Polishing process of optical element for nanoflow cytometer
Through multi-step polishing process and specific parameter control, the problem that traditional processes cannot meet the high requirements of nanometer flow cytometer optical components is solved, the surface is atomically smooth, the optical performance and production efficiency are improved, and the service life is extended.
Patent Information
- Application Number
- CN202411126252.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-15
AI Technical Summary
The traditional polishing process cannot meet the high requirements of nanometer flow cytometer on the surface finish, flatness and optical transmittance of optical components, resulting in light signal scattering and absorption, reducing the sensitivity and accuracy of detection, and limiting the performance and application of the instrument.
Adopt a multi-step polishing process, including pretreatment, rough polishing, fine polishing and chemical mechanical polishing, use specific polishing fluid and polishing abrasives, control particle size, pressure, rotation speed and environmental conditions, and monitor surface roughness in real time to ensure that the surface reaches the atomic level smooth.
It significantly improves the optical performance and imaging quality of optical elements, ensures that the surface roughness is reduced to less than 1 nanometer, improves product quality stability and production efficiency, extends service life, and reduces maintenance costs.
Smart Images

Figure CN118769140A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optical element processing, in particular to a polishing process for optical elements used in nanometer flow cytometers. Background Art
[0002] In the field of modern bioanalysis, nano-flow cytometer has become an indispensable key tool due to its ability to perform high-precision, high-sensitivity, multi-parameter quantitative analysis of single cells or particles. The excellent performance of this advanced instrument depends to a great extent on the quality of its internal optical components.
[0003] Key parameters such as the surface roughness, flatness, and optical transmittance of optical components directly determine the accuracy and reliability of nano-flow cytometers during detection and analysis. For example, extremely small surface roughness can reduce light scattering and reflection losses, ensuring accurate transmission and reception of optical signals; excellent flatness helps maintain the stability of the optical path and avoid light distortion and deviation; high optical transmittance allows more effective light signals to be captured by the instrument, thereby improving the sensitivity and accuracy of detection; however, it is not easy to achieve these ideal parameter indicators. Traditional polishing processes face many severe challenges when processing optical components for nano-flow cytometers. On the one hand, traditional processes often find it difficult to control the surface roughness below the nanometer level, and cannot meet the extremely high surface finish requirements of nano-flow cytometers for optical components. On the other hand, in terms of flatness control, traditional methods may cause tiny unevenness, affecting the consistency and accuracy of the optical path; in addition, traditional polishing processes also perform poorly in improving optical transmittance. Due to the inability to effectively remove tiny flaws and defects on the surface, light will be scattered and absorbed unnecessarily when passing through optical components, thereby reducing optical transmittance. This series of problems not only limits the performance of nanoflow cytometers, but also hinders their wider application in biomedical research, clinical diagnosis and other fields.
[0004] Therefore, developing an innovative and efficient polishing process to meet the stringent requirements of optical components for nano-flow cytometers has become an important problem that needs to be solved urgently in the current field of optical component manufacturing. Summary of the invention
[0005] Based on this, the purpose of the present invention is to provide a polishing process for an optical element for a nano-flow cytometer to solve the technical problems mentioned in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a polishing process for an optical element for a nanometer flow cytometer, comprising the following steps:
[0007] First, pre-treatment is performed to deeply clean the optical components with the help of ultrasonic cleaning technology. The cleaning liquid temperature is controlled at 30-40 degrees Celsius, the cleaning time is 15-20 minutes, and the ultrasonic frequency is set at 40-60kHz to remove surface impurities and oil stains for subsequent polishing operations;
[0008] Then, rough polishing is performed, using polishing abrasive with a particle size of 2-4 microns, a pressure of 0.6-0.8 MPa, a rotation speed of 600-800 rpm, and a polyurethane polishing pad with a hardness of 60-70 degrees Shore A to remove obvious scratches and unevenness, and reduce the surface roughness to 10 nanometers;
[0009] Then, fine polishing is performed, using polishing abrasive with a particle size of 0.2-0.8 microns, increasing the pressure to 1.2-1.8 MPa, increasing the speed to 1200-1800 rpm, and replacing the polishing pad with a flannel material with a nap length of 0.5-1 mm to reduce the surface roughness to less than 1 nanometer;
[0010] After that, chemical mechanical polishing is performed, using a polishing liquid containing specific chemical reagents, with the mechanical action pressure controlled at 0.2-0.4MPa and the polishing liquid flow rate at 50-80ml / min to achieve atomic-level smoothness of the surface;
[0011] Finally, post-treatment is carried out, washing with deionized water for 10-15 minutes, and then drying with nitrogen at a gas flow rate of 10-15 cubic meters per hour to completely remove residual polishing liquid and impurities.
[0012] During the entire polishing process, the polishing liquid contains 3%-7% of oxidizing agent hydrogen peroxide, 1%-3% of complexing agent ethylenediaminetetraacetic acid and 0.3%-0.7% of surfactant sodium dodecyl sulfate;
[0013] During rough polishing and fine polishing, the polishing equipment table should be kept level, and the levelness error should not exceed 0.05 mm / m. The surface roughness of the optical element should be monitored in real time and the parameters should be adjusted according to the results.
[0014] At the same time, the ambient temperature of the whole process is maintained at 20-25 degrees Celsius and the relative humidity is 50%-60%. The relative humidity of the environment is controlled at 30%-40% during post-processing drying.
[0015] In summary, the present invention mainly has the following beneficial effects:
[0016] 1. The present invention can effectively remove scratches, unevenness and impurities on the surface of optical elements through multi-step polishing treatment, including pretreatment, rough polishing, fine polishing and chemical mechanical polishing, reduce the surface roughness to less than 1 nanometer, and achieve atomic-level smoothness of the surface, thereby significantly improving the optical performance and imaging quality of the optical element.
[0017] 2. During the rough polishing and fine polishing processes, the present invention accurately controls the parameters such as the particle size, pressure, and rotation speed of the polishing abrasive, monitors the surface roughness in real time and makes adjustments, and at the same time maintains the horizontality of the workbench of the polishing equipment, thereby ensuring that each optical component can achieve a highly consistent polishing effect and improving the quality stability of the product.
[0018] 3. The polishing liquid of the present invention contains an oxidant, a complexing agent and a surfactant at a specific concentration, which helps to improve the polishing efficiency, reduce surface damage, and achieve a more uniform and fine polishing effect.
[0019] 4. The present invention utilizes reasonable process flow and parameter settings to shorten the polishing time, reduce the possibility of repeated processing, enable the optical element to complete the polishing process quickly and efficiently, and improve production efficiency.
[0020] 5. The entire polishing process of the present invention strictly controls and regulates the ambient temperature, relative humidity, cleaning and drying, so that the process has good controllability and repeatability, and can obtain stable high-quality products under different production conditions.
[0021] 6. The present invention reduces surface defects and stress concentration through fine polishing, thereby effectively extending the service life of optical elements in the nano-flow cytometer and reducing the maintenance cost of the equipment.
[0022] 7. The present invention has a wide range of applications. The polishing process is applicable to optical elements for nano-flow cytometers of various types and specifications, and has strong versatility and practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a flow chart of the polishing process of the present invention;
[0024] Figure 2 It is a structural schematic diagram of the CMP polishing machine of the present invention;
[0025] Figure 3 It is a schematic structural diagram of a detachable polishing head and a threaded connector of the present invention;
[0026] Figure 4 It is a schematic structural diagram of the threaded connector of the present invention from another angle.
[0027] In the figure: 1. CMP polishing machine; 2. Disassembled polishing head; 3. Threaded connector; 4. Nut; 5. Connecting plate; 6. Docking groove. DETAILED DESCRIPTION
[0028] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0029] The following describes an embodiment of the present invention based on its overall structure.
[0030] Embodiment 1
[0031] like Figure 1 As shown, in this embodiment, the polishing process of the optical element for the nano flow cytometer includes the following steps:
[0032] Take the optical element for nano-flow cytometer, and in the pretreatment step, control the temperature of the cleaning solution at 35 degrees Celsius, set the cleaning time to 18 minutes, and the ultrasonic frequency to 50 kHz;
[0033] When rough polishing, use polishing abrasive with a particle size of 3 microns, a pressure of 0.7 MPa, a speed of 700 rpm, and a polyurethane polishing pad with a hardness of 65 Shore A.
[0034] When fine polishing, use polishing abrasive with a particle size of 0.5 microns, a pressure of 1.5 MPa, a speed of 1500 rpm, and a flannel polishing pad with a nap length of 0.8 mm;
[0035] In chemical mechanical polishing, the mechanical action pressure is 0.3 MPa and the polishing liquid flow rate is 65 ml / min;
[0036] Post-treatment cleaning for 12 minutes, nitrogen drying gas flow rate 12 cubic meters / hour;
[0037] In the polishing liquid, the concentration of hydrogen peroxide is 5%, the concentration of ethylenediaminetetraacetic acid is 2%, and the concentration of sodium dodecyl sulfate is 0.5%;
[0038] The ambient temperature during the whole process was 22 degrees Celsius and the relative humidity was 55%, and the relative humidity during post-processing drying was 35%.
[0039] Embodiment 2
[0040] like Figure 1 As shown, in this embodiment, the polishing process of the optical element for the nano flow cytometer includes the following steps:
[0041] In the pretreatment, the cleaning solution temperature was 30 degrees Celsius, the cleaning time was 15 minutes, and the ultrasonic frequency was 40kHz;
[0042] For rough polishing, a polishing abrasive with a particle size of 2 microns was selected, the pressure was 0.6 MPa, the speed was 600 rpm, and a polyurethane polishing pad with a Shore A of 60 degrees was used;
[0043] For fine polishing, use polishing abrasive with a particle size of 0.2 microns, a pressure of 1.2 MPa, a speed of 1200 rpm, and a flannel polishing pad with a nap length of 0.5 mm;
[0044] The mechanical action pressure of chemical mechanical polishing is 0.2MPa, and the polishing liquid flow rate is 50ml / min;
[0045] Post-treatment cleaning for 10 minutes, nitrogen drying gas flow rate 10 cubic meters / hour;
[0046] The polishing liquid contains 3% hydrogen peroxide, 1% ethylenediaminetetraacetic acid, and 0.3% sodium dodecyl sulfate;
[0047] The ambient temperature during the process was 20 degrees Celsius and the relative humidity was 50%, and the relative humidity during post-treatment drying was 30%.
[0048] Embodiment 3
[0049] like Figure 1 As shown, in this embodiment, the polishing process of the optical element for the nano flow cytometer includes the following steps:
[0050] During pretreatment, the cleaning liquid temperature was 40 degrees Celsius, the cleaning time was 20 minutes, and the ultrasonic frequency was 60kHz;
[0051] For rough polishing, a polishing abrasive with a particle size of 4 microns, a pressure of 0.8 MPa, a rotation speed of 800 rpm, and a polyurethane polishing pad with a Shore A of 70 degrees was used;
[0052] Fine polishing uses polishing abrasive with a particle size of 0.8 microns, a pressure of 1.8 MPa, a speed of 1800 rpm, and a flannel polishing pad with a nap length of 1 mm;
[0053] Chemical mechanical polishing mechanical pressure 0.4MPa, polishing liquid flow rate 80ml / min;
[0054] Post-treatment cleaning for 15 minutes, nitrogen drying gas flow rate 15 cubic meters / hour;
[0055] The polishing liquid contains 7% hydrogen peroxide, 3% ethylenediaminetetraacetic acid, and 0.7% sodium lauryl sulfate;
[0056] The whole process environment temperature is 25 degrees Celsius, relative humidity is 60%, and the relative humidity is 40% during post-treatment drying.
[0057] Embodiment 4
[0058] like Figure 1 As shown, in this embodiment, the polishing process of the optical element for the nano flow cytometer includes the following steps:
[0059] In the pretreatment stage, the cleaning liquid temperature was 32 degrees Celsius, the cleaning time was 16 minutes, and the ultrasonic frequency was 45kHz;
[0060] For rough polishing, a polishing abrasive with a particle size of 2.5 microns was selected, the pressure was 0.65 MPa, the speed was 650 rpm, and a polyurethane polishing pad with Shore A 62 was used;
[0061] Fine polishing uses polishing abrasive with a particle size of 0.3 microns, a pressure of 1.3 MPa, a speed of 1300 rpm, and a flannel polishing pad with a nap length of 0.6 mm;
[0062] Chemical mechanical polishing mechanical pressure 0.25MPa, polishing liquid flow rate 55ml / min;
[0063] Post-treatment cleaning for 11 minutes, nitrogen drying gas flow rate 11 cubic meters / hour;
[0064] The polishing liquid contains 4% hydrogen peroxide, 1.5% ethylenediaminetetraacetic acid, and 0.4% sodium lauryl sulfate;
[0065] The ambient temperature of the entire process is 21 degrees Celsius and the relative humidity is 52%, and the relative humidity during post-processing drying is 32%.
[0066] See also Figure 2 — Figure 4 It should be noted that: the mechanical device used in the chemical mechanical polishing of the present invention is a CMP polishing machine 1, a detachable polishing head 2 is installed in the CMP polishing machine 1, and a threaded connector 3 corresponding to the detachable polishing head 2 is provided in the CMP polishing machine 1, and a nut 4 threadedly connected to the threaded connector 3 is rotatably installed at the end of the detachable polishing head 2;
[0067] When in use, the threaded connector 3 and the nut 4 will limit the connection between the detachable polishing head 2 and the CMP polishing machine 1, ensuring the stability of the detachable polishing head 2 when the CMP polishing machine 1 is running. At the same time, when the detachable polishing head 2 needs to be replaced, the detachable polishing head 2 can be separated from the threaded connector 3 by rotating the nut 4, which is convenient for the user to replace the detachable polishing head 2.
[0068] It should be further explained that a connecting plate 5 located inside the nut 4 is fixedly installed at the end of the detachable polishing head 2, and the width of the connecting plate 5 is smaller than the inner diameter of the nut 4, and a docking groove 6 corresponding to the connecting plate 5 is opened at the end of the threaded connector 3;
[0069] When the detachable polishing head 2 needs to be installed, because the corners of the opening position of the connecting groove 6 are all beveled, and because the end of the connecting plate 5 protrudes from the nut 4, the connecting plate 5 will first contact the end of the threaded connector 3, so that when the connecting plate 5 enters the docking groove 6, the end of the nut 4 will contact the threaded connector 3, thereby ensuring the stability of the movement of the detachable polishing head 2 during the installation and disassembly of the detachable polishing head 2, and when the CMP polishing machine 1 is running, the connecting plate 5 will cooperate with the docking groove 6 to ensure the stability of the detachable polishing head 2 during rotation, thereby preventing the nut 4 from separating from the threaded connector 3 when the detachable polishing head 2 is rotated.
[0070] Although an embodiment of the present invention has been shown and described, this specific embodiment is only an explanation of the present invention and is not a limitation of the invention. The specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. After reading this specification, those skilled in the art may make modifications, substitutions and variations to the embodiments without creative contribution as needed without departing from the principles and purpose of the present invention. However, as long as they are within the scope of the claims of the present invention, they are protected by patent law.
Claims
1. A polishing process for an optical element for a nano-flow cytometer, characterized in that: The following steps are involved: Step 1: Pretreatment: Use ultrasonic cleaning technology to deeply clean the optical components to ensure that the impurities and oil on the surface are completely removed, laying a solid foundation for subsequent polishing operations; during the ultrasonic cleaning process, control the cleaning liquid temperature at 30-40 degrees Celsius and the cleaning time is 15-20 minutes; Step 2: Rough polishing: Use polishing abrasives with a particle size of 2-4 microns, and perform preliminary polishing under the conditions of pressure setting at 0.6-0.8MPa and speed control at 600-800 rpm to remove obvious scratches and unevenness on the surface and reduce the surface roughness of the optical element to 10 nanometers; During the rough polishing process, the polishing pad used is made of polyurethane with a hardness of 60-70 degrees Shore A; Step 3: Fine polishing: Carefully select polishing abrasives with a particle size of 0.2-0.8 microns, increase the pressure to 1.2-1.8 MPa, and increase the speed to 1200-1800 rpm to reduce the surface roughness of the optical component to less than 1 nanometer; during fine polishing, the polishing pad is replaced with velvet material with a fluff length of 0.5-1 mm; Step 4: Chemical mechanical polishing: Use a polishing liquid containing specific chemical reagents and perform fine polishing under the coordination of mechanical action to achieve atomic-level smoothness of the surface; in chemical mechanical polishing, the pressure of the mechanical action is controlled at 0.2-0.4MPa, and the flow rate of the polishing liquid is 50-80ml / min; Step 5: Post-processing: The polished optical components are fully cleaned and efficiently dried to completely remove residual polishing liquid and impurities; deionized water is used for cleaning for 10-15 minutes, and nitrogen is used for drying at a gas flow rate of 10-15 cubic meters per hour.
2. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: The polishing liquid contains oxidizing agent hydrogen peroxide with a concentration in the range of 3%-7%, complexing agent ethylenediaminetetraacetic acid with a concentration in the range of 1%-3%, and surfactant sodium dodecyl sulfate with a concentration in the range of 0.3%-0.7%.
3. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: In the pretreatment step, the frequency of ultrasound was set at 40-60 kHz.
4. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: During the rough polishing and fine polishing steps, the worktable of the polishing equipment is kept horizontal, and the horizontality error does not exceed 0.05 mm / m.
5. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: The polishing head used for the chemical mechanical polishing is made of soft rubber material, and its Shore hardness is A30-40 degrees.
6. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: In the drying step of the post-processing, the relative humidity of the drying environment is controlled at 30%-40%.
7. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: During the entire polishing process, the ambient temperature is maintained at 20-25 degrees Celsius and the relative humidity is 50%-60%.
8. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: During the rough polishing and fine polishing steps, the surface roughness of the optical component is monitored in real time, and the polishing parameters are adjusted based on the monitoring results.
9. The polishing process for an optical element for a nano-flow cytometer according to claim 1, characterized in that: The mechanical equipment used in the chemical mechanical polishing is a CMP polishing machine (1), wherein a detachable polishing head (2) is installed in the CMP polishing machine (1), and a threaded connection head (3) corresponding to the detachable polishing head (2) is provided in the CMP polishing machine (1), and a nut (4) threadedly connected to the threaded connection head (3) is rotatably installed at the end of the detachable polishing head (2).
10. The polishing process for an optical element for a nano-flow cytometer according to claim 9, characterized in that: A connecting plate (5) located inside the nut (4) is fixedly mounted on the end of the detachable polishing head (2), the width of the connecting plate (5) is smaller than the inner diameter of the nut (4), and the end of the connecting plate (5) protrudes from the nut (4), and a docking groove (6) corresponding to the connecting plate (5) is provided on the end of the threaded connector (3).
Citation Information
Patent Citations
Additives for barrier chemical mechanical planarization
CN107586517A
Ultrasonic-assisted grinding and polishing method
CN107717640A
Chemico-mechanical polishing method for cadmium selenide crystals
CN109396967A
Chemical mechanical polishing process for gallium oxide single crystal wafer
CN115870873A
Method of polishing a large part and abrasive for use in the method
US20060111023A1
Cited By
Metal square mirror polishing method and tool
CN120395536A
Base material processing method
CN121223675A