Method for manufacturing multi-layer tunneling oxidation passivated back contact cell and back contact cell

By using a multi-layer tunneling oxidation passivation method in the back contact battery, combining air thermal oxidation and tubular PECVD technology, a composite tunneling oxide layer is formed, which solves the insufficient density of the tunneling polycrystalline passivation layer in the prior art. The problem is that the open circuit voltage, short circuit current and conversion efficiency of the battery are significantly improved, and the cost is reduced.

CN118825140BActive Publication Date: 2024-12-03GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411297189.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

In the existing back contact battery process, tube PECVD deposition tunneling polycrystalline as the front passivation layer, the density is insufficient, the passivation effect is poor, and the demand for back contact battery is not met. The equipment cost is high, which affects the battery product. Competitiveness.

Method used

By adopting the multi-layer tunneling oxidation passivation method, the first oxide layer, the second oxide layer and the oxygen-doped amorphous silicon layer are formed on the front of the silicon wafer, combined with air thermal oxidation and tubular PECVD deposition technology, a composite tunneling oxide layer is formed. , improve the passivation effect and save costs while not occupying the process beat.

Benefits of technology

It significantly improves the open circuit voltage, short circuit current and battery conversion efficiency, improves the passivation effect and the density of the film layer, reduces the refractive index and parasitic absorption of the film layer, and enhances the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825140B_ABST
    Figure CN118825140B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of back contact batteries, and specifically relates to a method for manufacturing a back contact battery with multi-layer tunneling oxidation passivation and a back contact battery, including sequentially depositing a first oxide layer, a second oxide layer and an oxygen-doped amorphous silicon layer on the front of a silicon wafer to form a passivation layer, and then depositing an anti-reflection layer; the first oxide layer is formed by air thermal oxidation deposition by heating the air without vacuuming, and the second oxide layer is formed by tubular PECVD deposition under vacuum and with laughing gas, and the thickness ratio of the first oxide layer to the second oxide layer is controlled to be 1: (0.6-3.4), the thickness of the first oxide layer is 0.6-1.2nm, and the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is 1: (0.3-10.8). The present invention can greatly improve the passivation effect, so that the open circuit voltage, short circuit current and battery conversion efficiency are significantly improved; and it does not occupy the process beat, saving costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back contact batteries, and in particular relates to a manufacturing method of a multi-layer tunneling oxidation passivated back contact battery and a back contact battery. Background Art

[0002] In the existing back contact battery process, the passivation layer on the front of the silicon wafer is generally a stack of an intrinsic amorphous silicon layer and an N-type doped amorphous or microcrystalline silicon layer, or a tunneling polycrystalline passivation contact. However, the key equipment involved in the use of a stack of an intrinsic amorphous silicon layer and an N-type doped amorphous or microcrystalline silicon layer as a passivation layer is mainly plate-type PECVD, which has a high equipment cost and is not conducive to the competitiveness of battery products.

[0003] However, when using tubular PECVD to deposit tunneling polycrystalline as a passivation layer, the tunneling layer is not dense enough and the passivation effect is poor, so it cannot be applied to the front film layer of the back contact battery.

[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defect of poor passivation effect of the back-contact battery in the prior art that uses tubular PECVD to deposit tunneling polycrystalline as the front passivation layer, and to provide a manufacturing method for a back-contact battery with multi-layer tunneling oxidation passivation and a back-contact battery, the front of which has a multi-layer tunneling oxidation passivation combined with an oxygen-doped amorphous silicon layer, which can greatly improve the passivation effect, so that the open circuit voltage, short-circuit current and battery conversion efficiency are significantly improved; and it does not occupy the process cycle, saving costs.

[0006] In order to achieve the above object, in a first aspect, the present invention provides a method for manufacturing a multi-layer tunneling oxidation passivated back contact cell, comprising the following steps:

[0007] S1, provide silicon wafers;

[0008] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer;

[0009] S3, performing an etching operation on the first semiconductor layer and the corresponding isolation layer on the back side obtained in S2 to form a second semiconductor opening region;

[0010] S4, performing texturing cleaning, and selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening region on the back side of the silicon wafer through cleaning as required;

[0011] S5, depositing a second semiconductor layer on the back surface obtained in S4;

[0012] S6. Depositing a first oxide layer, a second oxide layer and an oxygen-doped amorphous silicon layer on the front side of the silicon wafer in sequence to form a passivation layer, and then depositing an anti-reflection layer on the outer surface of the passivation layer; wherein the first oxide layer is formed by air thermal oxidation deposition by heating the air without vacuuming, and the second oxide layer is formed by tubular PECVD deposition in a vacuum state with nitrous oxide passing therethrough, and the thickness ratio of the first oxide layer to the second oxide layer is controlled to be 1:(0.6-3.4), the thickness of the first oxide layer is 0.6-1.2nm, and the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is 1:(0.3-10.8).

[0013] In some preferred embodiments of the present invention, the thickness of the second oxide layer is 0.8-2 nm.

[0014] In some preferred embodiments of the present invention, the thickness of the oxygen-doped amorphous silicon layer is 1-15 nm, and the effective oxygen doping concentration is 1×10 19 cm -3 -5×10 20 cm -3 .

[0015] In some preferred embodiments of the present invention, the deposition conditions of the first oxide layer include: the deposition temperature of the deposition equipment is preset to 350-550° C. so that the air temperature is raised to the deposition temperature, and the pressure is 5000-100000 Pa.

[0016] In some preferred embodiments of the present invention, the deposition time of the first oxide layer is 900-1500 s.

[0017] In some preferred embodiments of the present invention, the deposition conditions of the second oxide layer include: a deposition temperature of 400-550° C. and a pressure of 100-250 Pa.

[0018] In some preferred embodiments of the present invention, the deposition conditions of the second oxide layer also include: a nitrous oxide flow rate of 6000-12000 sccm, a power supply power of 3-10 kW, and a deposition time of 20-100 s.

[0019] In some preferred embodiments of the present invention, the first oxide layer, the second oxide layer and the oxygen-doped amorphous silicon layer are all deposited in a tubular CVD device.

[0020] In some preferred embodiments of the present invention, the oxygen-doped amorphous silicon layer is formed by tubular PECVD deposition and the deposition conditions include: introducing nitrous oxide, hydrogen and silane, the flow rate of nitrous oxide is 75-300sccm, the flow rate of hydrogen is 3000-8000sccm, the flow rate of silane is 500-3000sccm, the pressure is 350-500Pa, the deposition temperature is 400-550°C, the power supply is 2-8kW, and the time is 20-250s.

[0021] In some preferred embodiments of the present invention, the first semiconductor layer includes a first passivation layer and a first doped silicon layer, the second semiconductor layer includes a second passivation layer and a second doped silicon layer, the first passivation layer and the second passivation layer are each independently a tunneling oxide layer or an intrinsic silicon layer, and the first doped silicon layer and the second doped silicon layer are each independently polycrystalline silicon, amorphous silicon or microcrystalline silicon.

[0022] In some preferred embodiments of the present invention, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer includes a second tunneling oxide layer and a second doped polysilicon layer; the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the first tunneling oxide layer and the second tunneling oxide layer is 1: (0.3-1.5): (0.3-1.5).

[0023] In some preferred embodiments of the present invention, the thickness of the first tunnel oxide layer and the second tunnel oxide layer are independently 1-2 nm, the thickness of the first doped polysilicon layer is 70-120 nm, and the effective doping concentration is 1×10 20 cm -3 -5×10 21 cm -3 The thickness of the second doped polysilicon layer is 50-90nm and the effective doping concentration is 1×10 19 cm -3 -5×10 20 cm -3 .

[0024] In some preferred embodiments of the present invention, the anti-reflection layer is at least one of silicon nitride, aluminum oxide and silicon oxide.

[0025] In some preferred embodiments of the present invention, the anti-reflection layer is a combination of silicon nitride and silicon oxide, the thickness of the silicon nitride is 50-130 nm, and the thickness of the silicon oxide is 80-160 nm.

[0026] In some preferred embodiments of the present invention, the deposition process of the anti-reflection layer includes: first depositing silicon nitride, then performing hydrogen treatment, and then depositing silicon oxide; wherein the conditions for hydrogen treatment include: introducing hydrogen with a hydrogen flow rate of 3000-10000sccm, a pressure of 100-400Pa, a power supply of 3-10kW, a processing time of 300-2400s, and a deposition temperature of 400-550°C.

[0027] In some preferred embodiments of the present invention, the method for manufacturing the multi-layer tunneling oxidation passivated back contact cell further comprises:

[0028] S7, performing secondary etching on a portion of the second semiconductor layer on the back side of the silicon wafer to expose the first semiconductor layer, thereby forming a first semiconductor opening region spaced apart from the second semiconductor opening region;

[0029] S8, depositing a conductive film layer on the back side;

[0030] S9, performing three etching operations on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;

[0031] S10, forming metal electrodes on the outer surfaces of the conductive film layers corresponding to the first semiconductor opening region and the second semiconductor opening region respectively.

[0032] In a second aspect, the present invention provides a back-contact battery, which is manufactured by the method for manufacturing a multi-layer tunneling oxidation passivated back-contact battery described in the first aspect.

[0033] Beneficial effects:

[0034] Compared with the traditional tubular PECVD deposition of tunneling polycrystalline film structure, the present invention adopts the above-mentioned technical scheme, especially firstly heating the front side of the silicon wafer by air to perform air thermal oxidation to deposit the first oxide layer, and then using plasma chemical vapor deposition to deposit the second oxide layer. It is possible to first construct an oxide layer with a slow oxidation rate on the bottom layer to improve the oxidation uniformity, and then use plasma assisted oxidation to improve the density of the film layer, thereby obtaining a composite tunneling oxide layer with better uniformity and density. Combined with the oxygen-doped amorphous silicon layer, it is possible to reduce the refractive index of the film layer, reduce the parasitic absorption of the film layer, greatly improve the passivation effect, and significantly improve the open circuit voltage, short circuit current and battery conversion efficiency; and the air thermal oxidation deposition of the first oxide layer is carried out as the process temperature rises, does not occupy the process cycle, and saves costs. Among them, controlling the thickness ratio of the first oxide layer and the second oxide layer within the above-mentioned suitable range makes the interface between the silicon wafer and the oxygen-doped amorphous silicon have a good passivation effect, effectively reducing the interface state density; matching the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer within the above-mentioned suitable range is beneficial to taking into account both passivation and optical effects, and is beneficial to the improvement of current.

[0035] In a preferred embodiment of the present invention, a combination of silicon nitride and silicon oxide is used as an anti-reflection layer, and hydrogen treatment is performed after the silicon nitride is deposited, so that more hydrogen atoms can be further incorporated into the silicon wafer surface and the passivation layer, and the dangling bonds in the film layer can be repaired, thereby further improving the passivation effect, thereby further improving the battery conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0037] Figure 1 It is a schematic structural diagram of a back contact battery obtained by a specific implementation of the manufacturing method of the present invention.

[0038] Description of Reference Numerals

[0039] 1. Silicon wafer, 2. First tunneling silicon oxide layer, 3. N-type doped polysilicon layer, 5. Second tunneling silicon oxide layer, 6. P-type doped polysilicon layer, 7. Passivation layer, 7.1. First oxide layer, 7.2. Second oxide layer, 7.3. Oxygen-doped amorphous silicon layer, 8. Anti-reflection layer, 9. Transparent conductive film layer, 10. Metal electrode. DETAILED DESCRIPTION

[0040] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0042] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0043] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0044] In the present invention, the area close to the silicon wafer is referred to as the inside, and the area far from the silicon wafer is referred to as the outside.

[0045] In a first aspect, the present invention provides a method for manufacturing a multi-layer tunneling oxide passivated back contact cell, comprising the following steps:

[0046] S1, provide silicon wafers;

[0047] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer;

[0048] S3, performing an etching operation on the first semiconductor layer and the corresponding isolation layer on the back side obtained in S2 to form a second semiconductor opening region;

[0049] S4, performing texturing cleaning, and selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening region on the back side of the silicon wafer through cleaning as required;

[0050] S5, depositing a second semiconductor layer on the back surface obtained in S4;

[0051] S6. Depositing a first oxide layer, a second oxide layer and an oxygen-doped amorphous silicon layer in sequence on the front side of the silicon wafer to form a passivation layer, and then depositing an anti-reflection layer on the outer surface of the passivation layer; wherein the first oxide layer is formed by air thermal oxidation deposition by heating the air without vacuuming, and the second oxide layer is formed by tubular PECVD deposition in a vacuum state with nitrous oxide passing therethrough, and the thickness ratio of the first oxide layer to the second oxide layer is controlled to be 1:(0.6-3.4), preferably 1:(1.1-3.4), the thickness of the first oxide layer is 0.6-1.2nm, and the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is 1:(0.3-10.8), preferably 1:(1.41-2.50).

[0052] The thickness ratio of the first oxide layer and the second oxide layer is 1:(0.6-3.4), for example, it can be 1:0.6, 1:0.8, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.5, 1:2.8, 1:3.0, 1:3.1, 1:3.3, 1:3.4, etc., and the range between any two point values.

[0053] The ratio of the sum of the thicknesses of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is 1:(0.3-10.8), and specific examples include 1:0.3, 1:0.5, 1:0.6, 1:0.8, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.5, 1:2.8, 1:3.0, 1:3.1, 1:3.3, 1:3.4, 1:3.5, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:10.8, etc., and the range between any two point values.

[0054] In some preferred embodiments of the present invention, the thickness of the second oxide layer is 0.8-2 nm. Using the first oxide layer and the second oxide layer in a suitable thickness range can ensure the passivation effect and is more conducive to the improvement of the open circuit voltage.

[0055] In some preferred embodiments of the present invention, the thickness of the oxygen-doped amorphous silicon layer is 1-15 nm.

[0056] Preferably, the effective oxygen doping concentration of the oxygen-doped amorphous silicon layer is 1×10 19 cm -3 -5×10 20 cm -3 , preferably 1×10 20 cm -3 -5×10 20 cm -3 .

[0057] The present invention adopts an oxygen-doped amorphous silicon layer with a suitable thickness and an effective oxygen-doped concentration, which can effectively maintain passivation and reduce the surface refractive index of the film layer, and is more conducive to the improvement of the short-circuit current.

[0058] The deposition of the first oxide layer of the present invention is formed by oxidation during the air heating process, that is, it is carried out in the heating stage before the plasma deposition of the second oxide layer, which does not occupy the process cycle, saves costs, and forms a composite oxide layer with better density. In some preferred embodiments of the present invention, the deposition conditions of the first oxide layer include: the deposition temperature of the deposition equipment is preset to 350-550°C to heat the air to the deposition temperature, and the pressure is 5000Pa-100000Pa. The use of a suitable deposition temperature of the deposition equipment to form the first oxide layer in combination with a suitable high pressure can improve the uniformity of oxidation and is more conducive to improving the passivation quality of the film layer.

[0059] In some preferred embodiments of the present invention, the deposition time of the first oxide layer is 900-1500 s.

[0060] In some preferred embodiments of the present invention, the deposition conditions of the second oxide layer include: a deposition temperature of 400-550° C. and a pressure of 100-250 Pa. Adopting a suitable deposition temperature and a suitable low pressure to form the second oxide layer can improve the compactness of the film layer and is more conducive to improving the passivation level of the film layer.

[0061] In some preferred embodiments of the present invention, the deposition conditions of the second oxide layer further include: a laughing gas flow rate of 6000-12000 sccm, a power supply power of 3-10 kW, and a deposition time of 20-100 s. It is understood that the deposition time of the second oxide layer refers to the deposition time under the condition of reaching the deposition temperature of the second oxide layer.

[0062] In some preferred embodiments of the present invention, the first oxide layer, the second oxide layer and the oxygen-doped amorphous silicon layer are all deposited in a tubular CVD device.

[0063] In some preferred embodiments of the present invention, the oxygen-doped amorphous silicon layer is formed by tubular PECVD deposition. The deposition conditions of the oxygen-doped amorphous silicon layer preferably include: introducing nitrous oxide, hydrogen, and silane, the flow rate of nitrous oxide is 75-300sccm, preferably 100-300sccm, the flow rate of hydrogen is 3000-8000sccm, the flow rate of silane is 500-3000sccm, the pressure is 350-500Pa, the deposition temperature is 400-550°C, the power is 2-8kW, and the time is 20-250s.

[0064] In some preferred embodiments of the present invention, the first semiconductor layer includes a first passivation layer and a first doped silicon layer, the second semiconductor layer includes a second passivation layer and a second doped silicon layer, the first passivation layer and the second passivation layer are each independently a tunneling oxide layer or an intrinsic silicon layer, and the first doped silicon layer and the second doped silicon layer are each independently polycrystalline silicon, amorphous silicon or microcrystalline silicon. The intrinsic silicon layer is preferably an intrinsic amorphous silicon layer. One of the first doped silicon layer and the second doped silicon layer is N-type and the other is P-type.

[0065] In some preferred embodiments of the present invention, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer includes a second tunneling oxide layer and a second doped polysilicon layer. Both semiconductor layers adopt a tunneling polycrystalline structure, which, in conjunction with the front passivation layer, is more conducive to maintaining the overall passivation effect and film quality of the battery, and preventing the temperature of the front deposition from causing thermal damage to the back passivation effect.

[0066] Further preferably, the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the first tunnel oxide layer and the second tunnel oxide layer is 1: (0.3-1.5): (0.3-1.5), preferably 1: (0.83-1.50): (0.90-1.50). The specific film layer structure with the preferred suitable thickness ratio of the present invention is more conducive to improving the passivation effect of the battery as a whole.

[0067] In some preferred embodiments of the present invention, the thickness of the first tunnel oxide layer and the second tunnel oxide layer are independently 1-2 nm, the thickness of the first doped polysilicon layer is 70-120 nm, and the effective doping concentration is 1×10 20 cm -3 -5×10 21 cm -3 The thickness of the second doped polysilicon layer is 50-90nm and the effective doping concentration is 1×10 19 cm -3 -5×10 20 cm -3 .

[0068] The first tunnel oxide layer and the second tunnel oxide layer can be independently made of silicon oxide or aluminum oxide, etc., preferably silicon oxide.

[0069] In some preferred embodiments of the present invention, the anti-reflection layer is at least one of silicon nitride, aluminum oxide and silicon oxide.

[0070] In some preferred embodiments of the present invention, the anti-reflection layer is a combination of silicon nitride and silicon oxide, the thickness of the silicon nitride is 50-130nm, and the thickness of the silicon oxide is 80-160nm. The use of the anti-reflection layer of this suitable combination is more conducive to improving the short-circuit current of the battery.

[0071] In some preferred embodiments of the present invention, the deposition process of the anti-reflection layer includes: first depositing silicon nitride, then performing hydrogen treatment, and then depositing silicon oxide.

[0072] Further preferably, the conditions for hydrogen treatment include: introducing hydrogen with a hydrogen flow rate of 3000-10000 sccm, a pressure of 100-400 Pa, a power supply of 3-10 kW, a treatment time of 300-2400 s, and a deposition temperature of 400-550°C.

[0073] The present invention performs hydrogen treatment between two anti-reflection layers, which is more conducive to further incorporating more hydrogen atoms into the silicon wafer surface and the passivation layer, repairing dangling bonds in the film layer, improving the passivation level, and preventing plasma sputtering damage.

[0074] The type and thickness of the isolation layer in S2 can refer to the prior art, for example, it can be at least one of silicon nitride, silicon oxide, silicon oxynitride or nitrogen-containing polysilicon, preferably silicon nitride. The thickness of the isolation layer can be, for example, 40-90 nm.

[0075] The deposition method of the first semiconductor layer, the second semiconductor layer and the isolation layer in S2 can refer to the existing technology, as long as the target film layer with the required thickness and doping concentration can be obtained, and it will not be repeated here.

[0076] In some preferred embodiments of the present invention, the method for manufacturing the multi-layer tunneling oxidation passivated back contact cell further comprises:

[0077] S7, performing secondary etching on a portion of the second semiconductor layer on the back side of the silicon wafer to expose the first semiconductor layer, thereby forming a first semiconductor opening region spaced apart from the second semiconductor opening region;

[0078] S8, depositing a conductive film layer on the back side;

[0079] S9, performing three etching operations on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;

[0080] S10, forming metal electrodes on the outer surfaces of the conductive film layers corresponding to the first semiconductor opening region and the second semiconductor opening region respectively.

[0081] The optional range of the widths of the first semiconductor opening region, the second semiconductor opening region and the isolation groove of the present invention is relatively wide. Preferably, the width W1 of the second semiconductor opening region is 350-550 μm, the width W2 of the first semiconductor opening region is 100-250 μm, and the width W3 of the isolation groove is 20-100 μm.

[0082] In a second aspect, the present invention provides a back-contact battery, which is manufactured by the method for manufacturing a multi-layer tunneling oxidation passivated back-contact battery described in the first aspect.

[0083] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0084] Example 1

[0085] A method for manufacturing a multi-layer tunneling oxide passivated back contact cell, the steps are as follows:

[0086] S1, double-sided polishing of silicon wafer 1;

[0087] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer 1:

[0088] The first semiconductor layer comprises a first tunneling silicon oxide layer 2 and an N-type doped polysilicon layer 3. The isolation layer is silicon nitride. The first tunneling silicon oxide layer 2 has a thickness of 1.6 nm, the N-type doped polysilicon layer 3 has a thickness of 120 nm, and an effective doping concentration of 5.8×10 20 cm -3 , the thickness of the isolation layer is 70nm.

[0089] S3, performing an etching operation on the back side of the silicon wafer 1 to form a second semiconductor opening region, wherein the width W1 of the second semiconductor opening region is 500 μm.

[0090] S4, performing texturing and cleaning on the front and back opening areas of the silicon wafer 1. During the texturing and cleaning process, the isolation layer on the back of the silicon wafer 1 is removed simultaneously by the final cleaning solution;

[0091] S5, forming a second semiconductor layer on the back side of the silicon wafer 1;

[0092] The second semiconductor layer is a second tunneling silicon oxide layer 5 (with a thickness of 1.7 nm) and a P-type doped polysilicon layer 6 (with a thickness of 80 nm and an effective doping concentration of 7.6×10 19 cm -3 ) stack.

[0093] S6, forming a passivation layer 7 and an anti-reflection layer 8 on the front side of the silicon wafer 1:

[0094] The passivation layer 7 is a multi-layer tunneling oxidation passivation structure, which consists of a first oxide layer 7.1, a second oxide layer 7.2 and an oxygen-doped amorphous silicon layer 7.3. The first oxide layer 7.1 is deposited by air thermal oxidation process and has a thickness of 0.8nm. The second oxide layer 7.2 is formed by tubular PECVD deposition under vacuum and with nitrous oxide flowing in and has a thickness of 1nm. The oxygen-doped amorphous silicon layer 7.3 is formed by tubular PECVD deposition and has a thickness of 8nm and an effective oxygen concentration of 4×10 20 cm -3 .

[0095] The first oxide layer 7.1 is an air thermal oxidation process, specifically: the graphite boat carrying the silicon wafer 1 structure is sent into the furnace tube without vacuuming, the pressure is 10000Pa, the deposition time is 1080s, and the deposition temperature is 350-450° C. The first oxide layer 7.1 is deposited as the tubular CVD equipment heats up, and does not occupy the process cycle time.

[0096] When the second oxide layer 7.2 is deposited, the flow rate of the laughing gas is 8000 sccm, the pressure is 180 Pa, the power is 6 kW, the deposition time is 20 s, and the deposition temperature is 450°C.

[0097] When the oxygen-doped amorphous layer 7.3 is deposited, the flow rate of nitrous oxide is 150 sccm, the flow rate of hydrogen is 5000 sccm, the flow rate of silane is 1600 sccm, the pressure is 400 Pa, the power is 2.5 kW, the time is 115 s, and the deposition temperature is 450°C.

[0098] The anti-reflection layer 8 is a combination of silicon nitride and silicon oxide deposited in sequence, the thickness of silicon nitride is 90nm, and the thickness of silicon oxide is 130nm. When depositing the anti-reflection layer 8, after the silicon nitride coating is completed, hydrogen treatment is first performed, and then silicon oxide deposition is performed; wherein the conditions of the hydrogen treatment are: the flow rate of the hydrogen gas is 8000sccm, the pressure is 300Pa, the power is 6kW, the time is 900s, and the deposition temperature is 450°C.

[0099] S7, performing secondary etching on the back side of the silicon wafer 1 to form a first semiconductor opening region, wherein the width W2 of the first semiconductor opening region is 250 μm;

[0100] S8, depositing a transparent conductive film layer 9 on the back side of the silicon wafer 1;

[0101] S9, etching the transparent conductive film layer 9 on the back of the silicon wafer three times to form an isolation groove between the first semiconductor and the second semiconductor; the width W3 of the isolation groove is 90 μm, and the resistance between the first semiconductor and the second semiconductor after etching is greater than 1 kΩ.

[0102] S10, forming metal electrodes 10 on the outer surfaces of the first semiconductor opening region and the second semiconductor opening region corresponding to the back side of the silicon wafer 1, respectively, to obtain a back contact battery, such as Figure 1 shown.

[0103] Example 2

[0104] The method of Example 1 is referred to, except that the thickness of the first oxide layer in S6 is 1 nm, and the thickness ratio of the first oxide layer to the second oxide layer is calculated to be 1: 1. To meet this thickness, the deposition parameters of the first oxide layer need to be adjusted as follows: the atmospheric oxidation deposition time is extended by 30%.

[0105] Example 3

[0106] The method of Example 1 is referred to, except that the thickness of the oxygen-doped amorphous silicon layer in S6 is 5 nm, and the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is calculated to be 1:2.8. The deposition parameters of the oxygen-doped amorphous silicon layer that need to be adjusted to meet this thickness are: the deposition time is reduced by 40%.

[0107] Example 4

[0108] The method of Example 1 is followed, except that the effective oxygen doping concentration of the oxygen-doped amorphous silicon layer in S6 is 5×10 19 cm -3 In order to meet the effective oxygen doping concentration, the deposition parameters of the oxygen-doped amorphous silicon layer need to be adjusted as follows: reducing the nitrous oxide content to 75 sccm.

[0109] Example 5

[0110] The method of Example 1 is referred to, except that no hydrogen treatment is performed during the deposition of the anti-reflection layer.

[0111] Comparative Example 1

[0112] The method of Example 1 is followed, except that the passivation layer in S6 is a conventional tunneling polycrystalline passivation structure, specifically: a tunneling oxide layer and doped polysilicon are sequentially deposited on the front side of the silicon wafer by PECVD, the thickness of the tunneling oxide layer is 1.4 nm, the thickness of the doped polysilicon is 8 nm, and the effective doping concentration is 3×10 20 cm -3 .

[0113] Comparative Example 2

[0114] The method of Example 1 is referred to, except that in S6, the first oxide layer is not deposited, but the second oxide layer and the oxygen-doped amorphous silicon layer are directly deposited on the front surface.

[0115] Comparative Example 3

[0116] The method of Example 1 is referred to, except that the thickness of the first oxide layer in S6 is 0.5 nm, and the thickness ratio of the first oxide layer to the second oxide layer is calculated to be 1: 2. To meet this thickness, the deposition parameters of the first oxide layer need to be adjusted as follows: shortening the deposition time by 30%.

[0117] Comparative Example 4

[0118] The method of Example 1 is referred to, except that in S6, the oxygen-doped amorphous silicon layer is adjusted so that the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is 1:13.9. The deposition parameters of the oxygen-doped amorphous silicon layer that need to be adjusted to meet this thickness are: increasing the deposition time by 300%, and the thickness of the oxygen-doped amorphous silicon layer is 25 nm.

[0119] Test Case

[0120] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.

[0121] Table 1

[0122]

[0123] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention has a multi-layer tunneling oxide passivation on the front side combined with an oxygen-doped amorphous silicon layer and other structures, which can greatly improve the passivation effect, so that the open circuit voltage, short circuit current and battery conversion efficiency are significantly improved; and it does not occupy the process cycle, saving costs.

[0124] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the use of the preferred manufacturing process of the present invention is more conducive to improving the open circuit voltage, short circuit current and battery conversion efficiency.

[0125] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for manufacturing a multi-layer tunneling oxide passivated back contact cell, characterized in that: The steps include: S1, provide silicon wafers; S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer; S3, performing an etching operation on the first semiconductor layer and the corresponding isolation layer on the back side obtained in S2 to form a second semiconductor opening region; S4, performing texturing cleaning, and selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening region on the back side of the silicon wafer through cleaning as required; S5, depositing a second semiconductor layer on the back surface obtained in S4; S6. Depositing a first oxide layer, a second oxide layer and an oxygen-doped amorphous silicon layer on the front side of the silicon wafer in sequence to form a passivation layer, and then depositing an anti-reflection layer on the outer surface of the passivation layer; wherein the first oxide layer, the second oxide layer and the oxygen-doped amorphous silicon layer are all deposited in a tubular CVD device, and the first oxide layer is formed by air thermal oxidation deposition by heating the air without vacuuming, and the deposition conditions of the first oxide layer include: the deposition temperature of the deposition device is preset to 350-550°C so that the air is heated to the deposition temperature, and the pressure is 5000-100000Pa; the second oxide layer The second oxide layer is formed by tubular PECVD deposition under vacuum and with laughing gas, wherein the deposition conditions of the second oxide layer include: a deposition temperature of 400-550°C and a pressure of 100-250Pa; the thickness ratio of the first oxide layer to the second oxide layer is controlled to be 1:(0.6-3.4), the thickness of the first oxide layer is 0.6-1.2nm, the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the oxygen-doped amorphous silicon layer is 1:(0.3-10.8), the thickness of the oxygen-doped amorphous silicon layer is 5-15nm, and the effective oxygen concentration is 1×10 20 cm -3 -5×10 20 cm -3 .

2. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The thickness of the second oxide layer is 0.8-2 nm.

3. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The deposition time of the first oxide layer is 900-1500s.

4. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1 or 3, characterized in that: The deposition conditions of the second oxide layer also include: a nitrous oxide flow rate of 6000-12000sccm, a power supply power of 3-10kW, and a deposition time of 20-100s.

5. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The oxygen-doped amorphous silicon layer is formed by tubular PECVD deposition and the deposition conditions include: introducing nitrous oxide, hydrogen and silane, the flow rate of nitrous oxide is 75-300sccm, the flow rate of hydrogen is 3000-8000sccm, the flow rate of silane is 500-3000sccm, the pressure is 350-500Pa, the deposition temperature is 400-550°C, the power is 2-8kW, and the time is 20-250s.

6. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The first semiconductor layer includes a first passivation layer and a first doped silicon layer, the second semiconductor layer includes a second passivation layer and a second doped silicon layer, the first passivation layer and the second passivation layer are each independently a tunneling oxide layer or an intrinsic silicon layer, and the first doped silicon layer and the second doped silicon layer are each independently polycrystalline silicon, amorphous silicon or microcrystalline silicon.

7. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 6, characterized in that: The first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer includes a second tunneling oxide layer and a second doped polysilicon layer; the ratio of the sum of the thickness of the first oxide layer and the second oxide layer to the thickness of the first tunneling oxide layer and the second tunneling oxide layer is 1: (0.3-1.5): (0.3-1.5).

8. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 7, characterized in that: The thickness of the first tunnel oxide layer and the second tunnel oxide layer are independently 1-2 nm, the thickness of the first doped polysilicon layer is 70-120 nm, and the effective doping concentration is 1×10 20 cm -3 -5×10 21 cm -3 The thickness of the second doped polysilicon layer is 50-90nm and the effective doping concentration is 1×10 19 cm -3 -5×10 20 cm -3 .

9. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The anti-reflection layer is at least one of silicon nitride, aluminum oxide and silicon oxide.

10. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The method for manufacturing the multi-layer tunneling oxidation passivated back contact cell also includes: S7, performing secondary etching on a portion of the second semiconductor layer on the back side of the silicon wafer to expose the first semiconductor layer, thereby forming a first semiconductor opening region spaced apart from the second semiconductor opening region; S8, depositing a conductive film layer on the back side; S9, performing three etching operations on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove; S10, forming metal electrodes on the outer surfaces of the conductive film layers corresponding to the first semiconductor opening region and the second semiconductor opening region respectively.

11. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1, characterized in that: The anti-reflection layer is a combination of silicon nitride and silicon oxide, the thickness of the silicon nitride is 50-130nm, and the thickness of the silicon oxide is 80-160nm.

12. The method for manufacturing a multi-layer tunneling oxide passivated back contact cell according to claim 1 or 11, characterized in that: The deposition process of the anti-reflection layer includes: first depositing silicon nitride, then performing hydrogen treatment, and then depositing silicon oxide; wherein the conditions for hydrogen treatment include: introducing hydrogen with a hydrogen flow rate of 3000-10000sccm, a pressure of 100-400Pa, a power supply of 3-10kW, a processing time of 300-2400s, and a deposition temperature of 400-550°C.

13. A back contact battery, characterized in that: The battery is manufactured by the method for manufacturing a multi-layer tunneling oxidation passivated back contact battery as claimed in any one of claims 1 to 12.

Citation Information

Cited By

  • Back-contact cell resistant to light-induced degradation, method for manufacturing the same, and photovoltaic module