Method for preparing large-area oriented molecular sieve mixed matrix membrane based on selective etching

By using selective etching in the polymer to adjust the b-orientation of MFI molecular sieve crystals, and combining it with polyether block polyamide polymers, the compatibility issue between polymers and fillers is solved, achieving high permeability and high selectivity. The unique mixed matrix membrane improves gas or liquid separation efficiency and membrane stability.

CN118767708AActive Publication Date: 2024-10-15ZHEJIANG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410927774.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Poor adhesion between existing polymers and fillers leads to non-selective interfacial voids, polymer aging issues or inherent permeability-selectivity trade-offs that make it difficult to achieve a balance of high permeability and sufficient selectivity, and inorganic Traditional incompatibilities between fillers and polymers affect membrane uniformity and performance.

Method used

By combining high-performance CO2-affinity MFI zeolite filler with polyether block polyamide (pebax) polymer, selective etching method is used to adjust the morphology of MFI molecular sieve crystals to b orientation, combined with solution casting and gelation Curing technology realizes the directional self-assembly of molecular sieve materials in polymers and prepares large-area oriented molecular sieve mixed matrix membranes.

Benefits of technology

Achieving a balance of high permeability and high selectivity, improving membrane performance and stability, overcoming incompatibility between polymers and inorganic nanomaterials, extending membrane life, and providing efficient gas or liquid separation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767708A_ABST
    Figure CN118767708A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a large-area oriented molecular sieve mixed matrix membrane based on selective etching, the form of an MFI molecular sieve crystal is adjusted to a b-oriented sheet material through selective etching, the (0k0) crystal face is exposed to the maximum extent, and a basis is provided for ordered arrangement of nanosheets in a polymer matrix. By utilizing a solution pouring strategy, regulating and controlling the volatilization temperature of a solvent and combining the gel curing characteristic of pebax at room temperature, agglomeration of a molecular sieve material is effectively prevented, plane arrangement is formed in a polymer matrix, and the exposure degree of a vertical transmission pore channel is remarkably improved, so that the molecular transmission efficiency of the membrane and the permeation flux and selectivity of gas and liquid are improved; meanwhile, the stability and the service life of the membrane are enhanced. According to the method, the incompatibility between the traditional filler and the polymer is overcome, the large-area flexible mixed matrix MFI molecular sieve membrane and the ultrathin mixed matrix membrane are successfully prepared, and the defects of filler aggregation and non-selectivity are effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of separation membrane preparation, and in particular relates to a method for preparing a large-area oriented molecular sieve mixed matrix membrane based on selective etching. Background Art

[0002] To meet the industrial demand for efficient gas separation membranes, existing methods for preparing zeolite mixed matrix membranes include a variety of technical means. First, selecting polymers and inorganic fillers suitable for the target separation application is a key step. Fillers (such as zeolites, metal organic frameworks, etc.) usually need to be surface functionalized to improve their compatibility with the polymer matrix, such as modification with silane coupling agents or other surfactants. The functionalized filler is evenly dispersed in the polymer solution, and the uniformity of the mixed suspension is ensured by ultrasonic treatment and high shear stirring. The mixed suspension is formed into a membrane by casting, spin coating or blade coating, and then cured by solvent evaporation or phase inversion.

[0003] In order to further improve the performance of the membrane, annealing is a common method. Annealing the membrane above the polymer glass transition temperature (Tg) can enhance the interfacial bonding between the zeolite and the polymer matrix. However, annealing may lead to high-density accumulation of polymer chains, affecting the permeability and selectivity of the membrane. For this reason, a method of rapid cooling after annealing can be used to maintain a high free volume of the polymer chains, thereby increasing gas permeability without reducing selectivity.

[0004] The priming method is also widely used. By coating a layer of diluted polymer solution on the surface of the filler particles, the compatibility between the filler and the polymer matrix is ​​improved, and the interface defects are reduced, thereby improving the separation performance of the membrane. In addition, the template method and in-situ growth method further optimize the structure and performance of the membrane by introducing a template agent into the polymer matrix or directly growing zeolite materials in situ in the matrix to achieve uniform distribution and close bonding.

[0005] As the industry's demand for efficient and low-cost gas separation solutions continues to increase, these technologies combine the knowledge of materials science, chemical engineering and membrane technology to promote the application and development of zeolite mixed matrix membranes in carbon capture, gas purification and other fields. However, the following problems still exist:

[0006] Poor adhesion between polymer and filler, resulting in non-selective interfacial voids; polymer aging problems or inherent permeability-selectivity trade-offs, making it difficult to achieve a balance between high permeability and sufficient selectivity; traditional incompatibility between inorganic fillers and polymers; during the preparation process, precipitation or agglomeration of materials may affect the uniformity and performance of the membrane, so the dispersion problem of the filler needs to be solved. Summary of the invention

[0007] The purpose of the embodiments of the present application is to provide a method for preparing large-area oriented molecular sieve mixed matrix membranes based on selective etching, so as to solve the respective limitations of traditional polymer membranes and zeolite membranes in gas separation. By combining high-performance CO2-affinity MFI zeolite fillers with polyether block polyamide (pebax) polymers, a b-oriented (0k0) mixed matrix membrane that can be prepared on a large area is developed to achieve a balance between high permeability and high selectivity.

[0008] According to a first aspect of an embodiment of the present application, a method for preparing a large-area oriented molecular sieve mixed matrix membrane based on selective etching is provided, comprising:

[0009] (1) Synthesis of flake MFI molecular sieve crystals: A mixture with a molar ratio of 0.15TPAOH:1SiO2:1.6NH4F:15-300H2O is added into a homogeneous reaction oven, heated and rotated to obtain flake MFI molecular sieve crystals, and the template agent is removed by calcination. By rapidly optimizing the synthesis conditions, the generation of twins and symbiosis of flake MFI materials is reduced;

[0010] (2) Adjusting the crystalline state of the flaky MFI molecular sieve crystals: placing the flaky MFI molecular sieve crystals in a TAPOH solution, etching the flaky MFI molecular sieve crystals, performing tip ultrasound, and centrifuging to obtain a molecular sieve without twins and crosses, and adjusting the MFI molecular sieve crystals to b-oriented flaky materials by selective etching;

[0011] (3) Preparation of mixed matrix membrane: preparing a polymer solution and a molecular sieve solution, mixing the polymer solution and the molecular sieve solution and casting them into a culture dish, drying them overnight and vacuum drying them after standing, to obtain a mixed matrix membrane, combining solution casting and gel curing technology to achieve directional self-assembly of b-axis oriented molecular sieve materials in the polymer;

[0012] (4) Post-treatment of the mixed matrix membrane: The mixed matrix membrane was soaked in deionized water, peeled off from the culture dish and dried to obtain a large-area, flexible and stable self-supporting molecular sieve mixed matrix membrane.

[0013] Furthermore, in step (1), the temperature is heated to 100-120°C so that the MFI crystals tend to grow along the a-axis and the c-axis and show a relatively fast crystallization rate at a rotation speed of 40-80 rpm. The flaky MFI molecular sieve crystals are placed in a tubular furnace at 500-550°C for calcination for more than 10 hours to remove the organic template in the molecular sieve pores.

[0014] Furthermore, in step (2), a TAPOH solution with a concentration range of 0.18-0.23 M is used to selectively act on the defect sites of the MFI crystal, the etching temperature is 90-120° C., the etching time is 4-24 h, and the tip ultrasound time is 5-10 minutes.

[0015] Furthermore, in step (3), the polymer is selected from pedax1047, pedax1657, pedax4533, and pedax2533. After the polymer solution and the molecular sieve solution are mixed and poured into a culture dish, the overnight drying temperature is 50-70°C to avoid the sheet material being completely dried before the directional assembly is completed and a disordered film is formed due to the temperature being too high, and the solvent in the membrane cannot be completely removed and the pores are blocked due to the temperature being too low;

[0016] In one possible implementation, in step (3), a porous polymer substrate is attached to the surface of the solution. The porous polymer substrate can be polyvinylidene fluoride (PVDF), polycarbonate (PCTE) membrane, polytetrafluoroethylene (PTFE) membrane, polyethersulfone (PES) membrane, nylon membrane, etc. The ultra-thin film has a small transmission resistance during separation, so the separation efficiency is higher. By preparing an ultra-thin mixed matrix molecular sieve membrane on a porous polymer substrate, the difficulty of post-processing can be alleviated and the preparation is more convenient.

[0017] According to a second aspect of an embodiment of the present application, a large-area oriented molecular sieve mixed matrix membrane is provided, which is prepared by the method described in the first aspect.

[0018] The technical solution provided by the embodiments of the present application may have the following beneficial effects:

[0019] It can be seen from the above embodiments that the present application uses a selective etching method to adjust the morphology of the MFI molecular sieve crystals into a b-oriented sheet material, thereby maximally exposing the (0k0) crystal plane, providing a basis for the directional arrangement of the nanosheets in the polymer matrix; through the solution casting strategy and regulating the solvent evaporation temperature, the property of pebax gel solidification at room temperature is used to prevent the molecular sieve material from agglomerating, so that the sheet molecular sieve material can be arranged in a plane in the polymer matrix, maximally exposing the vertical transmission channels, providing the shortest molecular transmission path, improving the gas or liquid permeation flux and selectivity, and at the same time improving the performance and stability of the membrane, so that it has a longer life and higher gas separation or liquid separation efficiency in practical applications. rate; by loading air-permeable and sieving molecular sieves between polymers, the selectivity of polymers in the separation process is improved, thus overcoming the inherent problem of high permeability and low selectivity of polymers; taking advantage of the two-dimensional sheet material, the adhesion between the polymer and the polymer is increased, the interface pores are reduced, and the incompatibility between the polymer matrix and the inorganic nanomaterials is solved. A self-supporting large-area flexible mixed matrix MFI molecular sieve membrane and an ultra-thin mixed matrix molecular sieve membrane prepared on a porous polymer matrix are successfully prepared, which avoids the aggregation of fillers and the generation of non-selective defects, and no delamination occurs. It can be seen that the method is universal and provides high-performance solutions for the separation of various gases and liquids.

[0020] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0022] Figure 1 The scanning electron microscope image and X-ray diffraction image of the synthesized flaky MFI crystal in Example 1, wherein a) is a scanning electron microscope image of the synthesized flaky MFI material, b) is the size and thickness statistics of the corresponding molecular sieve obtained by optimizing the molar ratio of water to silicon dioxide in the present invention, and c) is an X-ray diffraction image of the synthesized MFI material;

[0023] Figure 2 Schematic diagram of the preparation of the mixed matrix membrane in Example 1;

[0024] Figure 3 The casting solutions with different mass percentages in Example 1 and the corresponding mixed matrix membranes;

[0025] Figure 4The top view and cross-sectional electron micrographs of the mixed matrix membrane in Example 1, wherein a) is a top view of a membrane with a loading of 65%, and bd) are cross-sectional images of the membrane at different magnifications;

[0026] Figure 5 Schematic diagram of the preparation of the mixed matrix membrane in Example 2;

[0027] Figure 6 is an electronic image of the mixed matrix film on the polymer substrate in Example 2;

[0028] Figure 7 X-ray diffraction images of 65% MFI loading in different polymer matrices in Example 3. DETAILED DESCRIPTION

[0029] Here, exemplary embodiments are described in detail, and examples thereof are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application.

[0030] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0031] Example 1 Preparation of self-supporting large-area oriented molecular sieve mixed matrix membrane

[0032] (1) Synthesis of flaky MFI molecular sieve crystals: A mixture having a molar ratio of 0.15 TPAOH (tetrapropylammonium hydroxide): 1 SiO2 (tetraethoxysilane): 1.6 NH4F (ammonium fluoride): 15-300 H2O (pure water) was added into a homogeneous reaction oven, heated to 100-120° C. and rotated at a speed of 40-80 rpm to obtain flaky MFI molecular sieve crystals, which were then calcined to remove the template agent therein;

[0033] To prepare plate-like MFI crystals with large size and small crystal thickness, we conducted experiments under the condition of SiO2 / H2O molar ratio of 90. It was observed that the lack of mechanical stirring during the aging stage led to abundant twin formation, which in turn caused all crystals to exhibit orthorhombic staggered growth after crystallization. However, the twin formation was significantly reduced when the aged precursor solution was stirred. Inspired by this, a rotational synthesis strategy was adopted to reduce the twin formation during crystallization.

[0034] In one embodiment, 8.598 g TPAOH (25%), 14.605 g TEOS (tetraethoxysilane) and 4 g water are added to a homogeneous reaction oven containing polytetrafluoroethylene and rotated at a speed of 60 rpm. The homogeneous reaction oven is a rotatable reactor, and the reactor contains 5 polytetrafluoroethylene cubes with a side length of 3 mm for stirring to ensure the uniformity of the system. Other high-temperature resistant items that do not react with the reaction system can also be used. The rotation speed of the reactor during the reaction is 40-80 rpm. Based on temperature optimization, between 100 and 120 ° C, MFI crystals tend to grow along two dimensions (a and c axes) and show a relatively fast crystallization rate. Therefore, at 120 ° C, after 12 hours of reaction, fortunately, the number of twins after synthesis is significantly reduced, which is attributed to the rotation interference that hinders the absorption of silicon on the crystal plate, thereby preventing the staggered growth of twins. The obtained powder is placed in a tube furnace at 500-550° C. and calcined for more than 10 hours, during which air is kept flowing to remove the organic template in the molecular sieve pores.

[0035] The size and morphology of the obtained products were confirmed by scanning electron microscopy, and the crystallinity of the products was confirmed by X-ray diffraction, as shown in Figure 1 As shown in a), through this step, an ultra-large plate-like MFI crystal with a size of 5.2×1.65μm and a thickness of 150±10nm can be obtained. Figure 1 b) shows the effect of the H2O / SiO2 ratio optimized in the present application on the thickness and size. The more water content in the reactants, the larger the size of the crystals and the thicker the thickness. Figure 1 c) in the figure shows that the material obtained in this step has very good crystallinity. The flaky MFI crystals can overcome the traditional incompatibility between inorganic fillers and polymers, which is mainly reflected in the fact that the flaky material has an extra-large and flat outer surface, which can be very well bonded to the polymer. The flaky MFI crystals are usually accompanied by twinning and symbiosis through traditional synthesis methods, thereby inhibiting the application of the material in separation membranes. A rotational synthesis strategy is adopted during the preparation process to reduce the formation of twins during the crystallization process.

[0036] (2) Crystalline state adjustment of flaky MFI molecular sieve crystals: Place the flaky MFI molecular sieve crystals in a 0.18-0.23M TAPOH solution, etch the flaky MFI molecular sieve crystals at 90-120° C. for 4-24 hours, and then perform tip ultrasound for 5-10 minutes to obtain a molecular sieve without twins and crosses; collect the sample by centrifugation at 5000 rpm.

[0037] By means of selective etching, the morphology of the MFI molecular sieve crystal is adjusted to a b-oriented flake material, exposing the (0k0) crystal plane to the maximum extent. In order to obtain highly b-oriented crystals, the present invention adopts a selective etching strategy to remove twins by using a diluted TAPOH solution with a concentration range of 0.18-0.23M for heterogeneous etching. The solution can selectively act on the defect sites of the MFI crystal. The present invention explores the effects of etching time and tip ultrasound on the morphology of MFI crystals (flake and coffin-shaped crystals). By changing the etching time in the TAPOH solution, we observed the changes in the morphology of the flake MFI crystals as the etching time increases. Etching was performed at 90°C for different times (4 hours, 8 hours, 12 hours, 18 hours and 24 hours). In the initial stage, the flake crystals are not etched. When weak etching was performed at 90°C for 4-8 hours without tip ultrasonic treatment, the morphology of the twins remained unchanged, but after a few seconds of electron beam irradiation, a large hole appeared, indicating that the crystallinity of the crystal was weaker than before, showing the potential for separating twins from the etched crystal. Subsequently, weak etching without shape destruction could be observed within 12-18 hours. As expected, by combining 5-10 minutes of tip ultrasonic treatment on the basis of 18 hours of etching, the twins can be separated from the sheet without destroying the shape of the sheet. Due to the weak crystallinity of twins and symbiotic sites, the free hydroxyl groups in the alkaline solution can etch the crystalline sites, among which TPAOH is selective and can spontaneously and selectively etch the weakly crystalline sites, which can remove twins and crossovers, so that the obtained material can always be stacked in layers in an orderly manner in the b orientation, so that an oriented film can be prepared.

[0038] The molecular sieve obtained in this step is an MFI type mesoporous molecular sieve with a pore size of 0.56-0.58 nm.

[0039] (3) Preparation of mixed matrix membrane: prepare a pedax polymer solution with a mass fraction of 1%-5% and a molecular sieve solution with an mass fraction of 8%, mix the polymer solution and the molecular sieve solution, the mass fraction of the molecular sieve in the mixed matrix solution is determined according to demand (the maximum can be configured to 65%), the higher the mass fraction, the stronger the sieving effect and the higher the selectivity, take 0.1g-2g and pour it into a glass culture dish, let it stand and then place it in an oven at 50-70°C for overnight drying, and then vacuum dry it for 2h to obtain a mixed matrix membrane;

[0040] In order to ensure the best separation efficiency, the present invention has developed appropriate strategies to achieve directional arrangement of nanosheets in the polymer matrix. Specifically, by adjusting parameters such as the concentration of the polymer solution and the evaporation temperature of the solvent, the nanosheets gradually arrange themselves according to the lowest energy configuration to form a planar arrangement structure. In addition, the gelation properties of the pebax polymer at room temperature can effectively prevent the agglomeration of the nanosheets, ensuring consistent directional arrangement in the polymer matrix, thereby forming an ideal molecular separation structure and improving the performance and application potential of the membrane.

[0041] The purchased granular pebax polymer (1047, 4533 or 2533, etc.) was dissolved in n-butanol and refluxed with stirring at 90°C for 8 hours. The mass percentage of the polymer solution was 1-5%. The etched molecular sieve was configured into an 8% solution. The solvent used was ethanol and water in a mass ratio of 7:3, and ultrasonic dispersion was performed. The polymer and molecular sieve solutions were then mixed and configured into solutions with a mass ratio of molecular sieve to polymer (i.e., the loading amount of molecular sieve) of 0, 3.5%, 10%, 20%, 30%, 45%, 55%, and 65%, respectively. 0.1g-2g was poured into a glass culture dish, allowed to stand for 1 hour, and then placed in a 50-70°C oven for overnight drying to obtain a mixed matrix membrane, such as Figure 2 As shown. Then vacuum drying is performed for 2 hours to remove the residual solvent in the oven and prevent the organic solvent from volatilizing and being inhaled into the human body. The evaporation temperature of the solvent should not be too high (not >70°C), otherwise the sheet material will be completely dry before the directional assembly is completed, which will easily lead to the formation of disordered membranes. If the evaporation temperature is too low (not <50°C), the solvent in the membrane cannot be completely removed, blocking the pores. This step solves the problem of precipitation and aggregation of inorganic materials in the polymer. The polymer pedax used is easy to form a gel at room temperature (solidified within 5 minutes), so the inorganic material will not precipitate or agglomerate when preparing the mixed matrix membrane.

[0042] Among them, the polyether block polyamide (PEBAX) is 1047, 1657, 4533, 2533, etc. In the specific implementation, the solvent is selected according to the selected PEBAX type. For example, PEBAX 1657 can also be a mixed solvent of ethanol and water.

[0043] (4) Post-treatment of the mixed matrix membrane: the mixed matrix membrane was soaked in deionized water for 1-2 minutes, then peeled off from the glass culture dish and dried in an oven at 100°C for 12 h to remove the residual solvent and water in the molecular sieve pores;

[0044] The dried mixed matrix membrane was soaked in deionized water for 1-2 minutes, and the mixed matrix membrane was peeled off from the glass with tweezers and placed on a clean glassware and dried in an oven at 100°C for 12 hours. Figure 3 The morphology and cross-sectional images of the dried mixed matrix membrane were characterized using scanning electron microscopy, as shown in Figure 4 As shown, Figure 4 a) shows good compatibility between the sheet material and the polymer without any defects. Figure 4 b) to d) in the figure are cross-sectional views of the film, showing a layer-by-layer stacking morphology, confirming that the film prepared by the above method is highly b-oriented. The preparation of the self-supporting film in this embodiment overcomes the limitation of the film substrate, and the self-supporting film can meet industrial applications, and the size of the self-supporting film can be customized according to the size of the equipment.

[0045] Example 2 Preparation of Ultrathin Mixed Matrix Molecular Sieve Membrane on Polymer Substrate

[0046] (1) Synthesizing flake MFI molecular sieve crystals according to step (1) in Example 1;

[0047] (2) adjusting the crystalline state of the flaky MFI molecular sieve crystals according to step (2) in Example 1;

[0048] (3) Prepare the mixed matrix membrane according to step (3) in Example 1, such as Figure 5 As shown, after the prepared mixed matrix solution is poured into a glass culture dish, a porous polymer substrate is attached to the surface of the mixed matrix solution, placed in an oven at 50-70°C for 12 hours, and dried under vacuum for 12 hours. The obtained product is as shown Figure 6 The polymer substrate can be polyvinylidene fluoride (PVDF), polycarbonate (PCTE) membrane, polytetrafluoroethylene (PTFE) membrane, polyethersulfone (PES) membrane, nylon membrane, etc.

[0049] (4) Post-treatment of the mixed matrix membrane was performed according to step (4) in Example 1.

[0050] Example 3 Preparation of b-oriented self-supporting mixed matrix molecular sieve membranes using different polymers

[0051] (1) Synthesizing flake MFI molecular sieve crystals according to step (1) in Example 1;

[0052] (2) adjusting the crystalline state of the flaky MFI molecular sieve crystals according to step (2) in Example 1;

[0053] (3) A mixed matrix membrane was prepared according to step (3) in Example 1, wherein the polymer used was replaced. The replaceable polymers include but are not limited to pebax 1657, pebax 1074, pebax 4533, and pebax 2533.

[0054] (4) Post-treatment of the mixed matrix film was performed according to step (4) in Example 1. The orientation of the dried film was characterized by X-ray diffraction, such as Figure 7 As shown, it shows a high degree of b-orientation, which proves that the compatibility between the sheet-like molecular sieve material and different polymer matrices is very good.

[0055] Those skilled in the art will readily appreciate other embodiments of the present application after considering the specification and practicing the contents disclosed herein. The present application is intended to cover any variations, uses or adaptations of the present application, which follow the general principles of the present application and include common knowledge or customary technical means in the art that are not disclosed in the present application.

[0056] It should be understood that the present application is not limited to the exact construction that has been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof.

Claims

1. A method for preparing a large-area oriented molecular sieve mixed matrix membrane based on selective etching, characterized in that: include: (1) Synthesis of flake MFI molecular sieve crystals: Add a mixture with a molar ratio of 0.15TPAOH:1SiO2:1.6NH4F:15-300H2O into a homogeneous reaction oven, heat and rotate to obtain flake MFI molecular sieve crystals, and calcine to remove the template agent therein; (2) Adjusting the crystal state of the flake MFI molecular sieve crystal: placing the flake MFI molecular sieve crystal in a TAPOH solution, etching the flake MFI molecular sieve crystal, performing tip ultrasound, and centrifuging to obtain a molecular sieve without twins and crosses; (3) Preparation of mixed matrix membrane: preparing a polymer solution and a molecular sieve solution, mixing the polymer solution and the molecular sieve solution and pouring them into a culture dish, standing them, drying them overnight and vacuum drying them, to obtain a mixed matrix membrane; (4) Post-treatment of the mixed matrix membrane: The mixed matrix membrane was soaked in deionized water, peeled off from the culture dish and dried.

2. The method according to claim 1, characterized in that In step (1), the temperature is heated to 100-120° C. and the rotation speed is 40-80 rpm.

3. The method according to claim 1, characterized in that In step (1), the flaky MFI molecular sieve crystals are placed in a tubular furnace at 500-550° C. and calcined for more than 10 hours.

4. The method according to claim 1, characterized in that: In step (2), a M TAPOH solution having a concentration range of 0.18-0.23 M is used.

5. The method according to claim 1, characterized in that In step (2), the etching temperature is 90-120° C. and the etching time is 4-24 hours.

6. The method according to claim 1, characterized in that In step (2), the tip ultrasound time is 5-10 minutes.

7. The method according to claim 1, characterized in that In step (3), the polymer is selected from pedax1047, pedax1657, pedax4533, and pedax2533.

8. The method according to claim 1, characterized in that In step (3), after the polymer solution and the molecular sieve solution are mixed and poured into a culture dish, the porous polymer substrate is attached to the surface of the solution.

9. The method according to claim 1, characterized in that: In step (3), the overnight drying temperature is 50-70°C.

10. A large-area oriented molecular sieve mixed matrix membrane, characterized in that: It is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Uniformly b-oriented mfi zeolite membrane with variable thickness supported on substrate and preparation method thereof

    CN101585545A

  • Method for preparing oriented MFI molecular sieve membrane in wide temperature range and application of oriented MFI molecular sieve membrane

    CN118059693A

  • The preparing method of MFI zeolite contaning preferred orientation and the MFI zeolite contaning preferred orientation thereby

    KR1020150142465A

  • Zeolite nanosheet membrane

    US20150045206A1

  • Systems, devices and methods for molecular separation

    US20180056246A1