Light-emitting diode epitaxial wafer and preparation method thereof, and light-emitting diode

By adopting a multi-layer P-type semiconductor layer in the GaN-based light emitting diode, the hole concentration of the P-type GaN layer is improved by introducing the MgN layer and In, the problem of low luminescence efficiency of the GaN-based light emitting diode is solved, and more efficient is achieved hole injection and luminescence efficiency.

CN118782704BActive Publication Date: 2024-11-22JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411266770.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The luminescence efficiency of GaN-based light-emitting diodes is mainly due to the low P-type doping concentration and the hole mobility is smaller than that of electrons, which leads to the mismatch between electrons and hole injection, which affects the luminescence efficiency. The commonly used electron barrier layer reduces hole injection. efficiency.

Method used

The P-type semiconductor layer structure is adopted that includes a first step layer and a second step layer. The first step layer is a MgN layer, an Alx1Iny1Ga1-x1-y1N layer and a P-type GaN layer. The second step layer is an Alx2Iny2Ga1-x2-y2N layer. The P-type InGaN layer and the non-doped GaN layer increase the hole concentration of the P-type GaN layer through the diffusion of the MgN layer and the introduction of In, reduce electron overflow and non-radiation recombination, and optimize hole injection.

Benefits of technology

It effectively improves hole injection efficiency and luminous efficiency, reduces electron overflow, forms a flat surface, lays the foundation for the subsequent electrode to form good ohmic contact, and improves the matching degree between holes and electrons in the multi-quantum well layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782704B_ABST
    Figure CN118782704B_ABST
Patent Text Reader

Abstract

The present invention discloses a light-emitting diode epitaxial wafer and a preparation method thereof, and a light-emitting diode, and relates to the field of semiconductor optoelectronic devices. The epitaxial wafer includes a substrate, a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer, and a P-type semiconductor layer in sequence; the P-type semiconductor layer includes a first step layer and a second step layer in sequence; the first step layer is a periodic structure, and each period includes a MgN layer, an Al layer, and a plurality of other layers stacked in sequence; x1 In y1 Ga 1‑x1‑y1 N layer and P-type GaN layer; the second step layer is a periodic structure, each period includes Al x2 In y2 Ga 1‑x2‑y2 N layer, P-type InGaN layer and undoped GaN layer; wherein x1≥x2, y1≤y2, and the doping concentration of the P-type GaN layer is less than the doping concentration of the P-type InGaN layer. The present invention can improve the luminous efficiency of the light-emitting diode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor optoelectronic devices, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and a light emitting diode. Background Art

[0002] The luminous efficiency of GaN-based light-emitting diodes is affected by many factors, which seriously restricts the commercial application of GaN semiconductor light-emitting diodes as high-brightness, high-power devices in the lighting field. Specifically, P-type doping of GaN is relatively difficult, and the P-type doping concentration is much lower than the N-type doping concentration. At the same time, the effective mass of holes is much greater than the effective mass of electrons, resulting in the mobility of holes being much lower than the mobility of electrons. These two factors make the injection rate of holes into the multi-quantum well region much lower than the injection rate of electrons, resulting in a mismatch between the injection of electrons and holes, which will affect the luminous efficiency of the light-emitting diode.

[0003] On the other hand, the epitaxial structure of the commonly used GaN-based light-emitting diodes generally includes: a buffer layer, an undoped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer arranged on a substrate. The electron blocking layer generally adopts a wide-bandgap AlGaN material, which can effectively block electron overflow, but also affects hole injection, further reducing the efficiency of hole injection into the multi-quantum well layer and reducing the luminous efficiency of the light-emitting diode. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a light emitting diode epitaxial wafer and a preparation method thereof, which can effectively improve the light emitting efficiency.

[0005] Another technical problem to be solved by the present invention is to provide a light emitting diode with high light emitting efficiency.

[0006] In order to solve the above problems, the present invention discloses a light-emitting diode epitaxial wafer, which comprises a substrate, a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer and a P-type semiconductor layer sequentially stacked on the substrate; the P-type semiconductor layer comprises a first step layer and a second step layer sequentially stacked on the multi-quantum well layer;

[0007] The first step layer is a periodic structure, and each period includes a MgN layer, an Al x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer;

[0008] The second stepped layer is a periodic structure, each period includes sequentially stacked Al x2 In y2 Ga 1-x2-y2N layer, P-type InGaN layer and undoped GaN layer;

[0009] Among them, x1≥x2, y1≤y2, and the doping concentration of the P-type GaN layer is less than the doping concentration of the P-type InGaN layer.

[0010] As an improvement of the above technical solution, the number of periods of the first stepped layer is 3 to 8; and / or

[0011] The thickness of the MgN layer is 1 nm to 10 nm; and / or

[0012] The Al x1 In y1 Ga 1-x1-y1 In the N layer, the value range of x1 is 0.02-0.15, the value range of y1 is 0.01-0.1, and the thickness is 1nm-10nm; and / or

[0013] The thickness of the P-type GaN layer is 5nm~10nm, and its doping concentration is 1×10 18 cm -3 ~1×10 19 cm -3 .

[0014] As an improvement of the above technical solution, the number of periods of the second stepped layer is 5 to 20; and / or

[0015] The Al x2 In y2 Ga 1-x2-y2 In the N layer, the value range of x2 is 0.01-0.1, the value range of y2 is 0.02-0.15, and the thickness is 5nm-10nm; and / or

[0016] The proportion of In in the P-type InGaN layer is 0.01-0.05, and its doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 , with a thickness of 1 nm to 10 nm; and / or

[0017] The thickness of the undoped GaN layer is 3nm-12nm.

[0018] As an improvement of the above technical solution, the Al x1 In y1 Ga 1-x1-y1 The N layer is gallium polar Al x1 In y1 Ga 1-x1-y1 N layers; and / or

[0019] The Al x2In y2 Ga 1-x2-y2 The N layer is nitrogen polar Al x2 In y2 Ga 1-x2-y2 N layers.

[0020] As an improvement of the above technical solution, in the first stepped layer, as the number of periods increases, the Al x1 In y1 Ga 1-x1-y1 In N layers, x1 increases and y1 decreases; and / or

[0021] In the second stepped layer, as the number of cycles increases, the Al x2 In y2 Ga 1-x2-y2 In the N layers, x2 changes gradually and y2 changes gradually.

[0022] As an improvement of the above technical solution, in the first stepped layer, as the number of periods increases, the doping concentration in the P-type GaN layer decreases; and / or

[0023] In the second stepped layer, as the number of periods increases, the doping concentration in the P-type InGaN layer increases.

[0024] Correspondingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned light-emitting diode epitaxial wafer, and comprises:

[0025] Providing a substrate, and sequentially growing a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer, and a P-type semiconductor layer on the substrate; the P-type semiconductor layer comprises a first stepped layer and a second stepped layer sequentially stacked on the multi-quantum well layer;

[0026] The first step layer is a periodic structure, and each period includes a MgN layer, an Al x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer;

[0027] The second stepped layer is a periodic structure, each period includes sequentially stacked Al x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and undoped GaN layer;

[0028] Among them, x1≥x2, y1≤y2.

[0029] As an improvement of the above technical solution, the growth temperature of the first step layer is 800° C. to 950° C., and the growth pressure is 50 torr to 500 torr; and / or

[0030] The growth temperature of the second step layer is 800° C. to 900° C., and the growth pressure is 50 torr to 500 torr.

[0031] As an improvement of the above technical solution, the growth atmosphere of the first stepped layer is H2; and / or

[0032] The growth atmosphere of the second step layer is N2.

[0033] Correspondingly, the present invention also discloses a light emitting diode, which includes the light emitting diode epitaxial wafer mentioned above.

[0034] The implementation of the present invention has the following beneficial effects:

[0035] 1. In the light emitting diode epitaxial wafer of one embodiment of the present invention, the P-type semiconductor layer includes a first stepped layer and a second stepped layer stacked in sequence; the first stepped layer is a periodic structure, and each period includes a MgN layer, an Al layer, and a Si layer stacked in sequence. x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer; the second step layer is a periodic structure, each period includes Al x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and undoped GaN layer; among them, the MgN layer can diffuse into the P-type GaN layer, so that the P-type doping element Mg in the P-type GaN layer can better replace the Ga position, reduce the formation of Mg-H bonds, and thus increase the hole concentration of the P-type GaN layer. x1 In y1 Ga 1-x1-y1 The N layer can form an electron trap, reduce electron overflow, and prevent electrons from forming too much non-radiative recombination in the P-type semiconductor layer. x2 In y2 Ga 1-x2-y2 The N layer can reduce the lattice mismatch between the first step layer and the second step layer, so that the P-type InGaN layer can adopt a higher doping concentration, thereby increasing the hole concentration of the P-type semiconductor layer as a whole. x2 In y2 Ga 1-x2-y2The N layer can also further prevent electron overflow. The In introduced into the P-type InGaN layer can also reduce the activation energy of the doping element Mg and increase the hole concentration. In addition, the introduction of In can also reduce the rough structure caused by the incorporation of Mg, making it easier to form a flat plane. Among them, the undoped GaN layer can further fill the defects on the surface of the P-type InGaN layer to form a flat and smooth surface, laying the foundation for the subsequent formation of a good ohmic contact with the electrode. In summary, the P-type semiconductor layer in this embodiment can effectively block electron overflow and improve the hole injection efficiency. It also increases the hole concentration and improves the matching degree between holes and electrons in the multi-quantum well layer, thereby effectively improving the luminous efficiency.

[0036] 2. Al in one embodiment of the present invention x1 In y1 Ga 1-x1-y1 The N layer is gallium polar Al x1 In y1 Ga 1-x1-y1 The N layer can reduce the incorporation of O impurities during the growth process, reduce the generation of defects, enhance the ability to block electrons, and improve the antistatic ability. x2 In y2 Ga 1-x2-y2 The N layer is nitrogen polar Al x2 In y2 Ga 1-x2-y2 The N layer can increase the incorporation efficiency of In, further reduce the activation energy of Mg, and increase the hole concentration.

[0037] 3. In one embodiment of the present invention, as the number of periods of the first step layer increases, the doping concentration in the P-type GaN layer decreases, which can make the holes evenly distributed on the surface, reduce the current congestion effect, improve the hole expansion efficiency, reduce the defect-trapped holes, and reduce non-radiative recombination.

[0038] 4. In one embodiment of the present invention, as the number of periods of the second step layer increases, the doping concentration in the P-type InGaN layer increases, which can increase more holes, reduce resistance, and reduce operating voltage. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a schematic structural diagram of a light emitting diode epitaxial wafer in one embodiment of the present invention;

[0040] Figure 2 It is a flow chart of a method for preparing a light emitting diode epitaxial wafer in one embodiment of the present invention. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0042] refer to Figure 1 An embodiment of the present invention discloses a light emitting diode epitaxial wafer, which includes a substrate 100, a buffer layer 200, an intrinsic GaN layer 300, an N-type GaN layer 400, a multi-quantum well layer 500 and a P-type semiconductor layer 600 stacked in sequence on the substrate 100; the P-type semiconductor layer 600 includes a first stepped layer 610 and a second stepped layer 620 stacked in sequence on the multi-quantum well layer 500; the first stepped layer 610 is a periodic structure, and each period includes a MgN layer 611, an AlN layer 620 stacked in sequence, and a second stepped layer 620 stacked in sequence. x1 In y1 Ga 1-x1-y1 N layer 612 and P-type GaN layer 613; the second step layer 620 is a periodic structure, each period includes Al x2 In y2 Ga 1-x2-y2 N layer 621, P-type InGaN layer 622 and undoped GaN layer 623; wherein, MgN layer 611 can diffuse into P-type GaN layer 613, so that the P-type doping element Mg in the P-type GaN layer can better replace Ga position, reduce the formation of Mg-H bonds, and thus increase the hole concentration of P-type GaN layer 613. x1 In y1 Ga 1-x1-y1 The N layer 612 can form an electron trap, reduce electron overflow, and prevent electrons from forming excessive non-radiative recombination in the P-type semiconductor layer 600. x2 In y2 Ga 1-x2-y2 The N layer 621 can reduce the lattice mismatch between the first stepped layer 610 and the second stepped layer 620, so that the P-type InGaN layer 622 can adopt a higher doping concentration, thereby increasing the hole concentration of the entire P-type semiconductor layer. x2 In y2 Ga 1-x2-y2The N layer 621 can also further prevent electron overflow. In order to better buffer the lattice mismatch and block electrons, x1≥x2 and y1≤y2 are controlled. The In introduced into the P-type InGaN layer 622 can also reduce the activation energy of the doping element Mg and increase the hole concentration. In addition, the introduction of In can also reduce the rough structure caused by the Mg incorporation, which is convenient for forming a flat plane. Further, the non-doped GaN layer 623 is used for defect filling, which further improves the flatness and smoothness of the P-type semiconductor layer, and lays the foundation for the subsequent formation of a good ohmic contact with the electrode. In addition, in this embodiment, the doping concentration of the P-type GaN layer 613 is controlled to be less than the doping concentration of the P-type InGaN layer 622 to optimize the distribution of holes and improve the efficiency of hole injection into the multi-quantum well layer 500. In addition, based on the P-type semiconductor layer 600 of this embodiment, the traditional electron blocking layer can be cancelled to reduce the blocking effect on holes. In summary, the P-type semiconductor layer 600 in this embodiment can effectively block electron overflow and improve the injection efficiency of holes. It also increases the hole concentration and the matching degree between holes and electrons in the multi-quantum well layer, thereby effectively improving the luminescence efficiency.

[0043] The number of periods of the first stepped layer 610 is 3 to 10, exemplarily 4, 6, 8 or 9, but not limited thereto, and preferably 3 to 8.

[0044] The thickness of the MgN layer 611 is 1 nm to 12 nm, exemplarily 2 nm, 4 nm, 6 nm, 8 nm or 11 nm, but not limited thereto, preferably 1 nm to 10 nm.

[0045] Among them, Al x1 In y1 Ga 1-x1-y1 The proportion of Al component in the N layer 612 (i.e. x1) is 0.02-0.2, and is 0.07, 0.12, 0.14 or 0.18, but is not limited thereto. Preferably, it is 0.02-0.15. Al x1 In y1 Ga 1-x1-y1 The ratio of In component in N layer 612 (i.e., y1) is 0.01-0.12, and is 0.02, 0.04, 0.06, 0.08 or 0.1, but not limited thereto. Preferably, it is 0.01-0.1. Al x1 In y1 Ga 1-x1-y1 The thickness of the N layer 612 is 1 nm to 15 nm, exemplarily 3 nm, 5 nm, 7 nm, 9 nm, 11 nm or 13 nm, but not limited thereto, preferably 1 nm to 10 nm.

[0046] The doping element in the P-type GaN layer 613 is Be or Mg, but is not limited thereto. Mg is preferred. The doping concentration in the P-type GaN layer 613 is 1×10 18 cm -3 ~5×10 19 cm -3 , exemplarily 3×10 18 cm -3 , 5×10 18 cm -3 ,7×10 18 cm -3 ,9×10 18 cm -3 , 1×10 19 cm -3 or 3×10 19 cm -3 , but not limited thereto. Preferably, the doping concentration of the P-type GaN layer 613 is 1×10 18 cm -3 ~1×10 19 cm -3 Specifically, through the MgN layer 611 and Al x1 In y1 Ga 1-x1-y1 The activation energy of the doped element Mg in the P-type GaN layer 613 is reduced due to the effect of the N layer 612. Therefore, when 1×10 18 cm -3 ~1×10 19 cm -3 When the doping concentration is 4×10 17 cm -3 ~1×10 18 cm -3 It should be noted that in the traditional epitaxial structure, the Mg doping element in the P-GaN layer is 1×10 20 cm -3 When the hole concentration can reach 5×10 17 cm -3 This embodiment significantly improves the hole concentration at a low doping concentration, and the low doping concentration also reduces the lattice damage to the P-type GaN layer 613, thereby improving its crystal quality.

[0047] The thickness of the P-type GaN layer 613 is 4 nm to 12 nm, exemplarily 5 nm, 7 nm, 9 nm or 11 nm, but not limited thereto, preferably 5 nm to 10 nm.

[0048] The number of periods of the second stepped layer 620 is 3-20, exemplarily 4, 8, 12 or 16, but not limited thereto, and preferably 5-20.

[0049] Among them, Al x2 In y2 Ga 1-x2-y2 The proportion (x2) of Al component in the N layer 621 is 0.01-0.1, and is 0.02, 0.04, 0.06 or 0.08 for example. x2 In y2 Ga 1-x2-y2 The ratio (y2) of the In component in the N layer 621 is 0.02-0.2, and is 0.05, 0.08, 0.11, 0.14 or 0.17, but is not limited thereto. Preferably, it is 0.02-0.15. Al x2 In y2 Ga 1-x2-y2 The thickness of the N layer 621 is 2 nm to 10 nm, exemplarily 3 nm, 5 nm, 7 nm or 9 nm, but not limited thereto, preferably 5 nm to 10 nm.

[0050] The proportion of In component in the P-type InGaN layer 622 is 0.01-0.08, and is 0.02, 0.04 or 0.06, but not limited thereto. Preferably, it is 0.01-0.05. The doping element of the P-type InGaN layer 622 is Be or Mg, but not limited thereto. Preferably, it is Mg. The doping concentration of the P-type InGaN layer 622 is 1×10 19 cm -3 ~5×10 21 cm -3 , exemplarily 3×10 19 cm -3 ,7×10 19 cm -3 , 2×10 20 cm -3 , 6×10 20 cm -3 , 8×10 20 cm -3 , 1×10 21 cm -3 or 4×10 21 cm -3 , but not limited thereto. Preferably 1×10 19 cm -3 ~1×10 21 cm -3 .

[0051] The thickness of the P-type InGaN layer 622 is 1 nm to 12 nm, exemplarily 3 nm, 5 nm, 7 nm or 11 nm, but not limited thereto, preferably 1 nm to 10 nm.

[0052] The thickness of the non-doped GaN layer 623 is 3 nm to 15 nm, exemplarily 5 nm, 7 nm, 9 nm, 11 nm or 13 nm, but not limited thereto, preferably 3 nm to 12 nm.

[0053] The substrate 100 is a sapphire substrate, a silicon substrate or a SiC substrate, but is not limited thereto. A sapphire substrate is preferred.

[0054] The buffer layer 200 may be an AlN layer or an AlGaN layer, but is not limited thereto. Preferably, it is an AlN layer. The thickness of the buffer layer 200 is 30 nm to 80 nm.

[0055] The intrinsic GaN layer 300 has a thickness of 1 μm to 3 μm.

[0056] The N-type GaN layer 400 is a Si-doped GaN layer, and its Si doping concentration is 5×10 18 cm -3 ~5×10 19 cm -3 , thickness is 1μm~3μm.

[0057] The multi-quantum well layer 500 is an InGaN-GaN type multi-quantum well structure or an InGaN-AlGaN type multi-quantum well structure, but is not limited thereto. Preferably, the multi-quantum well layer 500 is a periodic structure, the number of periods of which is 3 to 15, and each period includes sequentially stacked InGaN quantum well layers and GaN quantum barrier layers, wherein the proportion of In components in the InGaN quantum well layer is 0.1 to 0.3, the thickness of which is 3 nm to 5 nm, and the thickness of the GaN quantum barrier layer is 8 nm to 15 nm.

[0058] Preferably, in one embodiment, Al x1 In y1 Ga 1-x1-y1 The N layer 612 is a gallium-polar Al x1 In y1 Ga 1-x1-y1 The N layer can reduce the incorporation of O impurities during the growth process, reduce the generation of defects, enhance the blocking ability to electrons, and improve the anti-static ability.

[0059] Preferably, in one embodiment, Al x2 In y2 Ga 1-x2-y2 The N layer 621 is a nitrogen-polar Al x2 In y2 Ga 1-x2-y2 The N layer can increase the incorporation efficiency of In, further reduce the activation energy of Mg, and increase the hole concentration.

[0060] Preferably, in one embodiment, in the first step layer 610, as the number of cycles increases, Al x1 In y1 Ga 1-x1-y1 The proportion of Al component in N layer 612 (i.e. x1) increases gradually. x1 In y1 Ga 1-x1-y1 The proportion of In component in N layer 612 (i.e., y1) decreases. x1 In y1 Ga 1-x1-y1 In the N layer 612, x1 and y1 remain constant. Based on the above embodiment, the blocking effect on electrons can be further enhanced, and the antistatic ability can be improved. At the same time, the diffusion of Mg in the MgN layer 611 is also optimized, the hole concentration of the P-type GaN layer 613 is increased, and the luminous efficiency is improved.

[0061] Preferably, in one embodiment, in the second stepped layer 620, as the number of cycles increases, Al x2 In y2 Ga 1-x2-y2 The proportion of Al component (i.e. x2) in the N layer 621 decreases. x2 In y2 Ga 1-x2-y2 The proportion of In component in N layer 621 (i.e., y2) increases gradually. x2 In y2 Ga 1-x2-y2 In the N layer 621, x2 and y2 remain constant. Based on the above embodiment, the hole concentration of the P-type InGaN layer 622 can be further increased to improve the light emitting efficiency.

[0062] Preferably, in one embodiment, in the first step layer 610, as the number of periods increases, the doping concentration in the P-type GaN layer 613 decreases, and in the same period of the P-type GaN layer 613, the doping concentration remains constant. Based on the above embodiment, holes can be evenly distributed on the surface, current congestion effect is reduced, hole expansion efficiency is improved, defect-trapped holes are reduced, and non-radiative recombination is reduced.

[0063] Preferably, in one embodiment, in the second stepped layer 620, as the number of periods increases, the doping concentration in the P-type InGaN layer 622 increases, and in the same period of the P-type InGaN layer 622, the doping concentration remains constant. Based on the above embodiment, the hole concentration can be increased, and the overall resistance of the P-type semiconductor layer can be reduced, thereby reducing the operating voltage.

[0064] Accordingly, reference Figure 2The present invention also discloses a method for preparing a light emitting diode epitaxial wafer, which is used to prepare the light emitting diode epitaxial wafer, and comprises:

[0065] S1: providing a substrate;

[0066] S2: sequentially growing a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer and a P-type semiconductor layer on the substrate;

[0067] Specifically, step S2 includes:

[0068] S21: growing a buffer layer on the substrate;

[0069] Specifically, in one embodiment, an AlN layer may be grown by PVD or MOCVD as a buffer layer, but is not limited thereto.

[0070] S22: growing an intrinsic GaN layer on the buffer layer;

[0071] Specifically, in one embodiment, the intrinsic GaN layer is grown by MOCVD, the growth temperature is 1000° C. to 1200° C., and the growth pressure is 100 torr to 500 torr.

[0072] S23: growing an N-type GaN layer on the intrinsic GaN layer;

[0073] Specifically, in one embodiment, the N-type GaN layer is grown by MOCVD, the growth temperature is 1000° C. to 1200° C., and the growth pressure is 100 torr to 500 torr.

[0074] S24: growing a multi-quantum well layer on the N-type GaN layer;

[0075] Specifically, in one embodiment, an InGaN quantum well layer and a GaN quantum barrier layer are periodically grown by MOCVD, wherein the growth temperature of the InGaN quantum well layer is 750°C to 850°C, the growth pressure is 50 torr to 500 torr, and the growth temperature of the GaN quantum barrier layer is 850°C to 950°C, the growth pressure is 50 torr to 500 torr.

[0076] S25: growing a P-type semiconductor layer on the multi-quantum well layer;

[0077] Specifically, in one embodiment, step S25 includes:

[0078] S251: growing a first step layer on the N-type GaN layer;

[0079] Specifically, in one embodiment, the MgN layer, the Al x1 Iny1 Ga 1-x1-y1 N layer and P-type GaN layer until the first step layer is obtained.

[0080] The growth temperature of the first step layer is 800°C~950°C, and the growth pressure is 50torr~500torr.

[0081] Preferably, in one embodiment, the first step layer is grown in a H2 atmosphere so that Al x1 In y1 Ga 1-x1-y1 The N layer is gallium polar.

[0082] S252: growing a second stepped layer on the first stepped layer to obtain a P-type semiconductor layer;

[0083] Specifically, in one embodiment, Al is periodically grown by MOCVD. x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and undoped GaN layer until a second stepped layer is obtained.

[0084] Among them, the growth temperature of the second step layer is 800℃~900℃, and the growth pressure is 50torr~500torr.

[0085] Preferably, in one embodiment, the second step layer is grown in a N2 atmosphere so that Al x2 In y2 Ga 1-x2-y2 The N layer is nitrogen polar.

[0086] The present invention will be further described below with specific embodiments:

[0087] Example 1

[0088] This embodiment provides a light-emitting diode epitaxial wafer, which includes a substrate, a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer, and a P-type semiconductor layer stacked on the substrate in sequence. The substrate is a sapphire substrate. The buffer layer is an AlN layer with a thickness of 50 nm. The thickness of the intrinsic GaN layer is 2.5 μm. The Si doping concentration of the N-type GaN layer is 9×10 18 cm -3 , with a thickness of 2μm. The multi-quantum well layer is a periodic structure, and each period includes In 0.2 Ga 0.8 N quantum well layer and GaN quantum barrier layer, In 0.2 Ga 0.8 The thickness of the N quantum well layer is 3.5 nm, and the thickness of the GaN quantum barrier layer is 10 nm.

[0089] The P-type semiconductor layer includes a first step layer and a second step layer sequentially stacked on the multi-quantum well layer; the first step layer is a periodic structure with 5 periods, and each period includes a MgN layer, an Al layer, and a x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer; the thickness of MgN layer is 3nm, Al x1 In y1 Ga 1-x1-y1 The N layer (x1=0.05, y1=0.03) is nitrogen polar and has a thickness of 5 nm. The Mg doping concentration in the P-type GaN layer is 5×10 18 cm -3 , and its thickness is 8nm. The second step layer is a periodic structure with 10 periods. Each period includes Al x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and undoped GaN layer; Al x2 In y2 Ga 1-x2-y2 The N layer (x2=0.03, y2=0.08) is gallium polar, with a thickness of 5 nm. The proportion of In component in the P-type InGaN layer is 0.03, and the doping concentration is 1×10 20 cm -3 , with a thickness of 5nm; the thickness of the undoped GaN layer is 10nm.

[0090] The method for preparing the light emitting diode epitaxial wafer in this embodiment comprises the following steps:

[0091] (1) Providing a substrate;

[0092] (2) growing a buffer layer on the substrate;

[0093] Specifically, an AlN layer is grown by PVD to serve as a buffer layer.

[0094] (3) growing an intrinsic GaN layer on the buffer layer;

[0095] Specifically, the intrinsic GaN layer is grown by MOCVD, with a growth temperature of 1050° C. and a growth pressure of 300 torr.

[0096] (4) Growing an N-type GaN layer on the intrinsic GaN layer;

[0097] Specifically, the N-type GaN layer is grown by MOCVD, with a growth temperature of 1100° C. and a growth pressure of 300 torr.

[0098] (5) Growing a multi-quantum well layer on the N-type GaN layer;

[0099] Specifically, In is periodically grown by MOCVD. 0.2 Ga 0.8 N quantum well layer and GaN quantum barrier layer until a multi-quantum well layer is obtained. 0.2 Ga 0.8 The growth temperature of the N quantum well layer is 760°C and the growth pressure is 200 torr; the growth temperature of the GaN quantum barrier layer is 860°C and the growth pressure is 200 torr.

[0100] (6) growing a first step layer on the multi-quantum well layer;

[0101] Specifically, the MgN layer, Al x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer, until the first step layer is obtained. The growth temperature of the first step layer is 920°C, the growth pressure is 300 torr, and the growth atmosphere is N2.

[0102] (7) growing a second stepped layer on the first stepped layer to obtain a P-type semiconductor layer;

[0103] Among them, Al is grown periodically by MOCVD x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and non-doped GaN layer until a second step layer is obtained. The growth temperature of the second step layer is 850° C. and the growth atmosphere is H2.

[0104] Example 2

[0105] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 1 in that:

[0106] Al x1 In y1 Ga 1-x1-y1 The N layer is gallium polar, and the atmosphere during the preparation of the first step layer is H2.

[0107] The rest are the same as in Example 1.

[0108] Example 3

[0109] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 2 in that:

[0110] Al x2 In y2 Ga 1-x2-y2 The N layer is nitrogen polar, and the atmosphere during the preparation of the second step layer is N2. The doping concentration of the P-type InGaN layer is 3×10 20 cm -3 .

[0111] The rest are the same as in Example 2.

[0112] Example 4

[0113] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 3 in that:

[0114] In the first step layer, as the number of periods increases, Al x1 In y1 Ga 1-x1-y1 The proportion of Al components in the N layer increases, while the proportion of In components decreases. x1 In y1 Ga 1-x1-y1 In the N-layer, x1 and y1 remain constant. Specifically, in each cycle, x1 is 0.03, 0.04, 0.05, 0.06 and 0.07, and y1 is 0.05, 0.04, 0.03, 0.02 and 0.01.

[0115] In the second step layer, as the number of periods increases, Al x2 In y2 Ga 1-x2-y2 The proportion of Al components in the N layer decreases, while the proportion of In components increases. x2 In y2 Ga 1-x2-y2 In the N layer, x2 and y2 remain constant. Specifically, in each cycle, x2 is 0.05, 0.046, 0.042, 0.038, 0.034, 0.03, 0.026, 0.022, 0.018 and 0.014 respectively; y2 is 0.05, 0.055, 0.06, 0.065, 0.07, 0.075, 0.08, 0.085, 0.09 and 0.095 respectively.

[0116] The rest is the same as Example 3.

[0117] Example 5

[0118] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 4 in that:

[0119] In the first step layer, as the number of cycles increases, the doping concentration in the P-type GaN layer decreases. Moreover, in the same cycle, the doping concentration in the P-type GaN layer remains constant. Specifically, in each cycle, the doping concentration is: 3×10 18 cm -3 , 4×10 18 cm -3 , 5×1018 cm -3 , 6×10 18 cm -3 and 7×10 18 cm -3 .

[0120] In the second step layer, as the number of cycles increases, the doping concentration in the P-type InGaN layer increases. Moreover, in the same cycle, the doping concentration in the P-type InGaN layer remains constant. Specifically, in each cycle, the doping concentration is: 5×10 19 cm -3 , 6×10 19 cm -3 ,7×10 19 cm -3 , 8×10 19 cm -3 ,9×10 19 cm -3 , 1×10 20 cm -3 , 2×10 20 cm -3 , 3×10 20 cm -3 , 4×10 20 cm -3 and 5×10 20 cm -3 .

[0121] The rest are the same as in Example 4.

[0122] Comparative Example 1

[0123] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:

[0124] The P-type semiconductor layer is a P-GaN layer with a doping concentration of 5×10 19 cm -3 , with a thickness of 200nm. An AlGaN electron blocking layer is also provided between the P-type semiconductor layer and the multi-quantum well layer, with a thickness of 50nm.

[0125] The growth temperature of the P-GaN layer is 950°C and the growth pressure is 300 torr, and the growth temperature of the AlGaN electron barrier layer is 980°C and the growth pressure is 300 torr.

[0126] The rest are the same as in Example 1.

[0127] Comparative Example 2

[0128] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:

[0129] The P-type semiconductor layer does not include the first step layer, and the corresponding preparation method does not include the step of preparing this layer.

[0130] The rest are the same as in Example 1.

[0131] Comparative Example 3

[0132] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:

[0133] The P-type semiconductor layer does not include a second stepped layer, and the corresponding preparation method does not include a step of preparing this layer.

[0134] The rest are the same as in Example 1.

[0135] The light emitting diode epitaxial wafers of Examples 1 to 5 and Comparative Examples 1 to 3 were made into 10mil×24mil LED chips with a vertical structure, and their luminous brightness (120mA) was tested, and the luminous brightness improvement rate was calculated based on the data of Comparative Example 1. The specific results are shown in the following table:

[0136]

[0137] It can be seen from the table that when the P-type semiconductor layer in the embodiment of the present invention is used, the luminous brightness can be effectively improved.

[0138] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer and a P-type semiconductor layer stacked sequentially on the substrate; the P-type semiconductor layer comprises a first stepped layer and a second stepped layer stacked sequentially on the multi-quantum well layer; The first step layer is a periodic structure, and each period includes a MgN layer, an Al x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer; The second stepped layer is a periodic structure, each period includes sequentially stacked Al x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and undoped GaN layer; Among them, x1≥x2, y1≤y2, and the doping concentration of the P-type GaN layer is less than the doping concentration of the P-type InGaN layer.

2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The number of periods of the first stepped layer is 3 to 8; and / or The thickness of the MgN layer is 1 nm to 10 nm; and / or The Al x1 In y1 Ga 1-x1-y1 In the N layer, the value range of x1 is 0.02-0.15, the value range of y1 is 0.01-0.1, and the thickness is 1nm-10nm; and / or The thickness of the P-type GaN layer is 5nm~10nm, and its doping concentration is 1×10 18 cm -3 ~1×10 19 cm -3 .

3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The number of periods of the second step layer is 5 to 20; and / or The Al x2 In y2 Ga 1-x2-y2 In the N layer, the value range of x2 is 0.01-0.1, the value range of y2 is 0.02-0.15, and the thickness is 5nm-10nm; and / or The proportion of In in the P-type InGaN layer is 0.01-0.05, and its doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 , with a thickness of 1 nm to 10 nm; and / or The thickness of the undoped GaN layer is 3nm-12nm.

4. The light emitting diode epitaxial wafer according to any one of claims 1 to 3, characterized in that: The Al x1 In y1 Ga 1-x1-y1 The N layer is gallium polar Al x1 In y1 Ga 1-x1-y1 N layers; and / or The Al x2 In y2 Ga 1-x2-y2 The N layer is nitrogen polar Al x2 In y2 Ga 1-x2-y2 N layers.

5. The light emitting diode epitaxial wafer according to any one of claims 1 to 3, characterized in that: In the first stepped layer, as the number of cycles increases, the Al x1 In y1 Ga 1-x1-y1 In N layers, x1 increases and y1 decreases; and / or In the second stepped layer, as the number of cycles increases, the Al x2 In y2 Ga 1-x2-y2 In the N layers, x2 changes gradually and y2 changes gradually.

6. The light emitting diode epitaxial wafer according to any one of claims 1 to 3, characterized in that: In the first stepped layer, as the number of periods increases, the doping concentration in the P-type GaN layer decreases; and / or In the second stepped layer, as the number of periods increases, the doping concentration in the P-type InGaN layer increases.

7. A method for preparing a light emitting diode epitaxial wafer, for preparing the light emitting diode epitaxial wafer according to any one of claims 1 to 6, characterized in that: include: Providing a substrate, and sequentially growing a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a multi-quantum well layer, and a P-type semiconductor layer on the substrate; the P-type semiconductor layer comprises a first stepped layer and a second stepped layer sequentially stacked on the multi-quantum well layer; The first step layer is a periodic structure, and each period includes a MgN layer, an Al x1 In y1 Ga 1-x1-y1 N layer and P-type GaN layer; The second stepped layer is a periodic structure, each period includes sequentially stacked Al x2 In y2 Ga 1-x2-y2 N layer, P-type InGaN layer and undoped GaN layer; Among them, x1≥x2, y1≤y2.

8. The method for preparing a light emitting diode epitaxial wafer according to claim 7, characterized in that: The growth temperature of the first step layer is 800° C. to 950° C., and the growth pressure is 50 torr to 500 torr; and / or The growth temperature of the second step layer is 800° C. to 900° C., and the growth pressure is 50 torr to 500 torr.

9. The method for preparing a light emitting diode epitaxial wafer according to claim 7, characterized in that: The growth atmosphere of the first step layer is H2; and / or The growth atmosphere of the second step layer is N2.

10. A light emitting diode, characterized in that: It comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 6.