H2 sensor and preparation method thereof
By optimizing the thickness of the SnO2 and palladium particle layer and the thickness of the polymer layer in the H2 sensor, combined with the transition layer and the conductive layer, the problem of insufficient sensitivity and selectivity of the H2 sensor at room temperature in the existing technology is solved, and high sensitivity is achieved And H2 detection with short response time ensures the safety and long life of the sensor.
Patent Information
- Application Number
- CN202310321983.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing H2 sensors to achieve high sensitivity and selectivity at room temperature, and due to the flammability and high diffusivity of H2, there are safety issues and high power consumption when the sensor works at high temperatures.
An H2 sensor structure composed of a substrate, a SnO2 layer, a palladium particle layer and a polymer layer is used. The electrode layer is spaced between the palladium particle layer and the polymer layer. By optimizing the thickness of the SnO2 and palladium particle layers and the thickness of the polymer layer , combined with the transition layer and the conductive layer, to improve the sensitivity and selectivity of the sensor.
Highly sensitive detection of H2 at room temperature is achieved, with short response time and recovery time, good selectivity, and the sensor has a long service life.
Smart Images

Figure CN118731008A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an H2 sensor and its preparation method, belonging to the field of gas detection technology. Background Technology
[0002] To address climate change, energy systems are transitioning to technologies that reduce greenhouse gas emissions. H2 is a promising renewable and clean energy carrier because its combustion produces only H2O, exhibiting eco-friendly combustion characteristics. This has led to an increase in global demand for H2. H2 has been used as a feedstock in various industrial applications, including oil refineries, ammonia and methanol production, aerospace, and as fuel for fuel cells. However, H2 is a flammable and explosive gas with a low ignition energy (~0.017 mJ) and a wide concentration range in air (4%–75%). Furthermore, it is colorless and odorless. Therefore, to enable early leak detection and monitoring of H2 during production, transportation, storage, and end-use, and to mitigate the risks associated with its use in practical applications, it is crucial to develop highly sensitive, selective, and room-temperature-operable H2 sensors with long-term stability.
[0003] Semiconductor metal oxides (SMOs), such as tin oxide (SnO2), have been widely used for detecting various gases, including NO2, CO2, CO, H2S, VOCs, and H2, due to their excellent thermal stability, high chemical resistance, and low cost. Currently, various SnO2 structures are used as gas sensors, such as nanofibers, thin and thick films, nanoparticles, nanowires, sintered powders, and nanosheets. Thin-film nanostructures have been the most extensively studied in gas sensing due to their simple design and fabrication processes. Nanostructured SnO2 films can be prepared using sputtering, chemical vapor deposition, thermal evaporation, atomic layer deposition (ALD), and sol-gel methods. Regardless of the fabrication method, most sensors operate at high temperatures of 200–550 °C to achieve acceptable sensitivity and stability. However, due to the flammability and high diffusivity of H2, high-temperature operation leads to high power consumption, low selectivity, and safety issues. Furthermore, it is difficult to develop flexible SMO-based gas sensors because the normal operation of tin oxide films typically requires a high-temperature environment. Furthermore, the current sensor is installed at a considerable distance from the H2 leak point, which may cause a significant difference between the measured H2 concentration and the actual H2 concentration due to the highly diffusive nature of H2.
[0004] Different strategies have been developed to address these issues, achieve low-temperature operation, and improve sensitivity and selectivity; for example, decorating the SMO surface with noble metals (e.g., Pd, Pt, Au, and Rh), reducing film thickness to the nanoscale to modulate the film's electron mobility, and using separation films as selective layers. Noble metals enhance sensor sensitivity through chemisensitization to improve gas adsorption and desorption processes, and alter the position of the Fermi level through electronic sensitization. Another approach to improving sensor sensitivity is to make the SMO film thickness approach the Debye length (LD) to increase the surface-to-volume ratio and effectively modulate conductivity. At 250 °C, the LD of SnO2 is approximately 3 nm. When the film thickness is less than or equal to 6 nm, the SMO film ideally depletes all electrons, making it extremely sensitive to environmental changes. For example, Du et al. (X. Du and S.M. George, Thickness dependence of sensor response for CO gas sensing by tin oxide films grown using atomic layer deposition) used ALD to investigate the effect of SnO2 film thickness on the CO gas sensor response at 300 °C. The results show that the highest sensitivity to CO is achieved when the film thickness is 3 nm. Furthermore, Cai et al. (Z. Cai and S. Park, Synthesis of Pd nanoparticle-decorated SnO2 nanowires and determination of the optimum quantity of Pd nanoparticles for highly sensitive and selective hydrogen gas sensor) demonstrated that optimal palladium catalyst modification on SnO2 nanowires significantly improves the sensitivity at 300 °C. The gas-sensing properties of Pd-modified SnO2 films have been extensively studied. However, even after palladium modification, it is difficult to achieve excellent sensitivity at room temperature due to the lack of modulation in the depletion layer caused by large film thickness. Moreover, the effect of Pd content on the H2 sensing response of ultrathin SnO2 films with thicknesses on the order of LD is currently lacking investigation. Summary of the Invention
[0005] The purpose of this invention is to provide an H2 sensor with high sensitivity and good selectivity.
[0006] Another object of the present invention is to provide a method for preparing an H2 sensor.
[0007] To achieve the above objectives, the technical solution adopted by the H2 sensor of this invention is as follows:
[0008] An H2 sensor includes a substrate, a SnO2 layer, a palladium particle layer, and a polymer layer sequentially bonded together; the polymer layer is a polymethyl methacrylate layer.
[0009] The H2 sensor further includes an electrode layer; the electrode layer is spaced between the palladium particle layer and the polymer layer; or the electrode layer is spaced between the SnO2 layer and the polymer layer, and the palladium particle layer is located between the spaced electrode layers.
[0010] The H2 sensor of the present invention comprises a substrate, a SnO2 layer, a palladium particle layer and a polymer layer sequentially bonded together. When detecting H2 at room temperature, it has good selectivity, high sensitivity (response value up to 16600), short response time and recovery time (response time as low as 6s, recovery time as low as 5s) and long service life.
[0011] Preferably, the thickness of the SnO2 layer is 3 nm and the thickness of the palladium particle layer is 4 nm; or the thickness of the SnO2 layer is 5 nm and the thickness of the palladium particle layer is 2 nm; or the thickness of the SnO2 layer is 8 nm and the thickness of the palladium particle layer is 2 nm; or the thickness of the SnO2 layer is 11 nm and the thickness of the palladium particle layer is 3 nm.
[0012] Based on the applicant's extensive experimental research, due to the small thickness of the palladium particle layer, the performance of the H2 sensor obtained by spacing the electrode layer between the palladium particle layer and the polymer layer is close to that of the H2 sensor obtained by spacing the electrode layer between the SnO2 layer and the polymer layer.
[0013] Preferably, the weight-average molecular weight of the polymethyl methacrylate in the polymethyl methacrylate layer is 250,000 to 350,000.
[0014] Preferably, the thickness of the polymer layer is 50–70 nm. If the polymer layer is too thin, the hydrogen sensor will have poor selectivity in detecting hydrogen; if the thickness is too large, it will cause excessive gas selectivity and lead to reaction lag.
[0015] To improve the adhesion of the electrode layer to the palladium particle layer or the SnO2 layer, preferably, the electrode layer includes a transition layer and a conductive layer, wherein the transition layer is a Ti layer or a Cr layer; the electrode layer is spaced between the palladium particle layer and the polymer layer, and the electrode layer is disposed on the palladium particle layer through the transition layer; or the electrode layer is spaced between the SnO2 layer and the polymer layer, and the electrode layer is disposed on the SnO2 layer through the transition layer.
[0016] Preferably, the thickness of the transition layer is 2–3 nm. If the thickness of the transition layer is too small, it will cause the effect of improving the adhesion of the electrode layer to the palladium particle layer or SnO2 layer to fail.
[0017] Preferably, the thickness of the conductive layer is 5–10 nm. If the thickness of the conductive layer is too small, the conductivity will be poor; if the thickness is too large, the polymer layer will not be able to effectively encapsulate the electrode layer, resulting in poor selectivity of the hydrogen sensor in detecting hydrogen.
[0018] It is understood that the conductive layer is made of a conductive metal, and preferably, the conductive layer is an Au layer.
[0019] In this invention, when the electrode layer is spaced between the palladium particle layer and the polymer layer, the thickness of the polymer layer refers to the distance between the side of the polymer layer that is attached to the gas-chromic layer and the other side of the polymer layer (the side of the polymer layer that is attached to the palladium particle layer); when the electrode layer is spaced between the SnO2 layer and the polymer layer, and the palladium particle layer is located between the spaced electrode layers, the thickness of the polymer layer refers to the distance between the side of the polymer layer that is attached to the gas-chromic layer and the other side of the polymer layer (the side of the polymer layer that is attached to the palladium particle layer).
[0020] The technical solution adopted in the preparation method of the H2 sensor of the present invention is as follows:
[0021] The method for preparing the H2 sensor as described above includes the following steps: coating a SnO2 precursor solution onto a substrate, drying it to form a SnO2 layer, depositing a palladium particle layer on the SnO2 layer, depositing an electrode layer on the palladium particle layer at intervals, coating the electrode layer and the palladium particle layer with a polymer solution, and drying it to form a polymer layer.
[0022] Alternatively, a SnO2 precursor solution can be coated onto a substrate, dried to form a SnO2 layer, and then a palladium particle layer and an electrode layer can be deposited on the SnO2 layer to form an electrode layer with the palladium particle layer located between the electrode layers. Then, a polymer solution can be coated onto the palladium particle layer and the electrode layer, and dried to form a polymer layer.
[0023] The method for preparing the H2 sensor of the present invention is simple to operate and provides an effective way to develop robust, flexible, transparent and durable H2 sensors.
[0024] Preferably, the SnO2 precursor solution is prepared by a method comprising the following steps: mixing 2-methoxyethanol and stannous chloride dihydrate until stannous chloride dihydrate is completely dissolved, followed by solid-liquid separation to obtain the SnO2 precursor solution.
[0025] Preferably, the SnO2 precursor solution is coated using spin coating at a rotation speed of 1500–3000 rpm. For example, the SnO2 precursor solution is coated using spin coating at a rotation speed of 3000 rpm.
[0026] Preferably, a palladium particle layer is deposited on the SnO2 layer using a thermal evaporation deposition method, with a deposition rate of [missing information].
[0027] Preferably, the polymethyl methacrylate solution is an anisole solution of polymethyl methacrylate. Preferably, the weight-average molecular weight of the polymethyl methacrylate is 250,000 to 350,000.
[0028] Preferably, the concentration of the polymethyl methacrylate solution is 35–50 mg / mL. For example, the concentration of the polymethyl methacrylate solution is 40 mg / mL.
[0029] Preferably, the polymer solution is coated by spin coating, wherein the spin coating speed is 3000-4000 rpm.
[0030] Preferably, the drying temperature after coating with the polymer solution does not exceed 175°C. Attached Figure Description
[0031] Figure 1 This is a schematic diagram showing the thickness test results of SnO2 thin films prepared from SnO2 precursor sols of different concentrations by X-ray reflection.
[0032] Figure 2 This is a schematic diagram showing the results of characterizing the surface morphology of an 11 nm thick SnO2 thin film; where, Figure 2 a is the SEM image. Figure 2 b is the AFM diagram. Figure 2 c is the surface roughness analysis diagram;
[0033] Figure 3 A schematic diagram showing a high-resolution transmission electron microscope (HR-TEM) cross-sectional image of the Pd nanoparticle layer and the results of elemental composition analysis;
[0034] Figure 4 This is a schematic diagram illustrating the dynamic response of sensors with SnO2 films and palladium nanoparticles of different thicknesses in Experiment Example 3 at room temperature, with an air hydrogen content of 2%, and a bias voltage of 0.1V; where, Figure 4 a is a schematic diagram showing the dynamic response of sensors with SnO2 thin films of 3 nm thickness and palladium nanoparticles of different thicknesses. Figure 4 b is a schematic diagram showing the dynamic response of sensors with SnO2 thin films of 8 nm thickness and palladium nanoparticles of different thicknesses. Figure 4 c is a schematic diagram showing the dynamic response of sensors with SnO2 thin films of 11 nm thickness and palladium nanoparticles of different thicknesses. Figure 4 d represents the dynamic response of sensors with SnO2 thin films of 5 nm thickness and palladium nanoparticles of different thicknesses.
[0035] Figure 5 This is a schematic diagram showing the initial resistance test results of sensors with SnO2 films and Pd particle layers of different thicknesses in Experiment Example 3; where, Figure 5 a is a schematic diagram showing the initial resistance of sensors with SnO2 thin films of 3 nm thickness and palladium nanoparticles of different thicknesses. Figure 5 b is a schematic diagram showing the initial resistance of sensors with SnO2 thin films of 5 nm thickness and palladium nanoparticles of different thicknesses. Figure 5 c represents a schematic diagram of the initial resistance of sensors with SnO2 thin films of 8 nm thickness and palladium nanoparticles of different thicknesses. Figure 5 d is a schematic diagram of the initial resistance of sensors with SnO2 thin films of 11 nm thickness and palladium nanoparticles of different thicknesses.
[0036] Figure 6 These are TEM images of palladium nanoparticles with thicknesses of 1 nm, 3 nm, 5 nm, and 10 nm in Experiment Example 3; among them, Figure 6 a is a TEM image of a 1nm thick palladium nanoparticle layer when the SnO2 film thickness is 3nm. Figure 6 b is a TEM image showing the palladium nanoparticle layer with a thickness of 3 nm when the SnO2 film thickness is 3 nm. Figure 6 c is a TEM image showing the palladium nanoparticle layer with a thickness of 5 nm when the SnO2 film thickness is 3 nm. Figure 6 Image d shows a TEM image of a 10nm thick palladium nanoparticle layer when the SnO2 film thickness is 3nm. Figure 6 e is an HRTEM image of the palladium nanoparticle layer with a thickness of 3 nm when the thickness of the SnO2 film is 3 nm.
[0037] Figure 7 This is a schematic diagram showing the results of a sensor with a SnO2 film thickness of 3 nm and palladium nanoparticle thickness of 4 nm detecting hydrogen gas with a content of 20 ppm to 2% in the air, as described in Experiment Example 4.
[0038] Figure 8 This is a schematic diagram showing the results of a sensor with an 8 nm thick SnO2 film and a 2 nm thick palladium nanoparticle in Experiment Example 4 detecting hydrogen gas with a concentration of 20 ppm to 2% in the air.
[0039] Figure 9This is a schematic diagram showing the results of a sensor with a SnO2 film thickness of 11 nm and palladium nanoparticle thickness of 3 nm in Experiment Example 4 detecting hydrogen gas with a content of 20 ppm to 2% in the air.
[0040] Figure 10 This is a schematic diagram showing the results of a sensor with a SnO2 film thickness of 5 nm and palladium nanoparticle thickness of 2 nm in Experiment Example 4 detecting hydrogen gas with a content of 20 ppm to 2% in the air.
[0041] Figure 11 This is a schematic diagram showing the results of repeatability testing, response time and recovery time testing, selectivity and cross-selectivity testing, and long-term stability testing using a sensor with a SnO2 film thickness of 5 nm and Pd nanoparticle thickness of 2 nm in Experiment Example 4.
[0042] Figure 12 The diagram shows the response of the H2 sensor with a SnO2 film thickness of 100 nm in Experiment Example 4 to H2 concentrations of 0.01%, 0.05%, and 0.1% in the air at different temperatures (20–120 °C), as well as the transient response at room temperature.
[0043] Figure 13 This is a schematic diagram showing the detection results of the sensor used in Experiment Example 5 to detect H2 in air with different relative humidity and at different temperatures at room temperature.
[0044] Figure 14 This is a schematic diagram of the XPS spectral test results of SnO2 and Pd-SnO2 in Experimental Example 6;
[0045] Figure 15 This is a schematic diagram of the appearance of the flexible sensor in Experiment Example 7, as well as a schematic diagram of the results of repeatability testing, response time and recovery time testing, selectivity and cross-selectivity testing, and long-term stability testing using the flexible sensor. Detailed Implementation
[0046] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0047] The raw materials used in Examples 3-4 are as follows: tin chloride dihydrate (II) (>99.999%), PMMA (average molar weight 350,000), and anisole purchased from Sigma Aldrich; 2-methoxyethanol (2ME) purchased from Samchun Chemical; and transparent polyimide (PI) varnish purchased from Fafnie Korea. All chemicals were not further purified.
[0048] I. An embodiment of the H2 sensor of the present invention is as follows:
[0049] Example 1
[0050] The H2 sensor of this embodiment includes a substrate, a SnO2 layer, a palladium particle layer and a polymer layer that are sequentially bonded together; the polymer layer is a polymethyl methacrylate (PMMA) layer. The H2 sensor also includes an electrode layer, which is disposed between the palladium particle layer and the polymer layer. The electrode layer includes a transition layer and a conductive layer. The conductive layer is an Au layer and the transition layer is a Cr layer. The electrode layer is disposed on the palladium particle layer through the transition layer.
[0051] In this embodiment of the H2 sensor, the substrate is a silicon wafer with a thermally grown SiO2 thin film on its surface. The thickness of the silicon wafer is 1 mm, the thickness of the thermally grown SiO2 thin film is 300 nm, a SnO2 layer is disposed on the SiO2 thin film with a thickness of 5 nm, a palladium particle layer with a thickness of 2 nm, a transition layer with a thickness of 2 nm, a polymer layer with a thickness of 30 nm, and a conductive layer with a thickness of 10 nm. In this embodiment, the thickness of the polymer layer refers to the distance between the side of the polymer layer that is attached to the palladium particle layer and the side of the polymer layer that is away from the palladium particle layer.
[0052] Example 2
[0053] The only difference between the H2 sensor in this embodiment and the H2 sensor in Embodiment 1 is that the substrate of the H2 sensor in this embodiment is a polyimide film with a thickness of 800 nm.
[0054] II. An embodiment of the method for preparing the H2 sensor of the present invention is as follows:
[0055] Example 3
[0056] The method for preparing the H2 sensor in this embodiment is the same as the method for preparing the H2 sensor in Example 1, and specifically includes the following steps:
[0057] (1) Preparation of SnO2 precursor solution: Mix 2-methoxyethanol and stannous chloride dihydrate until stannous chloride dihydrate is completely dissolved, and then filter it with a 0.2μm polytetrafluoroethylene injection filter to obtain a stannous chloride dihydrate solution with a concentration of 0.05mol / L, which is the SnO2 precursor solution.
[0058] Preparation of PMMA solution: PMMA with a weight average molecular weight of 350,000 was added to anisole and stirred at 60°C for 6 hours to obtain a PMMA solution with a concentration of 40 mg / mL.
[0059] (2) Fabrication of the H2 sensor: The substrate (a silicon wafer with a thermally grown SiO2 film on its surface, wherein the thickness of the silicon wafer is 1 mm and the thickness of the thermally grown SiO2 film is 300 nm) was sequentially cleaned with deionized water, acetone, and isopropanol, and then cleaned with UV / ozone. A SnO2 precursor solution was spin-coated onto the SiO2 film on the cleaned substrate at a speed of 3000 rpm for 60 s. The substrate coated with the SnO2 precursor solution was then pre-baked at 100°C for 5 min, and then placed directly on a hot plate to heat the substrate in air at 400°C for 1 h to form a SnO2 film on the SiO2 film. Then, a thermal evaporation method was used on the SnO2 film to... Palladium particle catalysts were deposited at a rate of [missing information - likely a specific velocity or speed], and then electrode layers were deposited on the palladium particle layers using a thermal evaporation method. The electrode layers were spaced apart on the palladium particle layers, and each electrode layer consisted of a 2 nm thick Cr layer and a 10 nm thick Au layer. The Cr layer served as a transition layer to improve the adhesion of the Au layer to the palladium particle catalyst layer, and the Au layer served as a conductive layer, acting as both the source and drain electrodes. Finally, PMMA solution was spin-coated on both the electrode layers and the uncoated palladium particle catalyst layer at a speed of 4000 rpm for 30 s, and then baked at 175 °C for 10 min to form a polymer layer.
[0060] Example 4
[0061] The method for preparing the H2 sensor in this embodiment is the same as the method for preparing the H2 sensor in Example 3, and specifically includes the following steps:
[0062] (1) This step is the same as step (1) of the preparation method of the H2 sensor in Example 3;
[0063] (2) The substrate (a silicon wafer with a thermally grown SiO2 film on its surface, wherein the thickness of the silicon wafer is 1 mm and the thickness of the thermally grown SiO2 film is 300 nm) was sequentially cleaned with deionized water, acetone, and isopropanol, and then cleaned with UV / ozone. A transparent polyimide (PI) varnish was then spin-coated onto the SiO2 film of the cleaned substrate at a speed of 1000 rpm for 30 seconds. The substrate coated with the transparent polyimide (PI) varnish was then annealed at a heating rate of 2 °C / min to a certain temperature to form a PI layer on the SiO2 film. To avoid… The PI film exhibited wrinkling, so a staged annealing treatment was adopted. First, the substrate coated with transparent polyimide (PI) varnish was heated to 60°C and held for 30 minutes, then heated to 80°C and held for 30 minutes, then heated to 150°C and held for 30 minutes, then heated to 230°C and held for 60 minutes, and finally heated to 300°C and cooled to room temperature. Then, a SnO2 precursor solution was spin-coated onto the PI layer at 3000 rpm for 60 seconds. The substrate was then heated at 280°C for 4 hours to form a SnO2 film on the PI layer. Finally, thermal evaporation was used on the SnO2 film to... Palladium particle catalysts were deposited at a high rate, and then electrode layers were deposited on the palladium particle layers using thermal evaporation. The electrode layers were spaced apart on the palladium particle layers. The electrode layers included a 2 nm thick Cr layer and a 10 nm thick Au layer. The Cr layer served as a transition layer to improve the adhesion of the Au layer to the palladium particle catalyst layer. The Au layer served as a conductive layer, acting as the source and drain. Then, PMMA solution was spin-coated on the electrode layers and the palladium particle catalyst layer without electrode layers at a speed of 4000 rpm for 30 s. The coating was then baked at 175 °C for 10 min to form a polymer layer on the electrode layers and palladium particle catalyst layers. Finally, the PI layer was separated from the substrate to obtain a transparent flexible H2 sensor.
[0064] Comparative Example 1
[0065] The only difference between the preparation method of the H2 sensor in this comparative example and the preparation method of the H2 sensor in Example 3 is that the molecular weight of the PMMA used in the preparation of the PMMA solution in this comparative example is 200,000, and the thickness of the PMMA layer in the H2 sensor prepared by this comparative example is the same as the thickness of the polymer layer in the H2 sensor prepared by the preparation method of the H2 sensor in Example 2.
[0066] Comparative Example 2
[0067] The only difference between the preparation method of the H2 sensor in this comparative example and the preparation method of the H2 sensor in Example 3 is that the molecular weight of the PMMA used in the preparation of the PMMA solution in this comparative example is 400,000, and the thickness of the PMMA layer in the H2 sensor prepared by this comparative example is the same as the thickness of the polymer layer in the H2 sensor prepared by the preparation method of the H2 sensor in Example 2.
[0068] Comparative Example 3
[0069] The only difference between the preparation method of the H2 sensor in this comparative example and the preparation method of the H2 sensor in Example 3 is that the concentration of the PMMA solution in the preparation method of the H2 sensor in this comparative example is 30 mg / mL, and the thickness of the PMMA layer in the H2 sensor prepared by the preparation method of this comparative example is the same as the thickness of the polymer layer in the H2 sensor prepared by the preparation method of the H2 sensor in Example 2.
[0070] Comparative Example 4
[0071] The only difference between the preparation method of the H2 sensor in this comparative example and the preparation method of the H2 sensor in Example 3 is that the concentration of the PMMA solution in the preparation method of the H2 sensor in this comparative example is 55 mg / mL, and the thickness of the PMMA layer in the H2 sensor prepared by the preparation method of this comparative example is the same as the thickness of the polymer layer in the H2 sensor prepared by the preparation method of the H2 sensor in Example 2.
[0072] The instruments and methods used to test the sensing performance of the H2 sensor in the following experimental examples are as follows: An Agilent B15000A semiconductor parameter analyzer and an MSTECH probe station with ELFLOW high-performance MFC were used to measure the current-voltage characteristics and gas sensing response. The sensor was placed in a gas test chamber below the gas tube outlet, directly exposed to air containing a certain concentration of hydrogen. The sensor response was defined as I... g / I a , where I g and I a These represent the measured change in current (i.e., the change in current after exposure to air containing a certain concentration of hydrogen) and the initial current, respectively. For all measurements, the applied voltage and temperature were 100 mV and 20 °C, respectively.
[0073] Experimental Example 1
[0074] The performance and operating temperature of SMO-based sensors are strongly dependent on the film thickness and morphology, especially when the film thickness is on the nanometer scale, where the thickness and morphology have a greater impact on the performance of SMO-based sensors. To optimize the thickness of SnO2 films, SnO2 films with thicknesses ranging from 3 to 11 nm were prepared by varying the concentration of the SnO2 precursor solution. The thickness of SnO2 films prepared with different concentrations of SnO2 precursor solution was investigated using X-ray reflection, and the results are as follows: Figure 1 As shown, the root mean square roughness of SnO2 films with thicknesses of 3–11 nm was analyzed using both AFM and X-ray reflectance methods. Finally, the thickness and roughness of SnO2 films prepared from SnO2 precursor solutions of different concentrations were summarized and listed in Table 1.
[0075] Table 1. Thickness and root mean square roughness of SnO2 films prepared from SnO2 precursor solutions of different concentrations.
[0076] <![CDATA[Concentration of SnO2 precursor solution]]> <![CDATA[Thickness of SnO2 thin film]]> <![CDATA[Root mean square roughness of SnO2 thin film]]> 0.025mol / L 3nm 0.657nm 0.05 mol / L 5nm 0.560nm 0.075 mol / L 8nm 0.718nm 0.1 mol / L 11nm 0.885nm
[0077] Table 1 shows that the thickness of the SnO2 film increases proportionally with the concentration of the SnO2 precursor solution. The prepared SnO2 film thickness covers the Debye length of SnO2 (3 nm at 250 °C) to obtain a complete film that is fully electron-depleted and extremely sensitive to environmental changes. When the thickness of the SnO2 film increases from 3 nm to 11 nm, the root mean square roughness of the SnO2 film increases from 0.657 nm to 0.885 nm.
[0078] Experiment Example 2
[0079] The surface morphology of an 11 nm thick SnO2 film was investigated using high-resolution scanning electron microscopy (SEM) and atomic force microscopy (AFM). The results are as follows: Figure 2 As shown, where, Figure 2 a is the SEM image. Figure 2 b is the AFM diagram. Figure 2 c is the surface roughness analysis diagram (i.e., a schematic diagram of surface roughness tested under AFM).
[0080] from Figure 2 As can be seen, the SnO2 film exhibits uniform grain size and distribution, with good inter-grain connectivity. The high quality of the film is mainly attributed to the use of a suitable solvent for precursor preparation, an optimized preparation process, and a relatively low heating temperature for film formation.
[0081] Meanwhile, the 3 nm thick palladium nanoparticle layer on the SnO2 film was characterized using high-resolution transmission electron microscopy (HR-TEM). The HR-TEM cross-sectional image of the palladium nanoparticle layer is shown below. Figure 3 As shown in a and 3b, the crystal planes with lattice spacing values of 0.26 nm and 0.33 nm correspond to the (101) and (110) crystal planes of SnO2, respectively, and the crystal plane with a lattice spacing of 0.22 nm corresponds to the (111) crystal plane of Pd.
[0082] Finally, elemental composition analysis of the cross-section of the film after the deposition of the palladium nanoparticle layer was performed using energy-dispersive X-ray spectroscopy. The results are as follows: Figure 3 As shown in c, the results demonstrate the presence and uniform distribution of Sn, O, and Pd in the thin film.
[0083] Experimental Example 3
[0084] In terms of metal catalyst decoration on SMO, most researchers focus on optimizing the catalyst dosage by fixing the thickness of SMO. However, in reality, it is necessary to combine the thickness and morphology of SMO film to optimize the catalyst dosage in order to improve sensing performance.
[0085] This experimental example investigated the effects of Pd nanoparticle thickness (1–10 nm) and SnO2 film thickness (3 nm, 5 nm, 8 nm, and 11 nm, respectively) on the performance of the Pd-SnO2 sensor (prepared according to the preparation method of the H2 sensor in Example 3). Sensors with different Pd nanoparticle thicknesses and SnO2 film thicknesses were exposed to room temperature air (with an H2 content of 2%) to select the Pd nanoparticle thickness and SnO2 film thickness corresponding to the sensor with the best performance.
[0086] When the SnO2 film thickness in the sensor is 3 nm, and the palladium nanoparticle thicknesses are 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the dynamic response of the sensor at room temperature, with an H2 content (mass fraction) of 2% in the air, and a bias voltage of 0.1 V is as follows. Figure 4 As shown in a.
[0087] When the SnO2 film thickness in the sensor is 8 nm, and the palladium nanoparticle thicknesses are 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the dynamic response of the sensor at room temperature, with an H2 content (mass fraction) of 2% in the air, and a bias voltage of 0.1 V is as follows. Figure 4 As shown in b.
[0088] When the SnO2 film thickness in the sensor is 11 nm, and the palladium nanoparticle thicknesses are 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the dynamic response of the sensor at room temperature, with an H2 content (mass fraction) of 2% in the air, and a bias voltage of 0.1 V is as follows. Figure 4 As shown in c.
[0089] When the SnO2 film thickness in the sensor is 5 nm, and the palladium nanoparticle thicknesses are 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the dynamic response of the sensor at room temperature, with an H2 content (mass fraction) of 2% in the air, and a bias voltage of 0.1 V is as follows. Figure 4 As shown in d.
[0090] The above test results show that regardless of the SnO2 film thickness, the sensor response value changes significantly with increasing palladium nanoparticle thickness after contact with hydrogen. Furthermore, the sensor response value is maximized when the SnO2 film thickness is 5 nm and the Pd deposition thickness is 2 nm. For a given SnO2 film thickness, there is an optimal Pd nanoparticle thickness. When the SnO2 film thickness is 3 nm, the optimal palladium nanoparticle thickness is 4 nm; when the SnO2 film thickness is 5 nm, the optimal palladium nanoparticle thickness is 2 nm; when the SnO2 film thickness is 8 nm, the optimal palladium nanoparticle thickness is 2 nm; and when the SnO2 film thickness is 11 nm, the optimal palladium nanoparticle thickness is 3 nm. When the Pd nanoparticle thickness exceeds the optimal value, the sensor response decreases. The reason for the different optimal Pd nanoparticle thicknesses corresponding to different SnO2 film thicknesses is mainly due to the different surface roughness of the SnO2 film. During deposition, the effective surface area of palladium nanoparticles increases with increasing surface roughness of the SnO2 film. When the surface roughness of SnO2 is high, the content of Pd nanoparticles deposited on the SnO2 surface is larger. A 3nm SnO2 thickness is the optimal thickness while ensuring current stability. Considering the surface roughness, a 4nm Pd particle layer is chosen as the optimal condition.
[0091] To further investigate the influence of SnO2 film and Pd particle layer thickness on sensor performance, the initial resistance of sensors with SnO2 film and Pd particle layer thicknesses were tested. The results are as follows: Figure 5 As shown, when the thickness of the SnO2 thin film in the sensor is 3 nm, and the thickness of the palladium nanoparticles is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is as follows: Figure 5As shown in Figure a, when the thickness of the SnO2 thin film in the sensor is 5 nm, and the thicknesses of the palladium nanoparticles are 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is as follows: Figure 5 As shown in b, when the thickness of the SnO2 thin film in the sensor is 8 nm, and the thicknesses of the palladium nanoparticles are 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is as follows: Figure 5 As shown in Figure c, when the thickness of the SnO2 thin film in the sensor is 11 nm, and the thicknesses of the palladium nanoparticles are 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 nm, the initial resistance of the sensor is as follows: Figure 5 As shown in d.
[0092] The test results above show that during thermal evaporation, Pd initially forms scattered points and then gradually grows. When the evaporation thickness is low, the Pd scattered points are far apart, and only a few Pd grains connect to form electronic conduction paths, resulting in high resistance values. Furthermore, as the Pd thickness changes, the electrical conduction path of the sensor changes; when the Pd thickness exceeds the optimal value, the response values of all sensors decrease.
[0093] Meanwhile, TEM was used to characterize Pd-SnO2 films with different Pd nanoparticle thicknesses. TEM images of palladium nanoparticle layers with thicknesses of 1 nm, 3 nm, 5 nm, and 10 nm when the SnO2 film thickness was 3 nm are shown below. Figure 6 As shown, from Figure 6 It can be seen that the Pd nanoparticles are distributed on the surface of the SnO2 film, and before the optimal Pd thickness is reached, they only move through the SnO2 conduction pathway ( Figure 6 a, Figure 6 b and Figure 6 e); When the Pd thickness exceeds the optimal thickness, particle bonding and agglomeration occur. This creates additional electronic pathways through the Pd layer, thus reducing the sensor response due to its effect on sensor carrier modulation. Figure 6 c and Figure 6 d).
[0094] Experiment Example 4
[0095] After obtaining the optimal SnO2 film thickness and Pd particle layer thickness, sensors with different SnO2 film thicknesses and corresponding optimal Pd particle layer thicknesses were used to detect hydrogen gas with a mass fraction (20 ppm to 2%) in the air. The sensors were first exposed to room temperature air containing 0.002% hydrogen, and the resistance response (IL) of the H2 sensor was tested at different times. g / I aAfter the test results stabilized, the hydrogen sensor was placed in room temperature air without hydrogen, and the resistance response (I) of the H2 sensor was measured at different times. g / I a After the test results stabilized, the sensor was exposed to room temperature air containing a higher concentration of hydrogen, and the test was repeated. The hydrogen concentration (mass fraction) was 0.002%, 0.005%, 0.01%, 0.025%, 0.05%, 0.08%, 0.1%, 0.5%, 0.8%, 1%, 1.5%, and 2%, respectively. When the thickness of the SnO2 film in the sensor was 3 nm and the thickness of the palladium nanoparticles was 4 nm, the detection results were as follows. Figure 7 As shown, when the thickness of the SnO2 thin film in the sensor is 8 nm and the thickness of the palladium nanoparticles is 2 nm, the detection results are as follows. Figure 8 As shown, when the thickness of the SnO2 thin film in the sensor is 11 nm and the thickness of the palladium nanoparticles is 3 nm, the detection results are as follows. Figure 9 As shown, when the thickness of the SnO2 thin film in the sensor is 5 nm and the thickness of the palladium nanoparticles is 2 nm, the detection results are as follows. Figure 10 As shown in the figure. The test results above indicate that when the SnO2 film thickness in the sensor is 5 nm and the palladium nanoparticle thickness is 2 nm, the sensor exhibits the highest response value of 16623 when detecting hydrogen gas with a mass fraction of 2% in the air. This response value is higher than the response value of hydrogen sensors disclosed in the prior art when detecting hydrogen gas at room temperature.
[0096] The test results above show that the sensor has the highest response value when detecting hydrogen gas when the SnO2 film thickness is 5 nm and the Pd nanoparticle thickness is 2 nm.
[0097] Based on the above conclusions, further research was conducted on other performance aspects of the sensor. First, an H2 sensor (the H2 sensor of Example 1) with a SnO2 thin film thickness of 5 nm and Pd nanoparticle thickness of 2 nm was used to repeatedly detect H2 containing 2% by mass in air at room temperature. The repeatability method was as follows: the sensor was first exposed to room temperature air containing 2% by mass hydrogen, and the resistance response (IL) of the hydrogen sensor at different times was tested. g / I a After the test results stabilized, the hydrogen sensor was placed in room temperature air without hydrogen, and the resistance response (I) of the hydrogen sensor was measured at different times. g / I a After the test results stabilize, the sensor is exposed to room temperature air containing 2% hydrogen by mass for the next test cycle. The repeatability test is conducted for a total of 10 cycles, and the test results are as follows: Figure 11As shown in figure a. Repeated detection experiments show that the prepared sensor has good and stable response performance when detecting H2.
[0098] Meanwhile, the response time and recovery time of an H2 sensor (the H2 sensor of Example 1) with a SnO2 film thickness of 5 nm and Pd nanoparticle thickness of 2 nm were tested when detecting H2 containing a mass fraction of 2% in the air at room temperature. The test results are as follows: Figure 11 As shown in b, the results indicate that the response time is 6 s and the recovery time is 5 s. The catalytic activity of nano-Pd reduces the activation energy of the surface reaction, thereby improving the adsorption and desorption of H2 molecules.
[0099] Since common toxic gases such as CO, CO2, and CH4 have been shown to react with palladium catalysts, in order to study the selectivity of the sensor of this invention for H2, an H2 sensor (the H2 sensor of Example 1) with a SnO2 film thickness of 5 nm and a Pd nanoparticle thickness of 2 nm was tested at room temperature to detect air containing 0.005% by mass of H2, CO, CO2, and CH4, as well as air containing H2, CO, CO2, and CH4 simultaneously (each with a mass fraction of 0.005%). The results are as follows: Figure 11 As shown in c.
[0100] One drawback of current SMO sensors is their lack of long-term stability. This is mainly because the active Pd sites dissociated from H2 are easily poisoned by chemisorption by gases in the environment (such as CO and CH4). The long-term stability of the sensor was tested at room temperature using the following method: An H2 sensor (the H2 sensor of Example 1) with a SnO2 film thickness of 5 nm and Pd nanoparticle thickness of 2 nm was used to detect H2 in the air at mass fractions of 0.1% or 0.01% at room temperature. The resistance response (IL) of the hydrogen sensor was measured at different time points. g / I a After the test results stabilized, the hydrogen sensor was placed in room temperature air without hydrogen, and the resistance response (I) of the hydrogen sensor was measured at different times. g / I a After the test results stabilize, proceed to the next testing cycle; repeat the experiment 3-5 times every 24 hours and calculate the average value. The results of the repeated experiments are as follows: Figure 11 As shown in d. Because the selective PMMA layer protects the active Pd sites from the effects of toxic gases, the sensor exhibits good long-term stability.
[0101] In addition, an H2 sensor with a SnO2 film thickness of 100 nm and a Pd nanoparticle thickness of 2 nm, prepared according to the method of Example 3, was used to study the response of an air H2 concentration (mass fraction) of 0.01%, 0.05%, and 0.1% at different temperatures (20–120 °C), as well as the transient response to an air H2 concentration (mass fraction) of 0.1% at room temperature. The results are as follows: Figure 12 As shown.
[0102] Meanwhile, to evaluate the effects of the molecular weight of PMMA and the concentration of the PMMA solution on the performance of the prepared H2 sensors, the response values of the H2 sensors prepared in Comparative Examples 1-4 when detecting hydrogen gas with a mass fraction of 2% in the air, the response time and recovery time when detecting air containing 2% H2 at room temperature, and the response values when detecting air containing H2, CO, CO2, and CH4 (all with a mass fraction of 0.005%) at room temperature were tested according to the above method. The test results showed that compared with the H2 sensor prepared in Example 3, the performance of the H2 sensors prepared in Comparative Examples 1-4 was worse (smaller response values, longer response times and recovery times).
[0103] Experimental Example 5
[0104] To test the effect of air humidity on the detection results, an H2 sensor with a SnO2 film thickness of 5 nm and Pd nanoparticle thickness of 2 nm was used to detect H2 in air at different relative humidities at room temperature. The relative humidity of the air ranged from 0% to 85%, and the mass fraction of H2 in the air was 0.1%. The detection results are as follows: Figure 13 As shown in a.
[0105] To test the effect of temperature on the detection results, an H2 sensor with a SnO2 film thickness of 5 nm and Pd nanoparticle thickness of 2 nm was used to detect H2 in air at different temperatures (20–120 °C) at room temperature. The H2 content (mass fraction) in the air was 0.005%, 0.01%, 0.025%, 0.05%, 0.08%, and 0.1%, respectively. The detection results are as follows: Figure 13 As shown in b, the test results show that the sensor exhibits a stable response at all temperatures, with a relatively high response value at 100℃.
[0106] Experimental Example 6
[0107] The H2 sensing mechanism of the sensor can be described by the changes in conductivity or resistance in different gases caused by variations in carrier concentration during adsorption, electron transfer, and desorption. This can be further explained by the current changes and chemical sensing mechanisms of a noble metal-modified SMO-based sensor. The sensitization effect of Pd was investigated using XPS spectroscopy of SnO2 and Pd-SnO2, and the contributions of the two sensitization mechanisms to the sensor response were quantified. Figure 14 As shown, the Sn spectra of SnO2 and Pd-SnO2 before and after Pd deposition are basically the same, indicating that the electronic interaction between Pd and SnO2 is not significant. Therefore, the sensor response must be due to chemical sensitization or the catalytic effect of Pd, which decomposes oxygen into highly reactive substances. This can be explained by the O1s spectra of SnO2 and Pd-SnO2. The O1s spectra before and after deposition are significantly different, reflecting the lattice oxygen (O2) in the O1s spectra of Pd / SnO2. latt ), surface reactive oxygen species (O) ads ) and surface OH groups. Surface active oxygen (O ads The catalytic effect of Pd increases the amount of reactive oxygen species (O2) on the surface of metal oxides. 2- O - O 2- The O1s spectrum indicates that the Pd / SnO2 film has extremely high surface O content. ads The concentration (49.96%) was higher than the surface O of the original SnO2. ads Concentration (3.88%). This is due to the catalytic overflow effect of the Pd catalyst, which significantly activates molecular oxygen by generating a large change in resistance or conductivity to the metal oxide, thereby enhancing the sensing response and resulting in a higher sensor response.
[0108] Experimental Example 7
[0109] This experimental example investigated the response of a transparent, flexible H2 sensor to different concentrations of H2 at room temperature. The H2 sensor from Example 2 (such as...) was used... Figure 15 (a) The sensor was exposed to different concentrations of H2 (H2 concentration in air ranges from 100 ppm to 2%), and the resistance response (I) of the H2 sensor was tested at different times. g / I a The result is as follows Figure 15 As shown in b. The results show that the sensor has a response value of 2300 for H2 in the air with a mass fraction of 2%, exhibiting good sensitivity. The H2 sensor of Example 2 was then used to repeatedly detect H2 in the air with a mass fraction of 2% or 0.1% at room temperature (test cycle of 10 cycles), and the results are as follows. Figure 15As shown in c and 15d, the H2 sensor of Example 2 exhibits good stability and slight drift. The cross-selectivity of the H2 sensor of Example 2 for CO, CO2, and CH4 was also tested. Specifically, the H2 sensor of Example 2 was used to detect gases A, B, C, D, and E at room temperature. Gas A was air containing H2 (H2 concentration of 50 ppm), gas B was air containing H2 and CO (H2 and CO concentrations of 50 ppm each), gas C was air containing H2 and CO2 (H2 and CO2 concentrations of 50 ppm each), gas D was air containing H2 and CH4 (H2 and CH4 concentrations of 50 ppm each), and gas E was air containing H2, CO, CO2, and CH4 (H2, CO, CO2, and CH4 concentrations of 50 ppm each). The test results are shown below. Figure 15 As shown in e. As mentioned earlier, due to the thin PMMA layer, the influence of interfering gases is almost eliminated, and the sensitivity remains almost constant regardless of the environment. Furthermore, the response of the H2 sensor of Example 2 to H2 concentrations (mass fractions) of 0.01%, 0.025%, 0.05%, and 0.08% in the air at different temperatures (20–120°C) was tested, and the results are as follows. Figure 15 As shown in f. Although the response is very high at room temperature (20°C), the response value increases almost 7 times when the temperature is increased to 100°C.
Claims
1. A H2 sensor, characterized in that: It comprises a substrate, a SnO2 layer, a palladium particle layer and a polymer layer which are sequentially laminated; the polymer layer is a polymethyl methacrylate layer; The H2 sensor further comprises an electrode layer; the electrode layer is spaced between the palladium particle layer and the polymer layer; or the electrode layer is spaced between the SnO2 layer and the polymer layer, and the palladium particle layer is located between the spaced electrode layers.
2. The H2 sensor according to claim 1, characterized in that The thickness of the SnO2 layer is 3nm, and the thickness of the palladium particle layer is 4nm; or the thickness of the SnO2 layer is 5nm, and the thickness of the palladium particle layer is 2nm; or the thickness of the SnO2 layer is 8nm, and the thickness of the palladium particle layer is 2nm; or the thickness of the SnO2 layer is 11nm, and the thickness of the palladium particle layer is 3nm.
3. The H2 sensor according to claim 1, characterized in that The weight average molecular weight of the polymethyl methacrylate in the polymethyl methacrylate layer is 250,000 to 350,000.
4. The H2 sensor according to claim 1, characterized in that The thickness of the polymer layer is 50-70 nm.
5. The H2 sensor according to any one of claims 1 to 4, characterized in that: The electrode layer includes a transition layer and a conductive layer, the transition layer is a Ti layer or a Cr layer; the electrode layer is arranged between the palladium particle layer and the polymer layer, and the electrode layer is arranged on the palladium particle layer through the transition layer; or the electrode layer is arranged between the SnO2 layer and the polymer layer, and the electrode layer is arranged on the SnO2 layer through the transition layer.
6. The H2 sensor according to claim 5, characterized in that The thickness of the transition layer is 2-3 nm.
7. The method for preparing a H2 sensor according to any one of claims 1 to 6, characterized in that: The following steps are involved: A SnO2 precursor solution is coated on a substrate to form a SnO2 layer after drying, a palladium particle layer is deposited on the SnO2 layer, an electrode layer is deposited on the palladium particle layer at intervals, and a polymer solution is coated on the electrode layer and the palladium particle layer to form a polymer layer after drying; Alternatively, a SnO2 precursor solution is coated on the substrate to form a SnO2 layer after drying, and then a palladium particle layer and an electrode layer are deposited on the SnO2 layer to form spaced electrode layers, with the palladium particle layer being located between the spaced electrode layers, and then a polymer solution is coated on the palladium particle layer and the electrode layer to form a polymer layer after drying.
8. The method for preparing the H2 sensor according to claim 7, characterized in that: The SnO2 precursor solution is prepared by a method comprising the following steps: mixing 2-methoxyethanol and stannous chloride dihydrate until the stannous chloride dihydrate is completely dissolved, and separating the solid from the liquid to obtain the SnO2 precursor solution.
9. The method for preparing the H2 sensor according to claim 7, characterized in that: The concentration of the polymethyl methacrylate solution is 35-50 mg / mL.
10. The method for preparing the H2 sensor according to claim 7, characterized in that: The temperature of drying after coating the polymer solution does not exceed 175°C.
Citation Information
Cited By
Nano array for exposing SnO2 high-activity crystal face, preparation method and application of nano array in hydrogen sensing
CN120717819A
A sensor for hydrogen detection and a method of manufacture of the sensor
CZ20250087A3
A sensor for hydrogen detection and a method of manufacture of the sensor