A flip-chip LED chip and its preparation method
By using a composite Cappping layer composed of Ti and Ni materials to cover the silver reflector layer in the flip-up LED chip, the problem of poor sensitivity and adhesion of the silver mirror structure to moisture and organic matter is solved, and the stability and brightness of the chip are improved , reducing the risk of divestiture.
Patent Information
- Application Number
- CN202411245507.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The silver mirror structure flip-fitting LED chip is sensitive to organic matter such as moisture, oxygen and sulfide, and is prone to oxidation, vulcanization or contamination, resulting in a decrease in optical properties, and the adhesion of metal silver is poor, which is prone to the risk of peeling and interface failure.
The composite Capping layer consisting of Ti and Ni materials stacked successively covers the silver reflector layer, and controls the film angle and thickness of the Capping layer to optimize optical performance and protection effects, and improves the between the silver reflector layer and the upper material. Adhesion.
By optimizing the structure of the Capping layer, the stability and brightness of the silver reflector layer are improved, the risks of peeling and interface failure are reduced, and the reliability of the overall structure is enhanced.
Smart Images

Figure CN118763162B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a flip-chip LED chip and a preparation method thereof. Background Art
[0002] With the rapid development of semiconductor lighting technology, light-emitting diodes (LEDs) have become the mainstream choice for the new generation of lighting sources due to their high efficiency, energy saving, and environmental protection. Among the many LED technologies, flip-chip LEDs (FCLEDs) have gradually attracted widespread attention in the industry due to their superior thermal management performance and high light efficiency. In order to further improve the performance of flip-chip LEDs, the introduction of silver mirror structures has become an important research direction. The silver mirror structure is a design that uses silver as a reflective layer on the surface of the LED chip.
[0003] It should be noted that the silver mirror layer in the silver mirror structure flip-chip LED chip is one of the key light extraction structures. However, the silver mirror layer is sensitive to moisture, oxygen, sulfide and other organic matter in the environment, and is prone to oxidation, sulfidation or contamination, resulting in a decrease in its optical performance. At the same time, since the adhesion of metallic silver itself is often poor, it is prone to the risk of peeling and interface failure. Therefore, it is necessary to improve the preparation process of the silver mirror layer to improve its stability and durability.
[0004] Protecting the silver mirror layer and improving the adhesion of the silver mirror are important steps to ensure the long-term stability and performance of the silver mirror structure flip-chip LED chip. At present, the commonly used method is usually to cover the silver mirror layer with a capping layer to protect the silver layer. The capping layer is located on the surface of the silver mirror layer and plays a role of sealing and protection. How to make a good capping layer is the key to preparing high-performance silver mirror products. Summary of the invention
[0005] Based on this, the purpose of the present invention is to provide a flip-chip LED chip and a preparation method thereof, aiming to improve the luminance of the flip-chip LED chip while improving the stability and reliability of the overall structure and reducing the risk of peeling and interface failure.
[0006] A flip-chip LED chip according to an embodiment of the present invention comprises a silver reflector layer and a capping layer covering the silver reflector layer, wherein the capping layer is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, wherein the materials of the first sublayer, the third sublayer and the fifth sublayer are all Ti, the materials of the second sublayer and the fourth sublayer are Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer;
[0007] When the film angle of the silver reflector layer is a preset angle, the film angle of the capping layer should be greater than half of the preset angle, and the distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is 0.2 μm to 2 μm.
[0008] Furthermore, the flip-chip LED chip further includes an N-type GaN layer, an active layer, a P-type GaN layer, an ITO layer, a protective layer and an electrode layer;
[0009] The N-type GaN layer, the active layer, the P-type GaN layer, the ITO layer, the silver reflector layer, the capping layer and the protective layer are deposited in sequence, wherein the silver reflector layer covers the ITO layer, and a through hole is opened at a corresponding position of the protective layer for setting the electrode.
[0010] Furthermore, the thickness of the first sublayer and the third sublayer is 40nm-100nm, the thickness of the second sublayer and the fourth sublayer is 20nm-100nm, and the thickness of the fifth sublayer is 5nm.
[0011] Furthermore, the thickness of the silver reflector layer is 100nm-150nm.
[0012] Furthermore, the preset angle is 20°~25°.
[0013] Furthermore, the electron beam evaporation equipment for the silver reflector layer and the capping layer is any one of a 32° plating pot equipment, a 45° plating pot equipment and an eccentric equipment.
[0014] A method for preparing a flip-chip LED chip according to an embodiment of the present invention is used to prepare the above flip-chip LED chip, and the preparation method comprises:
[0015] A silver reflector layer and a capping layer covering the silver reflector layer are sequentially deposited, wherein the capping layer is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, wherein the first sublayer, the third sublayer and the fifth sublayer are made of Ti, the second sublayer and the fourth sublayer are made of Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer;
[0016] When the film angle of the silver reflector layer is a preset angle, the film angle of the capping layer should be greater than half of the preset angle, and the distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is 0.2 μm to 2 μm.
[0017] The beneficial effects of the present invention are:
[0018] By setting a silver reflector layer and a Capping layer covering the silver reflector layer, the Capping layer is a composite structure composed of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, the materials of the first sublayer, the third sublayer and the fifth sublayer are all Ti, the materials of the second sublayer and the fourth sublayer are Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer; wherein, when the film angle of the silver reflector layer is a preset angle, the film angle of the Capping layer should be greater than half of the preset angle, and the distance between the bottom of the silver reflector layer and the bottom of the Capping layer is 0.2μm~2μm. Specifically, by controlling the thickness and angle of the Capping layer, the optical performance and protective effect of the Capping layer can be optimized, and the effective area of the silver reflector layer can be maximized; in addition, the Capping layer can improve the adhesion between the silver reflector layer and the upper material (such as packaging material or protective coating). By optimizing the interface adhesion, the stability and reliability of the overall structure can be improved, and the risk of peeling and interface failure can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of the structure of a flip-chip LED chip provided by an embodiment of the present invention;
[0020] Figure 2 A flow chart of a method for preparing a flip-chip LED chip provided by an embodiment of the present invention;
[0021] Figure 3 This is a SEM scanning electron microscope image of the silver reflector layer and the capping layer of the flip-chip LED chip in Example 3;
[0022] Figure 4 This is a SEM scanning electron microscope image of the silver reflector layer and the capping layer of the flip-chip LED chip in Example 6. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0024] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0026] refer to Figure 1 , is a schematic structural diagram of a flip-chip LED chip provided by an embodiment of the present invention, wherein the flip-chip LED chip comprises an N-type GaN layer 2, an active layer 3, a P-type GaN layer 4, an ITO layer 5, a silver reflector layer 6, a Capping layer 7 and a protective layer 8 deposited in sequence, wherein the Capping layer 7 covers the silver reflector layer 6, the silver reflector layer 6 covers the ITO layer 5, and a through hole is opened at a corresponding position of the protective layer 8 for setting an electrode. Among them, the material of the protective layer 8 is SiO2, a first through hole is opened in the protective layer 8 above the capping layer 7, a P-type electrode 9 is set at the first through hole, a second through hole is opened in the protective layer 8 above the N-type GaN layer 2, and an N-type electrode 10 is set at the second through hole. It can be understood that after the N-type GaN layer 2, the active layer 3, the P-type GaN layer 4, and the ITO layer 5 are deposited on the substrate 1 in sequence, a pattern is made on the ITO by photolithography technology, and the ITO in a specific area is etched by wet etching using a photoresist as a mask to obtain the ITO layer 5, and then the epitaxial layer is etched to the N-type GaN layer 2 by a dry etching process. It should be noted that epitaxial growth is performed on the substrate 1, and a flip-chip LED chip is prepared, and finally the prepared flip-chip LED chip is peeled off from the substrate 1.
[0027] In this embodiment, the capping layer 7 is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence. The materials of the first sublayer, the third sublayer and the fifth sublayer are all Ti, the materials of the second sublayer and the fourth sublayer are Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer. Specifically, the thicknesses of the first sublayer and the third sublayer are 40nm~100nm, the thicknesses of the second sublayer and the fourth sublayer are 20nm~100nm, and the thickness of the fifth sublayer is 5nm. For example, the thickness of the first sublayer and the third sublayer is 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, but not limited to this; the thickness of the second sublayer and the fourth sublayer is 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, but not limited to this; it can be understood that the thickness of the second sublayer and the fourth sublayer is the same, the thickness of the first sublayer and the third sublayer is the same, and the thickness of the second sublayer and the fourth sublayer may be the same as or different from that of the first sublayer and the third sublayer.
[0028] The thickness of the silver reflector layer 6 is 100 nm to 150 nm. Exemplarily, the thickness of the silver reflector layer 6 is 100 nm, 110 nm, 120 nm, 130 nm, 140 nm or 150 nm, but is not limited thereto.
[0029] It should be noted that when the film angle of the silver reflector layer 6 is a preset angle, the film angle of the capping layer 7 should be greater than half of the preset angle, and the distance between the lower bottom of the silver reflector layer 6 and the lower bottom of the capping layer 7 is 0.2μm~2μm. Specifically, the preset angle is 20°~25°. Exemplarily, the preset angle is 20°, 21°, 22°, 23°, 24° or 25°, etc., but not limited to this. It can be understood that when the film angle of the silver reflector layer 6 is 20°, the film angle of the capping layer 7 should be greater than 10°; when the film angle of the silver reflector layer 6 is 25°, the film angle of the capping layer 7 should be greater than 12.5°. In addition, illustratively, the distance between the bottom of the silver reflective mirror layer 6 and the bottom of the capping layer 7 is 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 1 μm, 1.5 μm or 2 μm, but is not limited thereto.
[0030] Furthermore, the electron beam evaporation equipment for the silver reflector layer 6 and the capping layer 7 is any one of a 32° plating pot equipment (Dome 32˚), a 45° plating pot equipment (Dome 45˚) and an eccentric equipment (Source Shift). Different evaporation equipment can make the deposited metal layer present different angles. The electron beam evaporation equipment for the silver reflector layer 6 and the capping layer 7 can be the same equipment or different equipment.
[0031] In this embodiment, the film angles of the silver reflector layer 6 and the capping layer 7 are mainly determined by the electron beam evaporation equipment, wherein the film angles of the evaporated films are Dome 32˚>Dome 45˚>Source Shift. It can be understood that the distance between the bottom of the silver reflector layer 6 and the bottom of the capping layer 7 is mainly determined by the angle relationship between the two. When the film angle of the silver reflector layer 6 remains unchanged, the larger the film angle of the capping layer 7 is, the smaller the distance is; when the film angle of the capping layer 7 remains unchanged, the larger the film angle of the silver reflector layer 6 is, the larger the distance is.
[0032] refer to Figure 2 The present invention also provides a method for preparing a flip-chip LED chip, which specifically includes the following steps:
[0033] S100: providing a substrate;
[0034] The substrate may be a sapphire substrate, wherein a mixed solution of deionized water, ammonia water and hydrogen peroxide is used to perform ultrasonic cleaning on the sapphire substrate to remove organic matter and particulate matter on the surface.
[0035] S200: depositing an N-type GaN layer, an active layer, a P-type GaN layer, an ITO layer, a silver reflector layer, a capping layer and a protective layer in sequence on the substrate along the epitaxial growth direction;
[0036] S300: peeling off the substrate;
[0037] Specifically, S200 includes:
[0038] S201: growing a 1μm gallium nitride buffer layer, a 4μm N-type GaN layer, and three periods of active layers on a sapphire substrate in sequence by MOCVD (Metal-organic Chemical Vapor Deposition) technology, wherein the thickness of a single quantum well layer is 3nm, the thickness of a single quantum barrier layer is 12nm, the quantum well layer is an InGaN layer, and the quantum barrier layer is a GaN layer, then growing a 20nm thick P-type AlGaN layer and a P-type GaN layer to obtain a GaN epitaxial wafer, which is then cleaned with an organic solution;
[0039] S202: depositing an ITO layer on the GaN epitaxial wafer by magnetron sputtering technology, making a pattern on the ITO layer by photolithography technology, etching the ITO layer in a specific area by wet etching using a photoresist as a mask, and then continuing to etch the epitaxial layer to the N-type GaN layer by dry etching process;
[0040] S203: reserving a pattern on a wafer by photolithography technology, and depositing metallic silver on the wafer by electron beam evaporation technology to obtain a silver reflector layer;
[0041] S204: Continue to deposit a capping layer on the surface of the silver reflector layer by using electron beam evaporation technology to protect the silver reflector layer;
[0042] S205: depositing another protective layer on the silver reflector layer, and forming a conductive through hole by dry etching technology;
[0043] S206: depositing a multilayer metal film (such as Ti / Al / Ni / Au) by electron beam evaporation or sputtering equipment to form an N-type electrode and a P-type electrode;
[0044] Trimethylaluminum (TMAl), trimethylindium (TMIn), trimethylgallium or triethylgallium (TMGa or TEGa) are used as precursors of group III sources, ammonia (NH3) and antimonide (SbH3) are used as precursors of group V sources, silane (SiH4) and bismuthocene magnesium (Cp2Mg) are used as precursors of N-type dopants and P-type dopants, respectively, and nitrogen and hydrogen are used as carrier gases.
[0045] The present invention will be further described below with specific embodiments:
[0046] Example 1
[0047] Embodiment 1 of the present invention provides a flip-chip LED chip, which includes a GaN buffer layer, an N-type GaN layer, an active layer, a P-type AlGaN layer, a P-type GaN layer, an ITO layer, a silver reflector layer, a Capping layer, and a protective layer deposited in sequence, wherein the Capping layer covers the silver reflector layer, the silver reflector layer covers the ITO layer, and a through hole is provided at a corresponding position of the protective layer for setting an electrode. The material of the protective layer is SiO2, a first through hole is provided in the protective layer above the Capping layer, a P-type electrode is provided at the first through hole, a second through hole is provided in the protective layer above the N-type GaN layer, and an N-type electrode is provided at the second through hole. It can be understood that after the N-type GaN layer, the active layer, the P-type GaN layer, and the ITO layer are deposited on the substrate in sequence, a pattern is made on the ITO by photolithography technology, a photoresist is used as a mask, and the ITO in a specific area is etched by wet etching, and then the epitaxial layer is etched to the N-type GaN layer by dry etching. It should be noted that epitaxial growth is carried out on a substrate to prepare a flip-chip LED chip, and finally the prepared flip-chip LED chip is peeled off from the substrate.
[0048] In this embodiment, the capping layer is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, the materials of the first sublayer, the third sublayer and the fifth sublayer are all Ti, the materials of the second sublayer and the fourth sublayer are Ni, the thickness of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all 100nm, and the thickness of the fifth sublayer is 5nm. The capping layer is electron beam evaporated using a 32° plating pot equipment.
[0049] The thickness of the silver reflector layer is 120 nm, and it is deposited by electron beam evaporation using a 32° plating pot equipment.
[0050] It should be noted that the film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 30.4°. The distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is 0.12 μm.
[0051] The embodiment of the present invention further provides a method for preparing a flip-chip LED chip, which specifically comprises the following steps:
[0052] 1. Provide a substrate;
[0053] The substrate may be a sapphire substrate, wherein the sapphire substrate is ultrasonically cleaned for 5 minutes using a mixed solution of deionized water, ammonia water and hydrogen peroxide to remove organic matter and particulate matter on the surface.
[0054] 2. Depositing a GaN buffer layer, an N-type GaN layer, an active layer, a P-type AlGaN layer, a P-type GaN layer, an ITO layer, a silver reflector layer, a capping layer and a protective layer in sequence on the substrate along the epitaxial growth direction;
[0055] 3. Peel off the substrate;
[0056] Specifically, the steps of sequentially depositing a GaN buffer layer, an N-type GaN layer, an active layer, a P-type AlGaN layer, a P-type GaN layer, an ITO layer, a silver reflector layer, a capping layer and a protective layer on the substrate along the epitaxial growth direction include:
[0057] Step 1: Using MOCVD (Metal-organic Chemical Vapor Deposition) technology, a 1μm gallium nitride buffer layer, a 4μm N-type GaN layer, and three periods of active layers are grown on a sapphire substrate in sequence, wherein the thickness of a single quantum well layer is 3nm, the thickness of a single quantum barrier layer is 12nm, the quantum well layer is an InGaN layer, and the quantum barrier layer is a GaN layer. Then, a P-type AlGaN layer and a P-type GaN layer with a thickness of 20nm are grown to obtain a GaN epitaxial wafer, which is then cleaned with an organic solution. Specifically, the GaN epitaxial wafer is sequentially immersed in acetone ultrasound for 5min, isopropanol shaking for 30s, and sulfuric acid and hydrogen peroxide mixed solution (sulfuric acid: hydrogen peroxide = 5:1) at 90°C for 5min;
[0058] Step 2: Deposit an ITO layer with a thickness of 15 nm on the GaN epitaxial wafer using magnetron sputtering technology, make a pattern on the ITO layer using photolithography technology, etch the ITO layer in a specific area using wet etching using photoresist as a mask, and then continue to etch the epitaxial layer to the N-type GaN layer using a dry etching process;
[0059] Step 3: Pre-set a pattern on the wafer by photolithography technology, and deposit metallic silver on the wafer by electron beam evaporation technology to obtain a silver reflector layer with a thickness of 120 nm, wherein the electron beam evaporation equipment is a 32° plating pot equipment;
[0060] Step 4: Continue to deposit a Capping layer on the surface of the silver reflector layer by electron beam evaporation technology to protect the silver reflector layer, wherein the electron beam evaporation equipment is a 32° plating pot equipment, and the Capping layer is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, wherein the materials of the first sublayer, the third sublayer and the fifth sublayer are all Ti, the materials of the second sublayer and the fourth sublayer are Ni, the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all 100 nm, and the thickness of the fifth sublayer is 5 nm;
[0061] Step 5: depositing a 600nm thick SiO2 protective layer on the silver reflector layer, and making conductive through holes by dry etching technology;
[0062] Step 6: Deposit multiple layers of metal films (such as Ti / Al / Ni / Au) through electron beam evaporation or sputtering equipment to form N-type electrodes and P-type electrodes.
[0063] In this embodiment, trimethylaluminum (TMAl), trimethylindium (TMIn), trimethylgallium or triethylgallium (TMGa or TEGa) are used as precursors of the group III source, ammonia (NH3) and antimonide (SbH3) are used as precursors of the group V source, silane (SiH4) and bismuth magnesium (Cp2Mg) are used as precursors of the N-type dopant and the P-type dopant, respectively, and nitrogen and hydrogen are used as carrier gases.
[0064] Example 2
[0065] Embodiment 2 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation device of the capping layer is an eccentric device. The film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 11.5°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 1.43 μm.
[0066] Example 3
[0067] Embodiment 3 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation device of the capping layer is an eccentric device, and the thickness of the silver reflector layer is 100 nm. The film angle of the silver reflector layer is 22.9°, and the film angle of the capping layer is 10.8°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 1.46 μm.
[0068] Example 4
[0069] Embodiment 4 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation device of the capping layer is an eccentric device, and the thickness of the silver reflector layer is 150nm. The film angle of the silver reflector layer is 24°, and the film angle of the capping layer is 12.1°. The distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is 1.42μm.
[0070] Example 5
[0071] Embodiment 5 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation equipment of the capping layer is a 45° plating pot equipment. The film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 26.8°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 0.33 μm.
[0072] Example 6
[0073] Embodiment 6 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation device of the capping layer is an eccentric device, and the thicknesses of the first sublayer, the second sublayer, the third sublayer, and the fourth sublayer are all 50 nm. The film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 9°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 1.28 μm.
[0074] Example 7
[0075] Embodiment 7 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation equipment of the capping layer is a 45° plating pot equipment, and the thicknesses of the first sublayer, the second sublayer, the third sublayer, and the fourth sublayer are all 50 nm. The film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 20.4°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 0.44 μm.
[0076] Example 8
[0077] Embodiment 8 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation device of the capping layer is an eccentric device, the thickness of the first sublayer and the third sublayer are both 40nm, and the thickness of the second sublayer and the fourth sublayer are both 20nm. The film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 8.7°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 1.4μm.
[0078] Example 9
[0079] Embodiment 9 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation equipment of the capping layer is a 45° plating pot equipment, the thickness of the first sublayer and the third sublayer are both 40nm, and the thickness of the second sublayer and the fourth sublayer are both 20nm. The film angle of the silver reflector layer is 23.5°, and the film angle of the capping layer is 15.5°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 0.56μm.
[0080] Example 10
[0081] Embodiment 10 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation device for the silver reflector layer is a 45° plating pot device, and the electron beam evaporation device for the capping layer is an eccentric device. The film angle of the silver reflector layer is 7.8°, and the film angle of the capping layer is 11.5°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 1.21 μm.
[0082] Embodiment 11
[0083] Embodiment 11 of the present invention also provides a flip-chip LED chip and a preparation method thereof, which is different from Embodiment 1 in that the electron beam evaporation equipment of the silver reflector layer is a 45° plating pot equipment, the electron beam evaporation equipment of the capping layer is an eccentric equipment, and the thickness of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all 50nm. The film angle of the silver reflector layer is 7.8°, and the film angle of the capping layer is 9.2°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 0.93μm.
[0084] Example 12
[0085] Embodiment 12 of the present invention also provides a flip-chip LED chip and a method for preparing the same. The difference from Embodiment 1 is that the electron beam evaporation equipment for the silver reflector layer is a 45° plating pot equipment, the electron beam evaporation equipment for the capping layer is an eccentric equipment, the thickness of the first sublayer and the third sublayer are both 40nm, and the thickness of the second sublayer and the fourth sublayer are both 20nm. The film angle of the silver reflector layer is 7.8°, and the film angle of the capping layer is 8.5°. The distance between the bottom of the silver reflector layer and the bottom of the capping layer is 0.67μm.
[0086] Comparative Example 1
[0087] Comparative Example 1 also provides a flip-chip LED chip and a preparation method thereof, which is different from Example 1 in that there is no capping layer.
[0088] The flip-chip LED chips in Examples 1 to 12 and Comparative Example 1 were tested under the same conditions (test current 120 mA), and the specific results are as follows:
[0089]
[0090] It can be seen from the table that the brightness of the flip-chip LED chip prepared in the embodiment of the present invention is improved to varying degrees, and the falling of the silver reflector layer is significantly improved. Figure 3 and Figure 4 , Figure 3 This is a SEM scanning electron microscope image of the silver reflector layer and the capping layer of the flip-chip LED chip in Example 3. Figure 4 This is a SEM scanning electron microscope image of the silver reflector layer and the capping layer of the flip-chip LED chip in Example 5. It can be found that when the distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is as small as possible, the film angle of the silver reflector layer is larger, so that the silver reflector layer can occupy a larger area and improve the brightness of the chip.
[0091] In summary, the flip-chip LED chip and the preparation method thereof in the embodiments of the present invention are provided with a silver reflector layer and a Capping layer covering the silver reflector layer. The Capping layer is a composite structure composed of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence. The materials of the first sublayer, the third sublayer and the fifth sublayer are all Ti, the materials of the second sublayer and the fourth sublayer are Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer. When the film angle of the silver reflector layer is a preset angle, the film angle of the Capping layer should be greater than half of the preset angle, and the distance between the lower bottom of the silver reflector layer and the lower bottom of the Capping layer is 0.2μm~2μm. Specifically, by controlling the thickness and angle of the capping layer, the optical performance and protective effect of the capping layer can be optimized, and the effective area of the silver reflector layer can be maximized; in addition, the capping layer can improve the adhesion between the silver reflector layer and the upper material (such as packaging material or protective coating). By optimizing the interface adhesion, the stability and reliability of the overall structure can be improved, and the risk of peeling and interface failure can be reduced.
[0092] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A flip-chip LED chip, characterized in that: It comprises a silver reflector layer and a capping layer covering the silver reflector layer, wherein the capping layer is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, wherein the first sublayer, the third sublayer and the fifth sublayer are made of Ti, the second sublayer and the fourth sublayer are made of Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer; Wherein, when the film angle of the silver reflector layer is a preset angle, the film angle of the capping layer should be greater than half of the preset angle, the preset angle is 20°~25°, and the distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is 0.2μm~2μm; The flip-chip LED chip further includes an N-type GaN layer, an active layer, a P-type GaN layer, an ITO layer, a protective layer and an electrode layer; The N-type GaN layer, the active layer, the P-type GaN layer, the ITO layer, the silver reflector layer, the capping layer and the protective layer are deposited in sequence, wherein the silver reflector layer covers the ITO layer, and a through hole is opened at a corresponding position of the protective layer for setting the electrode; The thickness of the first sublayer and the third sublayer is 40nm-100nm, the thickness of the second sublayer and the fourth sublayer is 20nm-100nm, and the thickness of the fifth sublayer is 5nm; The thickness of the silver reflector layer is 100nm-150nm.
2. The flip-chip LED chip according to claim 1, characterized in that: The electron beam evaporation equipment for the silver reflector layer and the capping layer is any one of a 32° plating pot equipment, a 45° plating pot equipment and an eccentric equipment.
3. A method for preparing a flip-chip LED chip, characterized in that: Used to prepare the flip-chip LED chip according to any one of claims 1-2, the preparation method comprising: A silver reflector layer and a capping layer covering the silver reflector layer are sequentially deposited, wherein the capping layer is a composite structure consisting of a first sublayer, a second sublayer, a third sublayer, a fourth sublayer and a fifth sublayer stacked in sequence, wherein the first sublayer, the third sublayer and the fifth sublayer are made of Ti, the second sublayer and the fourth sublayer are made of Ni, and the thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are all greater than the thickness of the fifth sublayer; When the film angle of the silver reflector layer is a preset angle, the film angle of the capping layer should be greater than half of the preset angle, and the distance between the lower bottom of the silver reflector layer and the lower bottom of the capping layer is 0.2 μm to 2 μm.