphatic, branched aliphatic, and alicyclic aliphatic can be exemplified. As "poly", two, three, four, etc. can be exemplified.
[0024] Examples of the linear aliphatic diisocyanate include one or more selected from trimethylene diisocyanate, tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, hexamethylene diisocyanate, octamethylene diisocyanate, and decamethylene diisocyanate.
[0025] Examples of the branched aliphatic diisocyanate include one or more selected from methyl 2,6-diisocyanatohexanoate and trimethylhexamethylene diisocyanate.
[0026] Examples of the alicyclic aliphatic diisocyanate include dicyclohexylmethane-4,4′-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane (1,3-bis(isocyanatomethyl)cyclohexane), cyclohexane-1,4-diylbis(methylene)diisocyanate, 1-methylcyclohexane-2,4-diyldiisocyanate, 1,4-cyclohexane diisocyanate, hydrogenated xylene diisocyanate, hydrogenated toluene diisocyanate, and at least one selected from norbornene diisocyanate.
[0027] Examples of the linear aliphatic triisocyanate include lysine triisocyanate and the like.
[0028] As other polyisocyanates, examples include: the polyisocyanates exemplified above, adducts of various known polyisocyanates; polymers of these isocyanates, etc. As such polyisocyanates, examples include biuret, urate, adduct, allophanate, etc. As biuret of polyisocyanate, examples include product names: "Duranet 24A-100", "Duranet 22A-75P", "Duranet 21S-75E" (above, manufactured by Asahi Chemical Industry Co., Ltd.), etc. As urate of polyisocyanate, examples include product names: "Coronet HK", "Coronet HXR" (all manufactured by Tosoh Corporation), etc. Examples of the adduct of polyisocyanate include product names such as "Duranet P301-75E" (manufactured by Asahi Kasei Corporation). Examples of the allophanate of polyisocyanate include product names such as "Coronet 2770" (manufactured by Tosoh Corporation).
[0029] Since the adhesive layer is likely to have excellent durability after a moisture and heat resistance test and a light resistance test and to show good conformability to height differences, the component (a2) is preferably an aliphatic diisocyanate, and more preferably a linear aliphatic diisocyanate and / or an alicyclic aliphatic diisocyanate.
[0030] The average number of isocyanate groups of the component (a2) may be about 2 or more and about 10 or less. In addition, the average number of isocyanate groups can be calculated by the following formula: Average number of isocyanate groups = (number average molecular weight (Mn) × isocyanate group concentration (%)) / (42.02 × 100). The isocyanate group concentration (%) in the formula is a value measured by the method described in JIS K 1603-1:2007.
[0031] As the upper limit of the molecular weight of the component (a2), 1000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, etc. can be exemplified, and as the lower limit, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, 25, etc. can be exemplified. As an embodiment, the molecular weight of the component (a2) is preferably about 25 to 1000. In the present disclosure, when only "molecular weight" is recorded, it means a value calculated based on an atomic weight standard.
[0032] In the total amount of 100 mass% of the components (a1), (a2) and (a3) of the present disclosure, as an upper limit of the content (converted to solid content) of the component (a2), 50 mass%, 45 mass%, 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, 5 mass%, 1 mass%, 0.5 mass% and the like can be exemplified, and as a lower limit, 45 mass%, 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, 5 mass%, 1 mass%, 0.5 mass%, 0.1 mass% and the like can be exemplified. In one embodiment, in order to well demonstrate the effects of the present disclosure, the content of component (a2) in the total amount of 100% by mass of the components (a1), (a2) and (a3) of the present disclosure (converted to solid content) is preferably 0.1% by mass to 50% by mass.
[0033] In the total amount of 100 mol% of the components (a1), (a2) and (a3) of the present disclosure, the upper limit of the content (solid content conversion) of the component (a2) may be 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, etc., and the lower limit may be 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, etc. In one embodiment, in order to well show the effect of the present disclosure, the content (solid content conversion) of the component (a2) in the total amount of 100 mol% of the components (a1), (a2) and (a3) of the present disclosure is 25 mol% to 60 mol%.
[0034] The upper limit of the content ratio (mass basis, solid content conversion) of the component (a1) to the component (a2) [((a1) component) / ((a2) component)] may be 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, etc., and the lower limit may be 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, etc. In one embodiment, the content ratio (mass basis, solid content conversion) of the component (a1) to the component (a2) [((a1) component) / ((a2) component)] is preferably about 50 / 50 to 99 / 1, and more preferably about 65 / 35 to 95 / 5.
[0035] The upper limit of the molar ratio of the component (a1) to the component (a2) [(component (a1)) / (component (a2))] may be 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, etc., and the lower limit may be 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, etc. In one embodiment, the molar ratio of the component (a1) to the component (a2) [(component (a1)) / (component (a2))] is preferably about 10 / 90 to 90 / 10.
[0036] The upper limit of the ratio of the number of moles of isocyanate groups (NCO (a2)) of the component (a2) to the number of moles of hydroxyl groups (OH (a1)) of the component (a1) (NCO (a2) / OH (a1)) can be 2.00, 1.95, 1.90, 1.85, 1.80, 1.75, 1.70, 1.65, 1.60, 1.55, 1.50, 1.45, 1.40, 1.35, 1.30, 1.25, 1.20, 1.15, 1.10, 1.05, 1.00, 0.95, 0.90, 0. 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, etc., and the lower limit may be 1.95, 1.90, 1.85, 1.80, 1.75, 1.70, 1.65, 1.60, 1.55, 1.50, 1.45, 1.40, 1.35, 1.30, 1.25, 1.20, 1.15, 1.10, 1.05, 1.00, 0.95, 0.90, 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, 0.50, etc. The ratio (NCO(a2) / OH(a1)) of the number of moles of isocyanate groups (NCO(a2)) of the component (a2) to the number of moles of hydroxyl groups (OH(a1)) of the component (a1) is usually about 0.5 to 2.00.
[0037] <(a3) Component> (a3) component is a hydroxyl-containing mono (meth) acrylate and / or an isocyanate-containing mono (meth) acrylate. By using (a3) component, the active energy ray-curable adhesive composition has excellent curability and the adhesive layer is easy to be excellent in cutting. In the case of manufacturing an active energy ray-curable adhesive composition that does not contain (a3) component, poor curing will occur, and the adhesive layer will become too soft at room temperature. When cutting a substrate containing such an adhesive layer, the adhesive layer is easily attached to the surface of the blade (edge) of the cutting equipment, so the active energy ray-curable adhesive composition that does not contain (a3) component is not preferred. In the case of using a hydroxyl-containing multi (meth) acrylate having multiple (meth) acryloyl groups as a substitute for (a3) component, the adhesive layer becomes too hard and difficult to exert adhesion, so it is not preferred. In the case of using a hydroxyl-containing alcohol as (a part of) a substitute for (a3) component, the active energy ray-curable adhesive composition will be poorly cured, and the cutting property of the obtained adhesive layer will also deteriorate, so it is not preferred.
[0038] Examples of the hydroxyl-containing mono(meth)acrylate include one or more selected from 2-hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxybutyl(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, glycerol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl(meth)acrylate.
[0039] Examples of the isocyanate group-containing mono(meth)acrylate include one or more selected from 2-((meth)acryloyloxy)ethyl isocyanate and 2-(2-(meth)acryloyloxyethyloxy)ethyl isocyanate.
[0040] Since the active energy ray-curable adhesive composition has excellent curability and the adhesive layer is easy to cut, the component (a3) is preferably an isocyanate group-containing mono(meth)acrylate having 5 to 10 carbon atoms, and more preferably 2-((meth)acryloyloxy)ethyl isocyanate.
[0041] The upper limit of the molecular weight of the component (a3) may be 1000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, etc., and the lower limit may be 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, 25, etc. In one embodiment, the molecular weight of the component (a3) is preferably about 25 to 1000.
[0042] The upper limit of the carbon number of the component (a3) is 30, 25, 20, 15, 10, 5, etc., and the lower limit is 25, 20, 15, 10, 5, 1, etc. In one embodiment, the component (a3) preferably has about 1 to 30 carbon atoms.
[0043] In the total amount of 100 mass % of the components (a1), (a2) and (a3) of the present disclosure, as the upper limit of the content (solid content conversion) of the component (a3), 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 5 mass %, 1 mass %, 0.5 mass %, 0.1 mass %, etc. can be exemplified, and as the lower limit, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 5 mass %, 1 mass %, 0.5 mass %, 0.1 mass %, 0.05 mass %, etc. can be exemplified. In one embodiment, in order to well show the effect of the present disclosure, the content (solid content conversion) of the component (a3) in the total amount of 100 mass % of the components (a1), (a2) and (a3) of the present disclosure is preferably 0.05 mass % to 40 mass %.
[0044] In the total amount of 100 mol% of the components (a1), (a2) and (a3) of the present disclosure, as an upper limit of the content (in terms of solid content) of the component (a3), 20 mol%, 19 mol%, 18 mol%, 17 mol%, 16 mol%, 15 mol%, 14 mol%, 13 mol%, 12 mol%, 11 mol%, 10 mol%, 9 mol%, 8 mol%, 7 mol%, 6 mol%, 5 mol%, 4 mol%, 3 mol%, 2 mol% and the like can be exemplified, and as a lower limit, 19 mol%, 18 mol%, 17 mol%, 16 mol%, 15 mol%, 14 mol%, 13 mol%, 12 mol%, 11 mol%, 10 mol%, 9 mol%, 8 mol%, 7 mol%, 6 mol%, 5 mol%, 4 mol%, 3 mol%, 2 mol% and the like can be exemplified. In one embodiment, in order to demonstrate the effects of the present disclosure well, the content of component (a3) in the total amount of component (a1), component (a2) and component (a3) of the present disclosure is 1 mol% to 20 mol% (solid content conversion).
[0045] Examples of the upper limit of the content ratio of component (a1) to component (a3) (based on mass, calculated as solid content) [(component (a1)) / (component (a3))] include 99.9 / 0.1, 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, etc., and examples of the lower limit include 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, and 55 / 45, etc. In one embodiment, the content ratio (mass basis, solid content conversion) of component (a1) to component (a3) [(component (a1)) / (component (a3))] is preferably about 55 / 45 to 99.9 / 0.1, and more preferably about 80 / 20 to 95 / 5.
[0046] As the upper limit of the content ratio (mass basis, solid content conversion) of the component (a2) to the component (a3) [((a2) component) / ((a3) component)], 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, etc. can be exemplified, and as the lower limit, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, etc. can be exemplified. In one embodiment, the content ratio (mass basis, solid content conversion) of the component (a2) to the component (a3) [((a2) component) / ((a3) component)] is preferably about 55 / 45 to 99 / 1, and more preferably about 70 / 30 to 90 / 10.
[0047] The upper limit of the molar ratio of the component (a1) to the component (a3) [(component (a1)) / (component (a3))] may be 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, etc., and the lower limit may be 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, etc. In one embodiment, the molar ratio of the component (a1) to the component (a3) [(component (a1)) / (component (a3))] is preferably about 40 / 60 to 99 / 1.
[0048] The upper limit of the mol ratio of the component (a2) to the component (a3) [((a2) component) / ((a3) component)] may be 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, etc., and the lower limit may be 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, etc. In one embodiment, the mol ratio of the component (a2) to the component (a3) [((a2) component) / ((a3) component)] is preferably about 50 / 50 to 99 / 1.
[0049] <Other additives that can be blended with component (A)> The component (A) may contain various additives as necessary. Examples of the additives include catalysts, crystal nucleating agents, crystallization accelerators, chain transfer agents, and the like.
[0050] Regarding the method for producing component (A), various known methods for producing polyurethane can be used. Component (a1) and component (a2) can be reacted to temporarily produce a urethane prepolymer having one or more isocyanate groups or hydroxyl groups at the end (also referred to as "component (A')" in the present disclosure), and then component (A') is reacted with component (a3) to obtain component (A). The reaction temperature and reaction time are generally above 70°C and below 85°C, and above 1 hour and below 5 hours. When producing the above-mentioned polyurethane resin, one or more selected from components (c1) and (c2) of the present disclosure can be appropriately used as a diluent.
[0051] The upper limit of the weight average molecular weight of the component (A) may be 100000, 90000, 80000, 70000, 60000, 50000, 40000, 30000, 20000, 15000, 10000, etc., and the lower limit may be 90000, 80000, 70000, 60000, 50000, 40000, 30000, 20000, 15000, 10000, 5000, etc. In one embodiment, the weight average molecular weight of the component (A) is preferably 5000 to 100000, more preferably 15000 to 90000. If the weight average molecular weight of component (A) is lower than the above lower limit, the adhesive force of the adhesive layer tends to be weak; if it is greater than the above upper limit, the viscosity of the active energy ray-curable adhesive composition tends to be high and the production tends to be difficult. In the present disclosure, the weight average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography.
[0052] The upper limit of the (meth)acrylic acid equivalent of the component (A) is 1000 g / eq, 900 g / eq, 800 g / eq, 700 g / eq, 600 g / eq, 500 g / eq, 400 g / eq, 390 g / eq, 380 g / eq, 370 g / eq, 360 g / eq, 350 g / eq, 340 g / eq, 330 g / eq, 320 g / eq, 310 g / eq, 300 g / eq, 290 g / eq, 280 g / eq, 270 g / eq, 260 g / eq, 250 g / eq, 240 g / eq, 230 g / eq, 220 g / eq, 210 g / eq, 200 g / eq, 190 g / eq, 180 g / eq, 170 g / eq, g / eq, 190 g / eq, 180 g / eq, 170 g / eq, 160 g / eq, 150 g / eq, and the like can be exemplified as the lower limit. In one embodiment, the (meth)acrylic acid equivalent of component (A) is preferably about 150 g / eq to 1000 g / eq. If the (meth)acrylic acid equivalent of component (A) is too much, the adhesive force tends to be low, so it is preferably about below the above upper limit. In the present disclosure, the (meth)acrylic acid equivalent is expressed as the solid mass g of component (A) per (meth)acrylic acid group.
[0053] The upper limit of the content (solid content conversion) of the component (A) in the total amount of 100 mass% of the components (A), (B), and (C) of the present disclosure may be 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, etc., and the lower limit may be 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, etc. In one embodiment, the content (solid content conversion) of the component (A) in the total amount of 100 mass% of the components (A), (B), and (C) of the present disclosure may be 10 mass% to 40 mass%, preferably 15 mass% or more and 40 mass% or less, and more preferably 20 mass% or more and 30 mass% or less, from the perspective of excellent curability of the active energy ray-curable adhesive composition, excellent adhesion and conformability of the adhesive layer.
[0054] <(B) Component> Component (B) is a mono(meth)acrylate containing a primary hydroxyl group. By using component (B), the curability of the active energy ray-curable adhesive composition is excellent, and the durability of the adhesive layer after the moisture and heat resistance test is excellent. When a mono(meth)acrylate without a hydroxyl group or a mono(meth)acrylate containing a secondary hydroxyl group is used as a substitute for component (B), the durability of the adhesive layer after the moisture and heat resistance test is likely to deteriorate.
[0055] (B) Component may be one or more selected from 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate.
[0056] The component (B) is preferably 2-hydroxyethyl (meth)acrylate and / or 4-hydroxybutyl (meth)acrylate because the active energy ray-curable adhesive composition has excellent curability and the adhesive layer has excellent durability after a moisture and heat resistance test.
[0057] Examples of the upper limit of the content ratio of the component (A) to the component (B) (based on mass, in terms of solid content) [(component (A)) / (component (B))] include 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, and 20 / 80, and examples of the lower limit include 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85. In one embodiment, from the viewpoint that the adhesive layer easily shows excellent height difference conformability and durability after moisture and heat resistance test, the content ratio (mass basis, solid content conversion) of component (A) to component (B) [(component (A)) / (component (B))] is preferably about 15 / 85 to 85 / 15.
[0058] In the total amount of 100 mass% of the components (A), (B) and (C) of the present disclosure, as an upper limit of the content (converted to solid content) of the component (B), 35 mass%, 34 mass%, 33 mass%, 32 mass%, 31 mass%, 30 mass%, 29 mass%, 28 mass%, 27 mass%, 26 mass%, 25 mass%, 24 mass%, 23 mass%, 22 mass%, 21 mass% and the like can be exemplified, and as a lower limit, 34 mass%, 33 mass%, 32 mass%, 31 mass%, 30 mass%, 29 mass%, 28 mass%, 27 mass%, 26 mass%, 25 mass%, 24 mass%, 23 mass%, 22 mass%, 21 mass%, 20 mass% and the like can be exemplified. In one embodiment, from the viewpoint that the adhesive layer easily shows excellent height difference conformability and durability after moisture and heat resistance test, the content of component (B) in the total amount of 100 mass % of components (A), (B) and (C) disclosed in the present invention (converted into solid content) is greater than 20 mass % and less than 35 mass %, preferably greater than 25 mass % and less than 35 mass %, and more preferably greater than 30 mass % and less than 35 mass %.
[0059] <(C) Ingredients> The component (C) is a (meth)acrylate having no hydroxyl group. As the component (C), one or more selected from (c1) and (c2) can be exemplified, wherein (c1) is a (meth)acrylate having a glass transition temperature (also referred to as "Tg" in the present disclosure) lower than -5°C when forming a homopolymer, and (c2) is a (meth)acrylate having a glass transition temperature of -5°C or higher when forming a homopolymer. In addition, the "glass transition temperature when forming a homopolymer" adopts the value described in "Polymer Handbook" of Wiley-Interscience.
[0060] <(c1) ingredient> The component (c1) is a (meth)acrylate having a glass transition temperature of less than -5°C when it is a homopolymer. By using the component (c1), the adhesive layer is flexible and has good conformability to unevenness.
[0061] As the component (c1), there can be exemplified tetradecyl methacrylate (Tg: -72°C), 2-ethylhexyl acrylate (Tg: -70°C), ethoxydiethylene glycol acrylate (Tg: -70°C), isooctyl acrylate (Tg: -70°C), ethyl carbitol acrylate (Tg: -67°C), n-octyl acrylate (Tg: -65°C), lauryl methacrylate (Tg: -65°C), isononyl acrylate (Tg: -58°C), n-butyl acrylate (Tg: -56°C), 2-methoxyethyl acrylate (Tg: -50°C) ), isodecyl methacrylate (Tg: -41°C), nonyl acrylate (Tg: -37°C), 2-ethoxyethyl methacrylate (Tg: -31°C), isobutyl acrylate (Tg: -26°C), n-lauryl acrylate (Tg: -23°C), phenoxyethyl acrylate (Tg: -22°C), isooctadecyl acrylate (Tg: -18°C), 2-ethylhexyl methacrylate (Tg: -10°C), and one or more of (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate (Tg: -7°C).
[0062] The component (c1) is preferably 2-ethylhexyl acrylate because the adhesive layer has excellent flexibility and conformability to uneven heights.
[0063] The upper limit of the number of carbon atoms of the alkyl group of the component (c1) is 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, etc., and the lower limit is 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, etc. In one embodiment, the number of carbon atoms of the alkyl group of the component (c1) is preferably 4 or more and 18 or less.
[0064] In the total amount of 100 mass % of the components (A), (B) and (C) of the present disclosure, the upper limit of the content (converted to solid content) occupied by the component (c1) may be 40 mass %, 35 mass %, 30 mass %, 25 mass %, etc., and the lower limit may be 35 mass %, 30 mass %, 25 mass %, 20 mass %, etc. In one embodiment, from the viewpoint that the adhesive layer becomes soft and the conformability to the height difference is easy to be excellent, in the total amount of 100 mass % of the components (A), (B) and (C) of the present disclosure, the content (converted to solid content) occupied by the component (c1) is 20 mass % or more and 40 mass % or less, preferably 25 mass % or more and 40 mass % or less, and more preferably 30 mass % or more and 40 mass % or less.
[0065] <(c2) ingredient> The component (c2) is a (meth)acrylate having a glass transition temperature of -5°C or higher when forming a homopolymer. By using the component (c2), the storage elastic modulus of the adhesive layer is increased, and the cutting property is excellent.
[0066] Examples of the component (c2) include 2-methoxyethyl methacrylate (Tg: -2°C), (3-ethyloxetan-3-yl)methyl methacrylate (Tg: 2°C), benzyl acrylate (Tg: 6°C), methyl acrylate (Tg: 8°C), cyclohexyl acrylate (Tg: 15°C), diethylaminoethyl methacrylate (Tg: 16°C to 24°C), dimethylaminoethyl methacrylate (Tg: 18°C), n-butyl methacrylate (Tg: 20°C), cyclic trimethylolpropane formal acrylate (Tg: 27°C), n-octadecyl acrylate (Tg: 30°C), n-octadecyl methacrylate (Tg: 38°C), tert-butyl acrylate (Tg: 41°C), glycidyl methacrylate (Tg: 50°C), and n-butyl methacrylate (Tg: 51°C). Tg: 46°C), isobutyl methacrylate (Tg: 48°C), 3,3,5-trimethylcyclohexyl acrylate (Tg: 52°C), benzyl methacrylate (Tg: 54°C), tetrahydrofurfuryl methacrylate (Tg: 60°C), glycidyl acrylate (Tg: 60°C), ethyl methacrylate (Tg: 65°C), cyclohexyl methacrylate (Tg: 66°C), isobornyl acrylate (Tg: 97°C), methyl methacrylate (Tg: 105°C), tert-butyl methacrylate (Tg: 107°C), dicyclopentanyl acrylate (Tg: 120°C), 1-adamantane acrylate (Tg: 153°C), and 1-adamantane methacrylate (Tg: 250°C).
[0067] The component (c2) is preferably isobornyl acrylate because the storage elastic modulus of the adhesive layer is increased and the cutting property is easily excellent.
[0068] The upper limit of the number of carbon atoms of the alkyl group of the component (c2) may be 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, etc., and the lower limit may be 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, etc. In one embodiment, the number of carbon atoms of the alkyl group of the component (c2) is preferably 4 or more and 18 or less.
[0069] In the total amount of 100 mass % of the components (A), (B) and (C) of the present disclosure, the upper limit of the content (converted to solid content) occupied by the component (c2) may be 25 mass %, 20 mass %, 15 mass %, etc., and the lower limit may be 20 mass %, 15 mass %, 10 mass %, etc. In one embodiment, in order to increase the storage elastic modulus of the adhesive layer and facilitate the excellent cutting property, in the total amount of 100 mass % of the components (A), (B) and (C) of the present disclosure, the content (converted to solid content) occupied by the component (c2) is 10 mass % or more and 25 mass % or less, preferably 10 mass % or more and 20 mass % or less, and more preferably 10 mass % or more and 15 mass % or less.
[0070] (C) The upper limit of the molecular weight of the component may be 1000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, etc., and the lower limit may be 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, 25, etc. In one embodiment, the molecular weight of the component (C) is preferably about 25 to 1000.
[0071] The upper limit of the content ratio (mass basis, solid content conversion) of the component (c1) to the component (c2) [(component (c1)) / (component (c2))] can be 90 / 10, 85 / 15, 80 / 20, 75 / 15, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, etc., and as the lower limit, 85 / 15, 80 / 20, 75 / 15, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, 10 / 90, etc. In one embodiment, the content ratio (mass basis, solid content conversion) [((c1) component) / ((c2) component)] of the component (c1) to the component (c2) is preferably about 10 / 90 to 90 / 10, because the adhesive layer becomes soft, the height difference conformability is excellent, and the storage elastic modulus is also increased, and the cutting property is excellent.
[0072] Examples of the upper limit of the content ratio of the component (A) to the component (C) (based on mass, in terms of solid content) [(component (A)) / (component (C))] include 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85. Examples of the lower limit include 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, and 10 / 90. In one embodiment, from the viewpoint that the adhesive layer becomes soft and has excellent conformability to height differences, and the storage elastic modulus is also increased and the cutting property is excellent, the content ratio of component (A) to component (C) (mass basis, solid content conversion) [(component (A)) / (component (C))] is preferably about 10 / 90 to 70 / 30.
[0073] Examples of the upper limit of the content ratio of the component (B) to the component (C) (based on mass, in terms of solid content) [(component (B)) / (component (C))] include 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85. Examples of the lower limit include 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, and 10 / 90. In one embodiment, the content ratio of component (B) to component (C) (based on mass, solid content conversion) [(component (B)) / (component (C))] is preferably about 10 / 90 to 70 / 30, since the adhesive layer becomes soft and thus has excellent conformability to height differences, the storage elastic modulus also increases and thus has excellent cuttability, and the durability after a moisture and heat resistance test is excellent.
[0074] In the total amount of 100 mass % of the components (A), (B) and (C) of the present disclosure, as the upper limit of the content (solid content conversion) occupied by the component (C), 65 mass %, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, etc. can be exemplified, and as the lower limit, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, etc. can be exemplified. In one embodiment, in the total amount of 100 mass % of the components (A), (B) and (C) of the present disclosure, the content (solid content conversion) occupied by the component (C) is 30 mass % or more and 65 mass % or less, preferably 40 mass % to 60 mass %, and more preferably 50 mass % to 55 mass %, from the viewpoint that the adhesive layer becomes soft, the height difference conformability is easy to be excellent, and the storage elastic modulus is also increased, and the cutting property is easy to be excellent.
[0075] <(D) Component> The active energy ray-curable adhesive composition of the present disclosure preferably contains a radical photopolymerization initiator (also referred to as “component (D)” in the present disclosure) because the adhesive layer has excellent curability.
[0076] As the component (D), one or more selected from an alkylphenone type photopolymerization initiator, an acylphosphine oxide type photopolymerization initiator, a hydrogen abstraction type photopolymerization initiator, and an oxime ester type photopolymerization initiator can be exemplified.
[0077] As the alkylphenone type photopolymerization initiator, there can be illustrated: for example, benzyl dimethyl ketal such as 2,2-dimethoxy-1,2-diphenyl-1-ethanone; α-hydroxyalkylphenones such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propanone, 1-hydroxy-cyclohexyl-phenyl-ketone, and 2-hydroxy-2-methyl-1-phenyl-1-propanone; α-aminoalkylphenones such as 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, etc.
[0078] Examples of the acylphosphine oxide-based photopolymerization initiator include one or more selected from 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.
[0079] Examples of the hydrogen abstraction type photopolymerization initiator include methyl phenylglyoxylate and the like.
[0080] Examples of the oxime ester photopolymerization initiator include one or more selected from 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime) and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetoxime).
[0081] The component (D) is preferably an α-hydroxyalkylphenone type photopolymerization initiator and / or an acylphosphine oxide type photopolymerization initiator because the active energy ray-curable adhesive composition has excellent curability.
[0082] (D) component may be a commercially available product. Examples of such products include 2,2-dimethoxy-1,2-diphenyl-1-ethanone (product name: "OMNIRAD 651", manufactured by IGM Resins Co., Ltd.), 2-hydroxy-2-methyl-1-phenyl-1-propanone (product name: "H0991", manufactured by Tokyo Chemical Industry Co., Ltd.) (product name: "OMNIRAD 1173", manufactured by IGM Resins Co., Ltd.) (product name: "Lunacure 100", manufactured by DKSH·Japan Co., Ltd.), 1-hydroxycyclohexyl phenyl ketone (product name: "OMNIRAD 184", manufactured by IGM Resins Co., Ltd.) (product name: "Lunacure 200", manufactured by DKSH·Japan Co., Ltd.), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propanone (product name: "OMNIRAD 2959", manufactured by IGM Resins Co., Ltd.), 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone (product name: "OMNIRAD 907", manufactured by IGM Resins Co., Ltd.), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (product name: "OMNIRAD TPO", manufactured by IGM Resins Co., Ltd.), phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (product name: "OMNIRAD 819", manufactured by IGM Resins Co., Ltd.), methyl phenylglyoxylate (product name: "OMNIRAD MBF", manufactured by IGM Resins Co., Ltd.), 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyl oxime) (product name: "OMNIRAD OXE 01", manufactured by IGM Resins Co., Ltd.), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetoxime) (product name: "OMNIRAD OXE 02", manufactured by IGM Resins Co., Ltd.), and the like.
[0083] The upper limit of the content (in terms of solid content) of the component (D) relative to the total amount of 100 mass% of the component (A), the component (B), and the component (C) of the present disclosure may be 5 mass%, 4 mass%, 3 mass%, 2 mass%, 1.5 mass%, 1 mass%, 0.5 mass%, 0.2 mass%, etc., and the lower limit may be 4 mass%, 3 mass%, 2 mass%, 1.5 mass%, 1 mass%, 0.5 mass%, 0.2 mass%, 0.1 mass%, etc. In one embodiment, the content (in terms of solid content) of the component (D) relative to the total amount of 100 mass% of the component (A), the component (B), and the component (C) of the present disclosure is preferably 0.1 mass% or more and 5 mass% or less, more preferably 0.2 mass% or more and 2 mass% or less, and still more preferably 0.2 mass% or more and 1.5 mass% or less.
[0084] <Other additives that can be used> The active energy ray-curable adhesive composition of the present disclosure may contain various additives as necessary.
[0085] Examples of the additives include surface conditioners, surfactants, ultraviolet absorbers, antioxidants, light stabilizers, tackifiers, inorganic fillers, silane coupling agents, colloidal silica, defoamers, wetting agents, rust inhibitors, plasticizers, chain transfer agents, and photosensitizers.
[0086] The active energy ray-curable adhesive composition of the present disclosure may contain a solvent, and examples of the solvent include ketone solvents, aromatic solvents, alcohol solvents, glycol solvents, glycol ether solvents, ester solvents, petroleum solvents, alkyl halide solvents, and amide solvents.
[0087] Examples of the ketone solvent include methyl ethyl ketone, acetylacetone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone.
[0088] Examples of the aromatic solvent include toluene and xylene.
[0089] Examples of the alcohol solvent include methanol, ethanol, n-propanol, isopropanol, and butanol.
[0090] Examples of the glycol solvent include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, and polypropylene glycol.
[0091] Examples of the glycol ether solvent include ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol monoisobutyl ether, and ethylene glycol mono-tert-butyl ether.
[0092] Examples of the ester solvent include ethyl acetate, butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, and propylene glycol monomethyl ether acetate.
[0093] Examples of the petroleum-based solvent include product names such as "T-SOL 100" and "T-SOL 150" (each manufactured by ENEOS Corporation).
[0094] Examples of the alkyl halide solvent include chloroform and the like.
[0095] Examples of the amide solvent include dimethylformamide and the like.
[0096] The active energy ray-curable adhesive composition of the present disclosure may be used without containing a solvent. Therefore, from the viewpoint of being able to suppress costs and environmental impact, the active energy ray-curable adhesive composition of the present disclosure preferably does not contain a solvent.
[0097] From the perspective of excellent handling performance of the active energy ray-curable adhesive composition, the viscosity (mPa·s / 25°C) of the active energy ray-curable adhesive composition of the present disclosure is preferably 100 or more and 10000 or less, more preferably 300 or more and 8000 or less, and even more preferably 500 or more and 7000 or less. In the present disclosure, the viscosity is a value measured by an E-type viscometer (product name: "TVE-10", manufactured by Toki Sangyo Co., Ltd.) (5 minutes).
[0098] The active energy ray-curable adhesive composition disclosed herein is obtained by mixing component (A), component (B), component (C), and, if necessary, component (D) and other additives that can be mixed. The order of mixing is not particularly limited, and the components can be mixed sequentially or all at once.
[0099] <Cured product> An active energy ray-curable adhesive composition that is cured by irradiating it with active energy rays such as ultraviolet rays is also an aspect of the present invention.
[0100] When the active energy ray-curable adhesive composition contains a solvent, it is conceivable to perform a drying treatment before ultraviolet irradiation.
[0101] As the ultraviolet light source, an ultraviolet irradiation device having a xenon lamp, a high-pressure mercury lamp, or a metal halide lamp can be exemplified. In this device, the conditions such as the irradiation intensity, the accumulated light amount, and the conveying speed of the ultraviolet light are generally as follows: the irradiation intensity is 80 mW / cm 2 Above and 160mW / cm 2 The conveying speed is 3m / min or more and 50m / min or less, and the accumulated light intensity is 100mJ / cm 2 Above and 3000mJ / cm2 the following.
[0102] A cured product can be obtained by applying an active energy ray-curable adhesive composition to various plastic film substrates to form a layer of the active energy ray-curable adhesive composition, and then irradiating the layer with ultraviolet rays.
[0103] Examples of the coating method of the active energy ray-curable adhesive composition include bar coating, Mayer bar coating, air knife coating, gravure coating, reverse gravure coating, offset printing, flexographic printing, and screen printing.
[0104] The coating weight is usually 1g / m after drying. 2 Above and 1000g / m 2 The following range, preferably 3g / m 2 Above and 500g / m 2 The following range.
[0105] The thickness of the cured product of the present disclosure is preferably 10 μm to 1000 μm, more preferably 25 μm to 700 μm after drying, because the adhesive layer can easily exhibit conformability to height differences and is less likely to generate bubbles.
[0106] The upper limit of the storage elastic modulus G' (also referred to as "G'" in the present disclosure) of the cured product of the present disclosure at 20°C and 1 Hz can be 100×10 5 Pa, 90×10 5 Pa, 80×10 5 Pa, 70×10 5 Pa, 60×10 5 Pa, 50×10 5 Pa, 40×10 5 Pa, 30×10 5 Pa, 20×10 5 Pa, 10×10 5 Pa, 5×10 5 Pa, 4×10 5 Pa, 3×10 5 Pa, 2×10 5 Pa, 1.5×10 5 Pa, etc. As the lower limit, 90×10 5 Pa, 80×10 5 Pa, 70×10 5 Pa, 60×10 5 Pa, 50×10 5 Pa, 40×10 5 Pa, 30×10 5Pa, 20×10 5 Pa, 10×10 5 Pa, 5×10 5 Pa, 4×10 5 Pa, 3×10 5 Pa, 2×10 5 Pa, 1.5×10 5 Pa, 1×10 5 In one embodiment, the lower limit of the storage elastic modulus G' of the cured product of the present invention at 20°C and 1 Hz is preferably greater than 1×10 5 Pa, more preferably 1.5×10 5 In one embodiment, the upper limit of the storage elastic modulus G' of the cured product of the present invention at 20°C and 1 Hz is preferably 100×10 5 Pa or less, more preferably 90×10 5 Pa or less. In the present disclosure, the storage elastic modulus of the cured product is determined by the method described in JIS K7244-1:1998.
[0107] Specifically, regarding the storage elastic modulus, the dynamic viscoelasticity was measured under the following conditions using a commercially available measuring machine (product name: "MCR302", manufactured by Antenna Pal Co., Ltd.) Then, the storage elastic modulus G' at 20°C was determined from the measurement results.
[0108] Deformation method: twist Measuring frequency: 1Hz Deformation: 0.01%~1% automatic setting Heating rate: 3℃ / min Measuring temperature: 0℃~100℃ Shape: parallel plate 8.0mmφ
[0109] In the present disclosure, the storage elastic modulus (G') refers to a value proportional to the maximum energy accumulated through the load cycle, which indicates the rigidity of the adhesive layer. In addition, rigidity refers to the difficulty of deformation relative to external forces such as bending and torsion. The larger the value of the storage elastic modulus at 20°C and 1 Hz, the higher the rigidity of the adhesive layer at 20°C; the smaller the value, the lower the rigidity of the adhesive layer at 20°C. The preferred storage elastic modulus G' of the cured product of the present disclosure at 20°C and 1 Hz is greater than 1×10 5 Pa, the cured product of the present disclosure tends to have excellent cuttability at room temperature.
[0110] <Molded article> Examples of application of the active energy ray-curable adhesive composition include application between substrates of various known articles. These articles are not particularly limited, and may be various known articles.
[0111] Examples of such articles include: main bodies of household appliances such as refrigerators, televisions, and air conditioners, and their remote controls; housings and displays of information terminals such as mobile phones, smart phones, tablet computers, and computers; and plastic molded products such as automobile parts and automobile interior materials.
[0112] The active energy ray-curable adhesive composition disclosed herein is suitable for optical applications. For example, it can be applied to a display panel of a multilayer structure in a digital display device. In addition, the adhesive layer at room temperature is strong and tough, and it is not easy to cause the problem that the cut portion adheres to the punching blade and cannot be separated during punching, and the problem that the adhesive layer adheres to the punching blade, so it can be cut into various shapes. Starting from the excellent transparency, the adhesive layer disclosed herein is also suitable for use in displays such as televisions, smart phones or tablet computers.
[0113] <Applicable base materials> The active energy ray-curable adhesive composition of the present disclosure can be applied to various substrates.
[0114] Examples of the substrate include metal, plastic, glass, and other resins. Examples of the metal include iron, aluminum, aluminum-plated steel sheets, tin-free steel sheets (TFS), stainless steel sheets, zinc phosphate-treated steel sheets, and treated steel sheets of zinc-zinc alloy plated steel sheets (bond steel sheets). Examples of the plastic include thermoplastic plastic base materials and thermosetting plastic base materials. Examples of the thermoplastic plastic substrate include general-purpose plastic substrates and engineering plastic substrates. Examples of general-purpose plastic substrates include olefin-based, polyester-based, acrylic-based, vinyl-based, and polystyrene-based substrates. Examples of the olefin-based hydrocarbons include polyethylene, polypropylene, and norbornene. Examples of the polyester include polyethylene terephthalate (PET) and polyethylene naphthalate (PEN). Examples of acrylic acids include polymethyl methacrylate (PMMA) and the like. Examples of the vinyl-based polymer include polyvinyl chloride, polyvinylidene chloride, and polyvinyl alcohol. Examples of the polystyrene resin include polystyrene (PS) resin, styrene-acrylonitrile (AS) resin, and styrene-butadiene-acrylonitrile (ABS) resin. Examples of the engineering plastic substrate include general-purpose engineering plastics and super engineering plastics. Examples of general-purpose engineering plastics include polycarbonate and polyamide (nylon). Examples of super engineering plastics include polyetheretherketone (PEEK) and the like. Examples of the thermosetting plastic substrate include polyimide, epoxy resin, and melamine resin. As other plastic base materials, triacetyl cellulose resin and the like can be exemplified. The substrate disclosed in the present invention is preferably a thermoplastic plastic substrate, more preferably at least one selected from polyester, acrylic and general engineering plastics, and even more preferably polyester or acrylic and general engineering plastics.
[0115] The adhesive layer of the present disclosure is particularly preferably used for optical purposes due to its excellent transparency. That is, the adhesive layer of the present disclosure is particularly suitable for being attached to an optical substrate. The adhesive layer of the present disclosure is suitable for use as an optical transparent adhesive (also referred to as "OCA" in the present disclosure).
[0116] The optical substrate of the present disclosure is not particularly limited, and may be various known substrates. The optical substrate may be used alone or in combination of two or more.
[0117] Examples of optical substrates include polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate (PEN); plastic films such as polyethylene film, polypropylene film, cellophane, diacetyl cellulose film, triacetyl cellulose film, acetyl cellulose butyrate film, polyvinyl chloride film, polyvinylidene chloride film, polyvinyl alcohol film, ethylene-vinyl acetate copolymer film, polystyrene film, polycarbonate film, polymethylpentene film, polysulfone film, polyetheretherketone film, polyethersulfone film, polyetherimide film, polyimide film, fluororesin film, polyamide film, acrylic resin film, norbornene resin film, and cycloolefin resin film; and plastic films such as glass, tin-doped indium oxide film, ITO film, and transparent conductive film.
[0118] Specifically, examples of the combination of the adhesive layer and the optical substrate of the present disclosure include: (1) glass, an adhesive layer of the present disclosure, and a transparent conductive film (also referred to as "ITO" in the present disclosure); (2) a support film, an adhesive layer of the present disclosure, and ITO; (3) a support film, an adhesive layer of the present disclosure, and a liquid crystal display; (4) Glass, the adhesive layer of the present disclosure, a liquid crystal display, etc. Example
[0119] Hereinafter, the present disclosure will be further specifically described by listing manufacturing examples, comparative manufacturing examples, embodiments, comparative examples, evaluation examples, and comparative evaluation examples, but the present disclosure is not limited to the embodiments. In the following description, parts and % are based on mass.
[0120] In the present examples, the weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) under the following conditions. (GPC measurement conditions) Model: Product name: "HLC-8220GPC", manufactured by Tosoh Corporation Column: Product name "TSKgel G1000H", "TSKgel G2000H", manufactured by Tosoh Corporation Developing solvent: tetrahydrofuran Flow rate: 0.6mL / min Measurement temperature: 40℃ Detector: Refractive Index Detector (RI) Standard: Monodisperse polystyrene Sample: 20 μL of a solution prepared from a 1% tetrahydrofuran solution based on solid content of the resin and filtered through a microfilter
[0121] In each of the manufacturing examples, the NCO determination method of the urethane prepolymer is as follows: Measuring device: Potentiometric automatic titrator (product name "AT-700", manufactured by Kyoto Electronic Industries, Ltd.) Determination order: 1: Weigh about 0.500 g to 1.000 g of a sample in a weighing bottle. 2: Inject 10 mL of 0.15 mol / L dibutylamine toluene solution. 3: Place the weighing bottle containing the sample into the ultrasonic cleaner to completely dissolve the sample. 4: Make sure the sample is completely dissolved and leave it for 15 minutes (out of direct sunlight or heat). 5: After 15 minutes, add 100 mL of isopropanol to the weighing bottle. Place the stirring plate in the weighing bottle. 6: Titrate with 0.1 mol / L hydrochloric acid solution (f=1.00) to determine the NCO value. Input the sample volume to the automatic titrator and measure. If the measured difference is within 0.30, it is considered "OK". If it is greater than 0.30, measure again to confirm that it is within 0.30.
[0122] <Production Example 1: Production of Component (A)-1> 77.2 parts of polytetramethylene ether glycol having a number average molecular weight of 2000 (product name: "PTMG2000", manufactured by Mitsubishi Chemical Co., Ltd.) (hereinafter referred to as "PTMG2000") as the component (a1), 7.9 parts of isophorone diisocyanate (product name: "Isophorone Diisocyanate", manufactured by Tokyo Chemical Industry Co., Ltd.) (hereinafter referred to as "IPDI") as the component (a2), 14 parts of 2-ethylhexyl acrylate (product name: "2-Ethylhexyl Acrylate", manufactured by Mitsubishi Chemical Co., Ltd.) (hereinafter referred to as "2-EHA") and 0.1 part of tin octylate were added to a reaction container equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube and an air inlet, and reacted at 70°C for 2 hours to obtain a 2-EHA solution of a hydroxyl-terminated urethane prepolymer as an intermediate. 0.9 parts of 2-isocyanatoethyl methacrylate (product name: "Kalenzu MOI", manufactured by Lezonack Co., Ltd.) (also referred to as "MOI" in the present disclosure) as the component (a3) is mixed with the obtained reaction product, and the mixture is reacted at 70°C for 2 hours. The completion of the reaction is confirmed by NCO measurement, thereby obtaining a 2-EHA solution of the reaction product (also referred to as "component (A)-1" in the present disclosure).
[0123] <Manufacturing Examples 2 to 5 and Comparative Manufacturing Examples 1 to 2: Manufacturing of Components (A)-2 to (A)-5 and Components (A)-C1 to (A)-C2> The same procedure as in Production Example 1 was carried out except that the contents of the components were changed as shown in Table 1. Table 2 shows the molar amounts of the components.
[0124] [Table 1]
[0125] The numbers in Table 1 represent the mass parts of the component (a1), the component (a1'), the component (a2), and the component (a3) in the component (A). The terms in Table 1 have the following meanings. ': Indicates the symbol of the comparison component. PTMG2000: Polytetramethylene ether glycol (product name: "PTMG2000", manufactured by Mitsubishi Chemical Co., Ltd.) PPG2000: Polypropylene glycol (Product name: "Apoker P-2000, Apod type, 2,000", manufactured by Fujifilm Wako Pure Chemical Co., Ltd.) IPDI: Isophorone diisocyanate (product name: "Isophorone Diisocyanate", manufactured by Tokyo Chemical Industry Co., Ltd.) HDI: Hexamethylene diisocyanate (product name: "HDI", manufactured by Tosoh Corporation) MOI: 2-isocyanatoethyl methacrylate (product name: "Karens MOI", manufactured by Resonac Co., Ltd.) 4HBA: 4-Hydroxybutyl Acrylate (Product name: "4-Hydroxybutyl Acrylate", "4-Hydroxybutyl Acrylate", manufactured by Mitsubishi Micron Co., Ltd.) HEA: 2-Hydroxyethyl acrylate (product name "HEA", manufactured by Osaka Organic Chemical Industry Co., Ltd.)
[0126] [Table 2]
[0127] The numbers in Table 2 represent the molar amounts of the component (a1), the component (a1)′, the component (a2), and the component (a3) in the component (A).
[0128] <Example 1 to Example 14 and Comparative Example 1 to Comparative Example 12: Preparation of Active Energy Ray-Curing Adhesive Compositions (1) to (14) and Active Energy Ray-Curing Adhesive Compositions (C1) to (C12)> Active energy ray-curable adhesive compositions (1) to (14) and active energy ray-curable adhesive compositions (C1) to (C12) were obtained by mixing the components in the mass % shown in Tables 3 and 4.
[0129] <Evaluation Example 1-1: Preparation of Adhesive Sheet (1)> The active energy ray-curable adhesive composition (1) was applied to a 75 μm thick heavy release treated polyester film (product name: "SP-PET-03-75BU", manufactured by Mitsui Chemicals Toselo Co., Ltd.) so that the thickness of the adhesive layer after curing was 600 μm, and the release treated surface of a 38 μm thick light release treated polyester film (product name: "SP-PET-01-75BU", manufactured by Mitsui Chemicals Toselo Co., Ltd.) was attached to the coating layer of the active energy ray-curable adhesive composition. Then, the adhesive layer was heated in the atmosphere by a high pressure mercury lamp (100 mW / cm 2 , 900mJ / cm 2 ) The obtained coating film is irradiated with ultraviolet rays to prepare a laminated film (1) including an adhesive layer (light release treated polyester film / adhesive layer / heavy release treated polyester film). Then, the light release treated polyester film and the heavy release treated polyester film are peeled off to obtain a sheet (adhesive sheet (1)) consisting only of the adhesive layer (also referred to as "cured product" in the present disclosure).
[0130] <Evaluation Examples 1-2 to 1-14 and Comparative Evaluation Examples 1-1 to 1-12: Adhesive Sheets (2) to (14) and Adhesive Sheets (C1) to (C12)> The same method as in Evaluation Example 1-1 was used except that the active energy ray-curable adhesive composition (1) was changed to active energy ray-curable adhesive composition (2) to active energy ray-curable adhesive composition (14) and active energy ray-curable adhesive composition (C1) to active energy ray-curable adhesive composition (C12). In addition, the active energy ray-curable adhesive composition (C7) of Comparative Example 7 was not included in the following evaluation because it was not sufficiently cured.
[0131] <Evaluation Example 2-1: Preparation of Laminated Body (1)> A laminated film similar to the laminated film (1) of Evaluation Example 1-1 was prepared, and the lightly releasable polyester film was peeled off from the laminated film, and a 50 μm thick polyester film (product name: "Cosmosine A-4300", manufactured by Toyobo Co., Ltd.) was laminated with a 2 kg roller, and then allowed to stand for 2 hours. Then, a test piece of 8 cm × 8 cm was cut from the sample, and the heavily releasable polyester film was peeled off to prepare a single-sided adhesive sheet (Cosmosine A-4300 / adhesive layer). A laminate (Cosmoshire A-4300 (50 μm thick) / adhesive layer (600 μm thick) / glass plate (2 mm thick)) was prepared by overlapping a single-sided adhesive sheet (adhesive layer / Cosmoshire A-4300) (5 cm × 5 cm × 650 μm) on a glass plate (10 cm × 10 cm × 2 mm) and bonding them together with a 2 kg roller.
[0132] <Evaluation Examples 2-2 to 2-14 and Comparative Evaluation Examples 2-1 to 2-12: Laminates (2) to (14) and Laminates (C1) to (C12)> The same procedures as in Evaluation Example 2-1 were followed except that the laminated film (1) of Evaluation Example 1-1 was changed to the laminated films (2) to (14) of Evaluation Examples 1-2 to 1-14 and the laminated films (C1) to (C12) of Comparative Evaluation Examples 1-1 to 1-12, respectively.
[0133] <Performance Evaluation (1): Adhesion> The laminate (1) to laminate (14) and laminate (C1) to laminate (C12) were left to stand for 24 hours at 25°C and 50% humidity. The single-sided adhesive sheet (adhesive layer / Cosmoshine A-4300) was peeled off from the glass plate in a 180° direction at a speed of 300 mm / min, and the adhesion (N / 25 mm) was measured. The measurement was performed using a commercially available machine (product name: "Tensilon Universal Material Testing Machine", manufactured by (Strain) エー·アンド·デイ). If it is 5N / 25mm or more, it means that the adhesion is good, and the higher the value, the better.
[0134] <Performance evaluation (2): Storage elastic modulus (G')> Adhesive sheets (1) to (14) and adhesive sheets (C1) to (C12) were placed in a commercially available measuring machine (product name "MCR302", manufactured by Antenna Pal Co., Ltd.) and their dynamic viscoelasticity was measured under the following conditions. Then, the storage elastic modulus G' at 20°C and 1 Hz was calculated based on the measurement results. If it is greater than 1.0×10 5 Pa indicates that the storage elastic modulus is high. In addition, the storage elastic modulus of the cured product obtained from the active energy ray-curable adhesive composition of Comparative Example 2 is too high, so it becomes a cured product with poor height difference conformability described later, and the storage elastic modulus of the cured product obtained from the active energy ray-curable adhesive composition of Comparative Example 11 is too low, so it becomes a cured product with poor cutting properties. (Measurement conditions) Deformation method: twist Measuring frequency: 1Hz Deformation: 0.01%~1% automatic setting Heating rate: 3℃ / min Measuring temperature: 0℃~100℃ Shape: parallel plate 8.0mmφ
[0135] <Performance evaluation (3): Height difference conformity> A laminated film similar to the laminated film (1) of Evaluation Example 1-1 was prepared, and the lightly releasable polyester film was further peeled off and replaced with a 50 μm thick polyester film (product name: "Cosmosine A-4300", manufactured by Toyobo Co., Ltd.) was laminated with a 2 kg roller and allowed to stand for 2 hours. Then, a test piece of 8 cm × 8 cm was cut from the sample, and the heavily releasable polyester film was peeled off to prepare a single-sided adhesive sheet (Cosmosine A-4300 / adhesive layer). A polyester film sheet (5 cm × 5 cm × 50 μm) was overlapped on a glass plate (10 cm × 10 cm × 2 mm), and a single-sided adhesive sheet (adhesive layer / Cosmosine A-4300) (5 cm × 5 cm × 150 μm) was further overlapped thereon, and the layers were bonded with a 2 kg roller to prepare a laminate (Cosmosine A-4300 (50 μm thick) / adhesive layer (600 μm thick) / polyester film sheet (50 μm thick) / glass plate (2 mm thick)), and the laminate was evaluated at 20° C. The height difference conformability of the adhesive layer in this state was visually evaluated according to the following criteria. The laminated films (2) to (14) of Evaluation Examples 1-2 to 1-14 and the laminated films (C1) to (C12) of Comparative Evaluation Examples 1-1 to 1-12 were evaluated in the same manner. AA: No lifting was found along the sides of the polyester film, and no bubbles were confirmed. A: No floating was found along the sides of the polyester film, but up to 5 tiny bubbles were confirmed B: Wide floating is found along each side of the polyester film, and not only tiny bubbles but also multiple large bubbles can be confirmed.
[0136] <Performance evaluation (4): Chromaticity (b*)> Adhesive sheets (1) to (14) and adhesive sheets (C1) to (C12) were measured using a commercially available measuring machine (product name: "Spectrocolorimeter SE6000", manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS Z 8781-4:2013, and b* was calculated by the basic coordinate method.
[0137] <Performance evaluation (5): Durability (after moisture and heat resistance test)> After the laminates (1) to (14) and the laminates (C1) to (C12) were left to stand in a constant temperature and humidity chamber at a temperature of 85°C and a humidity of 85% for 500 hours, the durability of the adhesive layer was evaluated according to the following criteria. A: No peeling of the substrate, displacement of the adhesive layer, whitening of the adhesive layer, bubbles, or damage to the adhesive layer. B: At least one defect of peeling of the substrate, displacement of the adhesive layer, whitening of the adhesive layer, bubbles, and damage to the adhesive layer occurs.
[0138] <Performance evaluation (6): Durability (after light resistance test)> The laminates (1) to (14) and the laminates (C1) to (C12) are heated to 50 mW / cm 2 After being left to stand in an SUV (product name: "Ultra-accelerated light resistance tester meter", manufactured by Daiplan Instruments Co., Ltd.) for 100 hours, a commercially available measuring machine (product name: "Spectrocolorimeter SE6000", manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure according to JIS Z 8781-4:2013, and the change (Δb*) relative to the b* value before the test was calculated.
[0139] [Table 3]
[0140] [Table 4]
[0141] The meanings of the terms in Tables 3 and 4 are as follows. ※1: The usage amount (mass %) described in the table is a ratio when the total mass of component (A), component (B), and component (C) (component (c1) and component (c2)) is set to 100 mass %. In addition, the mass % of component (A) does not include the 2-EHA solution. The 2-EHA solution of component (A) is included in the mass % of 2-EHA of component (c1). *2: The usage-amount (mass %) of (D) component is a ratio when the total mass of (A) component, (B) component and (C) component is 100 mass %. *3: In the light resistance test, the adhesive sheet of the laminate was partially destroyed after being left to stand for 100 hours, so it could not be measured. 4HBA: 4-Hydroxybutyl acrylate (Product name: "4-HBA", manufactured by Osaka Organic Chemical Industry Co., Ltd.) HEA: 2-Hydroxyethyl acrylate (product name: "HEA", manufactured by Osaka Organic Chemical Industry Co., Ltd.) 2EHA: 2-Ethylhexyl acrylate (Product name: "2-Ethylhexyl acrylate", manufactured by Mitsubishi Micron Co., Ltd., Tg: -70°C) NOAA: n-octyl acrylate (product name: "NOAA", manufactured by Osaka Organic Chemical Industry Co., Ltd., Tg: -65°C) IBXA: Isobornyl acrylate (product name: "IBXA", manufactured by Osaka Organic Chemical Industry Co., Ltd., Tg: 97°C) FA-513AS: dicyclopentanyl acrylate (product name: "FA-513AS", manufactured by Lexonack Holdecone Co., Ltd., Tg: 120°C) L200: 1-hydroxycyclohexyl phenyl ketone (product name: "Lunacure 200", manufactured by DKSH Japan Co., Ltd.).
Claims
1. An active energy ray-curable adhesive composition, wherein: The composition contains: (A) polyurethane, which is a reaction product of (a1) a polyether polyol containing a linear aliphatic hydrocarbon group, (a2) a polyisocyanate, and (a3) a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate, (B) a mono(meth)acrylate containing a primary hydroxyl group, and (C) a mono(meth)acrylate having no hydroxyl group; The component (C) contains (c1) and / or (c2), wherein (c1) is a (meth)acrylate having a glass transition temperature of less than -5°C when forming a homopolymer, and (c2) is a (meth)acrylate having a glass transition temperature of -5°C or higher when forming a homopolymer; With respect to the total amount of component (a1), component (a2) and component (a3), which is 100 mol%, component (a1) is 35 mol% to 70 mol%, component (a2) is 25 mol% to 60 mol%, and component (a3) is 1 mol% to 20 mol%; Relative to 100% by mass (solid content conversion) of the total amount of component (A), component (B) and component (C), component (A) is 10% to 40% by mass, component (B) is 20% to 35% by mass, component (c1) is 20% to 40% by mass, and component (c2) is 10% to 25% by mass. 2 . A cured product, which is a cured product of the active energy ray-curable adhesive composition according to claim 1 . 3 . An adhesive sheet comprising the cured product according to claim 2 on at least one surface of a substrate.